Nothing Special   »   [go: up one dir, main page]

JP3329895B2 - Resin composition - Google Patents

Resin composition

Info

Publication number
JP3329895B2
JP3329895B2 JP18276893A JP18276893A JP3329895B2 JP 3329895 B2 JP3329895 B2 JP 3329895B2 JP 18276893 A JP18276893 A JP 18276893A JP 18276893 A JP18276893 A JP 18276893A JP 3329895 B2 JP3329895 B2 JP 3329895B2
Authority
JP
Japan
Prior art keywords
group
terminal
weight
film
parts
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP18276893A
Other languages
Japanese (ja)
Other versions
JPH0733925A (en
Inventor
薫 池田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kuraray Co Ltd
Original Assignee
Kuraray Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kuraray Co Ltd filed Critical Kuraray Co Ltd
Priority to JP18276893A priority Critical patent/JP3329895B2/en
Publication of JPH0733925A publication Critical patent/JPH0733925A/en
Application granted granted Critical
Publication of JP3329895B2 publication Critical patent/JP3329895B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】本発明は、相溶性の優れた樹脂組成物に関
する。
[0001] The present invention relates to a resin composition having excellent compatibility.

【0002】[0002]

【従来の技術】従来、エチレン−ビニルアルコール系重
合体(以下これをEVOHと略記する)単独では柔軟性
および機械的特性が不十分であり、これを改善するため
にオレフィン系重合体とのブレンドが試みられている。
しかし、エチレン−ビニルアルコール系共重合体とオレ
フィン系重合体は相溶性が不良であるため、単純なブレ
ンドでは、フィルムの機械特性、透明性、均一性等が低
下し、使用に適さないことが多い。この相溶性を改善す
る方法として、オレフィン系重合体に不飽和カルボン酸
誘導体化合物、不飽和シラン化合物、不飽和エポキシ化
合物等を過酸化物を触媒として用いグラフト重合させる
ことにより反応性の官能基を導入することが公知になっ
ている。(例えば特開昭55−155042、特開昭5
0−155042、特開昭61−155412、特開平
3−88837)
2. Description of the Related Art Conventionally, ethylene-vinyl alcohol-based polymer (hereinafter abbreviated as EVOH) alone is insufficient in flexibility and mechanical properties, and is blended with olefin-based polymer in order to improve these properties. Have been tried.
However, since the ethylene-vinyl alcohol copolymer and the olefin polymer have poor compatibility, the mechanical properties, transparency, uniformity, etc., of the film may be reduced with a simple blend, making it unsuitable for use. Many. As a method of improving the compatibility, a reactive functional group is obtained by graft-polymerizing an unsaturated carboxylic acid derivative compound, an unsaturated silane compound, an unsaturated epoxy compound, or the like to an olefin polymer using a peroxide as a catalyst. It is known to be introduced. (For example, JP-A-55-155042,
0-155042, JP-A-61-155412, JP-A-3-88837)

【0003】[0003]

【発明が解決しようとする課題】しかしながら、側鎖に
反応性官能基を有するポリオレフィンとEVOHにポリ
オレフィンとのブレンドでは、特に反応性の官能基量が
多い場合、ポリオレフィンの側鎖の官能基とEVOHの
側鎖の水酸基が反応することによりゲル化し、フィルム
の外観が損なわれることが多い。しかして、本発明の目
的は、不要な架橋を抑えることにより、相溶性が良好
で、しかもゲルが少なくフィルムの外観が良好な樹脂組
成物を提供することにある。
However, in the case of blending a polyolefin having a reactive functional group in the side chain with a polyolefin in the EVOH, particularly when the amount of the reactive functional group is large, the functional group in the side chain of the polyolefin and the EVOH are not blended. The hydroxyl groups on the side chains react to cause gelation, often deteriorating the appearance of the film. Accordingly, an object of the present invention is to provide a resin composition having good compatibility, less gel, and good film appearance by suppressing unnecessary crosslinking.

【0004】上記の目的は、エチレン−ビニルアルコ−
ル系共重合体(A)およびカルボキシル基、カルボン酸
誘導体基、ケイ素含有基、エポキシ基、スルホン酸塩基
およびホスホン酸塩基からなる群より選ばれる官能基を
末端に有するオレフィン系重合体(B)を配合した樹脂
組成物を提供することによって達成される。
[0004] The purpose of the above is to provide ethylene-vinyl alcohol-
(A) and an olefin polymer (B) having at its terminal a functional group selected from the group consisting of a carboxyl group, a carboxylic acid derivative group, a silicon-containing group, an epoxy group, a sulfonate group and a phosphonate group. Is achieved by providing a resin composition containing

【0005】本発明に使用するEVOHは、エチレン−
ビニルエステル共重合体ケン化物であり、エチレン単位
の含有量は特に制限はないが、10〜70モル%の範囲
で選ばれ、好ましくは15〜60モル%、さらに20〜
60モル%が好ましく、最適には25〜55モル%であ
る。また、EVOHのビニルエステル単位のケン化度と
しては90〜100モル%の範囲から選ばれ、95〜1
00モル%が好ましく、99〜100モル%がより好ま
しい。ケン化度が低いと結晶化が低下し、ガスバリアー
性が低下し、また溶融時の熱安定性が悪化する場合があ
るので、ケン化度は高い方が好ましい。ここでビニルエ
ステルとしては酢酸ビニルが代表例として挙げられる
が、その他にプロピオン酸ビニル、ピバリン酸ビニル、
バレリン酸ビニル、カプリン酸ビニル、安息香酸ビニル
等のビニルエステルも挙げられる。これらのビニルエス
テルは一種あるいは二種以上混合して使用してもよい。
またEVOHはエチレン含有量、ケン化度、重合度の内
の少なくとも一つが異なるEVOHを混合して使用して
もよい。
[0005] The EVOH used in the present invention is ethylene-
It is a saponified vinyl ester copolymer, and the content of ethylene units is not particularly limited, but is selected in the range of 10 to 70 mol%, preferably 15 to 60 mol%, and more preferably 20 to 70 mol%.
60 mol% is preferred and optimally 25 to 55 mol%. The saponification degree of the vinyl ester unit of EVOH is selected from the range of 90 to 100 mol%,
00 mol% is preferable, and 99 to 100 mol% is more preferable. If the degree of saponification is low, crystallization decreases, the gas barrier property decreases, and the thermal stability during melting may deteriorate. Therefore, the degree of saponification is preferably higher. Here, as the vinyl ester, vinyl acetate may be mentioned as a typical example, but in addition, vinyl propionate, vinyl pivalate,
Vinyl esters such as vinyl valerate, vinyl caprate, and vinyl benzoate are also included. These vinyl esters may be used alone or in combination of two or more.
The EVOH may be a mixture of EVOHs different in at least one of the ethylene content, the degree of saponification, and the degree of polymerization.

【0006】EVOHには本発明の目的が阻害されない
範囲で他の共重合成分を含有させてもよい。ここで他の
一成分としてはプロピレン、1−ブテン、イソブテン等
のオレフィン系単量体;アクリルアミド、N−メチルア
クリルアミド、N−エチルアクリルアミド、N,N−ジ
メチルアクリルアミド等のアクリルアミド共重合体;メ
タクリルアミド、N−メチルメタクリルアミド、N−エ
チルメタクリルアミド、N,N−ジメチルメタクリルア
ミド等のメタクリルアミド共重合体;メチルビニルエ−
テル、tーブチルビニルエ−テル、ドデシルビニルエ−
テル等のビニルエ−テル系単量体;アリルアルコール;
ビニルトリメトキシシラン;N−ビニル−2−ピロリド
ン等が挙げられる。
[0006] The EVOH may contain other copolymer components as long as the object of the present invention is not hindered. Here, as another component, an olefin monomer such as propylene, 1-butene, isobutene; an acrylamide copolymer such as acrylamide, N-methylacrylamide, N-ethylacrylamide, N, N-dimethylacrylamide; methacrylamide Methacrylamide copolymers such as N, N-methylmethacrylamide, N-ethylmethacrylamide, N, N-dimethylmethacrylamide;
Ter, t-butyl vinyl ether, dodecyl vinyl ether
Vinyl ether monomers such as ter; allyl alcohol;
Vinyltrimethoxysilane; N-vinyl-2-pyrrolidone;

【0007】また本発明に用いるEVOHの好適な重合
度としては、フェノール85重量%および水15重量%
の混合溶媒中30℃における極限粘度が0.1〜5デシ
リッター/g(以下、dl/gと略記する)が好まし
く、0.2〜2dl/gがより好ましい。
The preferred degree of polymerization of EVOH used in the present invention is 85% by weight of phenol and 15% by weight of water.
The intrinsic viscosity in a mixed solvent of 30 ° C. is preferably 0.1 to 5 desilitters / g (hereinafter abbreviated as dl / g), more preferably 0.2 to 2 dl / g.

【0008】本発明に使用するカルボキシル基、カルボ
ン酸誘導体基、ケイ素含有基、エポキシ基、スルホン酸
塩基、ホスホン酸塩基からなる群から選ばれる官能基を
末端に有するオレフィン系重合体(B)とは、カルボキ
シル基、カルボン酸誘導体基、ケイ素原子を含む官能
基、エポキシ基、スルホン酸塩基、ホスホン酸塩基から
なる群選ばれる官能基を片末端または両末端に有するオ
レフィン系重合体である。
[0008] The olefin polymer (B) having a functional group selected from the group consisting of a carboxyl group, a carboxylic acid derivative group, a silicon-containing group, an epoxy group, a sulfonate group and a phosphonate group used in the present invention. Is an olefin polymer having at one or both terminals a functional group selected from the group consisting of a carboxyl group, a carboxylic acid derivative group, a functional group containing a silicon atom, an epoxy group, a sulfonate group and a phosphonate group.

【0009】本発明においてカルボキシル基およびカル
ボン酸誘導体基の例としては、カルボキシル基、下記一
般式(I)で示されるカルボン酸金属塩基、下記一般式
(II)で示される環状カルボン酸無水物基が挙げられ
る。本発明においてケイ素含有基の例としては、下記一
般式(III)で示されるシリルエーテル誘導体基が挙
げられる。また本発明においてエポキシ基は下記一般式
(IV)で示される。本発明にスルホン酸塩基は下記一
般式(V)で示される。本発明においてホスホン酸塩基
は下記一般式(VI)および下記一般式(VII)で示
される。
In the present invention, examples of the carboxyl group and the carboxylic acid derivative group include a carboxyl group, a carboxylate metal base represented by the following general formula (I), and a cyclic carboxylic anhydride group represented by the following general formula (II) Is mentioned. In the present invention, examples of the silicon-containing group include a silyl ether derivative group represented by the following general formula (III). In the present invention, the epoxy group is represented by the following general formula (IV). In the present invention, the sulfonate group is represented by the following general formula (V). In the present invention, the phosphonate groups are represented by the following general formula (VI) and the following general formula (VII).

【0010】[0010]

【化1】 Embedded image

【0011】[0011]

【化2】 Embedded image

【0012】[0012]

【化3】 Embedded image

【0013】[0013]

【化4】 Embedded image

【0014】[0014]

【化5】 Embedded image

【0015】[0015]

【化6】 Embedded image

【0016】[0016]

【化7】 Embedded image

【0017】(式中、nは1または2を表わす。Mはア
ルカリ金属またはアルカリ土類金属または亜鉛を表わ
す。X,Y,Zのうち少なくとも一つがアルコキシル基
を表わし、残りはメチル基、エチル基、プロピル基等の
脂肪族炭化水素基または芳香族炭化水素基を表わす。R
↑1,R↑2,R↑3は水素原子または低級アルキル基
を表わす。)
(In the formula, n represents 1 or 2. M represents an alkali metal or an alkaline earth metal or zinc. At least one of X, Y and Z represents an alkoxyl group, and the rest is a methyl group and an ethyl group. And an aliphatic hydrocarbon group such as a propyl group or an aromatic hydrocarbon group.
{1, R} 2 and R} 3 represent a hydrogen atom or a lower alkyl group. )

【0018】一般式(I)および一般式(V)〜(VI
I)で示されるカルボン酸塩基、スルホン酸塩基、ホス
ホン酸塩基の金属塩の具体例としては、ナトリウム塩、
カリウム塩等のアルカリ金属塩;マグネシウム、カルシ
ウム塩等のアルカリ土類金属塩、亜鉛塩が挙げられる。
Formulas (I) and (V) to (VI)
Specific examples of the metal salts of the carboxylate, sulfonic and phosphonate groups represented by I) include sodium salts,
Alkali metal salts such as potassium salts; alkaline earth metal salts such as magnesium and calcium salts; and zinc salts.

【0019】一般式(II)で示される環状カルボン酸
無水物基中の置換基R↑1,R↑2,R↑3の具体例と
しては、メチル基、エチル基、プロピル基等の低級脂肪
族炭化水素基および水素原子が挙げられる。これらのな
かで特に好適な例としては、R↑1,R↑2,R↑3が
すべて水素原子の場合が挙げられる。
Specific examples of the substituents R ↑ 1, R ↑ 2, and R ↑ 3 in the cyclic carboxylic anhydride group represented by the general formula (II) include lower fatty acids such as methyl, ethyl and propyl. Group hydrocarbon groups and hydrogen atoms. Of these, particularly preferred examples include a case where all of R ↑ 1, R ↑ 2, and R ↑ 3 are hydrogen atoms.

【0020】一般式(III)で示されるシリルエーテ
ル誘導体基中の置換基X,Y,Zの具体例としては、メ
トキシ基、エトキシ基、プロポキシ基、ブトキシ基等の
アルコキシ基;メチル基、エチル基、プロピル基、ブチ
ル基等の脂肪族炭化水素基;フェニル基等の芳香族炭化
水素基が挙げられる。特に好適な例として、R↑1,R
↑2,R↑3がすべてメトキシ基である場合、R↑1,
R↑2,R↑3がすべてエトキシ基である場合、R↑
1,R↑2がメトキシ基でR↑3がメチル基である場合
が挙げられる。
Specific examples of the substituents X, Y and Z in the silyl ether derivative group represented by the general formula (III) include an alkoxy group such as a methoxy group, an ethoxy group, a propoxy group and a butoxy group; a methyl group and an ethyl group. And aliphatic hydrocarbon groups such as a propyl group and a butyl group; and aromatic hydrocarbon groups such as a phenyl group. As a particularly preferred example, R ↑ 1, R
When {2, R} 3 are all methoxy groups,
When R 場合 2 and R ↑ 3 are all ethoxy groups,
1, R ↑ 2 is a methoxy group and R ↑ 3 is a methyl group.

【0021】前記官能基はポリオレフィン系重合体の実
質的に片末端あるいは両末端のみに存在していることが
好ましい。前記官能基の量は0.0001〜1meq/
g(ミリ等量/g)が好ましく、特に0.001〜0.
1meq/gの範囲が好ましい。
It is preferable that the functional group is present at substantially only one end or both ends of the polyolefin polymer. The amount of the functional group is 0.0001 to 1 meq /
g (milli-equivalent / g) is preferable, and particularly 0.001 to 0.
A range of 1 meq / g is preferred.

【0022】本発明に使用するカルボン酸誘導体基、含
ケイ素官能基、エポキシ基、スルホン酸塩基、ホスホン
酸塩基からなる群から選ばれる官能基を末端に有するオ
レフィン系重合体(B)を構成する単量体単位の具体例
としては、エチレン、プロピレン、1−ブテン、1−ペ
ンテン、4−メチル−1−ペンテン、1−ヘキセン、1
−ヘプテン、1−オクテン、1−ノネン、1−デセン等
が挙げられ、本発明のオレフィン系重合体(B)は上記
のオレフィン系単量体から選ばれる一つの単量体の単独
の重合体あるいは上記のオレフィン系単量体の共重合体
(ランダム共重合体、ブロック共重合体)あるいは上記
の単量体以外の単量体を共重合成分として含む共重合体
(ランダム共重合体、ブロック共重合体)が挙げられる
が、オレフィン系単量の重合体中に占める含有率は50
重量%以上が好ましく、80重量%以上がさらに好まし
い。上記オレフィン系単量体以外の構成成分としては、
アクリル酸メチル、アクリル酸エチル、アクリル酸ブチ
ル等のアクリル酸エステル系単量体;メタクリル酸メチ
ル、メタクリル酸エチル、メタクリル酸ブチル等のメタ
クリル酸エステル系単量体;酢酸ビニル、ピバリン酸ビ
ニル等のビニルエステル系単量体;塩化ビニル、塩化ビ
ニリデン、フッ化ビニル等が挙げられる。
The olefin polymer (B) having a functional group selected from the group consisting of a carboxylic acid derivative group, a silicon-containing functional group, an epoxy group, a sulfonate group and a phosphonate group used in the present invention is provided. Specific examples of the monomer unit include ethylene, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene,
-Heptene, 1-octene, 1-nonene, 1-decene, etc., and the olefin polymer (B) of the present invention is a homopolymer of one monomer selected from the above olefin monomers. Alternatively, a copolymer of the above-mentioned olefin-based monomer (random copolymer, block copolymer) or a copolymer containing a monomer other than the above-mentioned monomer as a copolymer component (random copolymer, block copolymer) Copolymer), but the content of the olefin-based monomer in the polymer is 50%.
% By weight or more, more preferably 80% by weight or more. As a component other than the olefin-based monomer,
Acrylate monomers such as methyl acrylate, ethyl acrylate and butyl acrylate; methacrylate monomers such as methyl methacrylate, ethyl methacrylate and butyl methacrylate; vinyl acetate and vinyl pivalate Vinyl ester-based monomers: vinyl chloride, vinylidene chloride, vinyl fluoride and the like.

【0023】上記の単量体により構成される、オレフィ
ン系共重合体(B)のベースポリマーのうち、特にエチ
レン系重合体(超低密度ポリエチレン、低密度ポリエチ
レン、中密度ポリエチレン、高密度ポリエチレン、直鎖
状低密度ポリエチレン、エチレン酢酸ビニル−共重合
体、エチレン−アクリル酸エステル共重合体、エチレン
−プロピレン共重合体等)、プロピレン系共重合体が好
適なものとして挙げられる。
Among the base polymers of the olefin copolymer (B) composed of the above-mentioned monomers, particularly, ethylene polymers (ultra low density polyethylene, low density polyethylene, medium density polyethylene, high density polyethylene, Suitable examples include a linear low-density polyethylene, an ethylene-vinyl acetate-copolymer, an ethylene-acrylate copolymer, an ethylene-propylene copolymer, and a propylene-based copolymer.

【0024】本発明に使用するオレフィン系重合体重合
体(B)の好適なメルトインデックス(MI)(190
℃、2160g荷重下で測定した値)は0.01〜10
00g/10分が好ましく、0.1〜100g/10分
がより好ましい。
Suitable melt index (MI) (190) of the olefin polymer (B) used in the present invention.
° C, a value measured under a load of 2160 g) is 0.01 to 10
00 g / 10 min is preferable, and 0.1 to 100 g / 10 min is more preferable.

【0025】次に本発明に用いるカルボン酸誘導体基、
含ケイ素官能基、エポキシ基、スルホン酸塩基、ホスホ
ン酸塩基からなる群から選ばれる官能基を末端に有する
オレフィン系重合体(B)の代表的製法について述べ
る。本発明に用いるカルボン酸誘導体基、含ケイ素官能
基、エポキシ基、スルホン酸塩基、ホスホン酸塩基から
なる群から選ばれる官能基を末端に有するオレフィン系
重合体(B)は末端に二重結合を有するポリオレフィン
の末端の二重結合を官能基変換することによって得られ
る。
Next, the carboxylic acid derivative group used in the present invention,
A typical method for producing an olefin polymer (B) having a terminal having a functional group selected from the group consisting of a silicon-containing functional group, an epoxy group, a sulfonate group and a phosphonate group will be described. The olefin polymer (B) having a functional group selected from the group consisting of a carboxylic acid derivative group, a silicon-containing functional group, an epoxy group, a sulfonate group and a phosphonate group at the terminal used in the present invention has a double bond at the terminal. It is obtained by converting a terminal double bond of a polyolefin having a functional group.

【0026】原料の二重結合を有するオレフィン系重合
体の代表的製法としては、1)通常のオレフィン系重合
体の末端に微量に存在する二重結合を利用する方法;
2)通常のオレフィン系重合体を無酸素条件下、熱分解
し、末端に二重結合を有するオレフィン系重合体を得る
製法;が挙げられる。1)については、公知のオレフィ
ン系重合体の製法を用いることができるが、特に、連鎖
移動剤として水素を用いず、重合触媒としてメタロセン
系重合触媒を用いる製法(例えば、DE403039
9)が好ましい。2)については、公知の方法(例えば
US2835659,3087922)によりオレフィ
ン系重合体を窒素雰囲気下や真空条件下等の無酸素条件
下で300℃〜500℃の温度で熱分解することによっ
て得られる。
As a typical method for producing an olefin polymer having a double bond as a raw material, 1) a method utilizing a trace amount of a double bond existing at a terminal of an ordinary olefin polymer;
2) A method for producing an olefin polymer having a double bond at a terminal by thermally decomposing an ordinary olefin polymer under oxygen-free conditions. For 1), a known method for producing an olefin polymer can be used. In particular, a method using a metallocene-based polymerization catalyst as a polymerization catalyst without using hydrogen as a chain transfer agent (for example, DE 403039).
9) is preferred. The method 2) can be obtained by thermally decomposing an olefin-based polymer at a temperature of 300 to 500 ° C. under an oxygen-free condition such as a nitrogen atmosphere or a vacuum condition by a known method (for example, US Pat. No. 2,835,559, 3087922).

【0027】末端にカルボキシル基を有するオレフィン
系重合体はベンゼン、トルエン、キシレン等の炭化水素
系溶媒中、アゾ系あるいは過酸化物系ラジカル開始剤存
在下で、末端に二重結合を有するポリオレフィンにチオ
グリコール酸、2−メルカプトプロピオン酸等のチオー
ル基を有するカルボン酸を付加させることによって得ら
れる。また、末端にカルボン酸塩基を有するオレフィン
系重合体は末端にカルボキシル基を有するオレフィン系
重合体を水酸化ナトリウム、炭酸ナトリウム、水酸化カ
リウム等の金属水酸化物、金属炭酸塩等により中和する
ことによって得られる。
An olefin polymer having a terminal carboxyl group can be converted to a polyolefin having a terminal double bond in a hydrocarbon solvent such as benzene, toluene or xylene in the presence of an azo or peroxide radical initiator. It is obtained by adding a carboxylic acid having a thiol group such as thioglycolic acid or 2-mercaptopropionic acid. Further, the olefin polymer having a carboxylic acid group at the terminal neutralizes the olefin polymer having a carboxyl group at the terminal with a metal hydroxide such as sodium hydroxide, sodium carbonate, potassium hydroxide, or a metal carbonate. Obtained by:

【0028】末端にカルボン酸無水物基を有するオレフ
ィン系重合体は末端に二重結合を有するオレフィン系重
合体とマレイン酸無水物、シトラコン酸無水物、イタコ
ン酸無水物等の不飽和カルボン酸無水物とを加熱反応さ
せることによって得られる。
The olefin polymer having a carboxylic acid anhydride group at the terminal is an olefin polymer having a double bond at the terminal and an unsaturated carboxylic acid anhydride such as maleic anhydride, citraconic anhydride, itaconic anhydride and the like. It is obtained by reacting a substance with heat.

【0029】末端に含ケイ素官能基を有するオレフィン
系重合体はベンゼン、トルエン、キシレン等の炭化水素
系溶媒中、ヘキサクロロ白金酸あるいはラジカル開始剤
存在下、末端に二重結合を有するポリオレフィンにトリ
メトキシシラン、トリエトキシシラン、ジメトキシメチ
ルシラン等のケイ素−水素結合を有するシラン化合物を
付加させることによって得られる。
An olefin polymer having a silicon-containing functional group at a terminal is converted to a polyolefin having a double bond at a terminal in a hydrocarbon solvent such as benzene, toluene, or xylene in the presence of hexachloroplatinic acid or a radical initiator. It is obtained by adding a silane compound having a silicon-hydrogen bond such as silane, triethoxysilane, dimethoxymethylsilane, and the like.

【0030】末端にスルホン酸塩基を有するポリオレフ
ィンはラジカル開始剤存在下で末端に二重結合を有する
ポリオレフィンにチオ酢酸を付加させ、さらにアルカリ
触媒存在下、メタノールを反応させることにより末端に
チオール基を有するポリオレフィンを得た後、さらにこ
れを次亜塩素酸ナトリウム等により酸化することによっ
て得られる。
The polyolefin having a sulfonic acid group at the terminal is obtained by adding thioacetic acid to a polyolefin having a double bond at the terminal in the presence of a radical initiator and then reacting with methanol in the presence of an alkali catalyst to form a thiol group at the terminal. After obtaining the polyolefin having, it is obtained by further oxidizing it with sodium hypochlorite or the like.

【0031】末端にエポキシ基を有するオレフィン系重
合体は末端に二重結合を有するオレフィン系重合体に過
酢酸、m−クロロ過安息香酸等の過酸を反応させること
によって得られる。
The olefin polymer having an epoxy group at the terminal can be obtained by reacting an olefin polymer having a double bond at the terminal with a peracid such as peracetic acid or m-chloroperbenzoic acid.

【0032】末端にホスホン酸塩基を有するオレフィン
系重合体はラジカル開始剤存在下で末端に二重結合を有
するオレフィン系重合体にホスホン酸ジアルキルエステ
ルを反応させることによって末端にホスホン酸ジアルキ
ルエステル基を有するオレフィン系重合体を得た後、塩
化水素によりを反応させ、さらに中和することによって
得られる。
The olefin polymer having a phosphonate group at the terminal is reacted with the dialkyl phosphonate to the olefin polymer having a double bond at the terminal in the presence of a radical initiator to form a dialkyl phosphonate group at the terminal. After obtaining an olefin polymer having the olefin polymer, the obtained olefin polymer is reacted with hydrogen chloride and further neutralized.

【0033】本発明の樹脂組成物は、前記したEVOH
(A)およびカルボン酸誘導体基、含ケイ素官能基、エ
ポキシ基、スルホン酸塩基、ホスホン酸塩基からなる群
より選ばれる官能基を末端に有するオレフィン系重合体
(B)からなり、成分(A)と成分(B)の重量配合比
は、99:1から1:99が好ましく、95:5から
5:99がより好ましい。成分(A)の特性、例えばガ
スバリア−性、耐溶剤性をより強く発揮させたい場合
は、(A):(B)は95:5〜50:50であること
が好ましく、成分(B)の特徴、例えば耐熱水性、機械
的特性をより強く発揮させたい場合は(A):(B)は
5:95〜50:50であることが好ましい。成分
(B)のベ−スポリマ−としてプロピレン系重合体を使
用する場合は、後述する実施例からも明らかなように、
耐熱水性が改善されるため、耐熱水性の要求される分
野、例えばレトルト用包装材料として極めて有用であ
る。また成分(B)のベ−スポリマ−として、エチレン
系重合体を使用する場合は、後述する実施例からも明ら
かなように、耐衝撃性が改善されるため、耐衝撃性が要
求される分野、例えばボトル、チュ−ブ、カップ、パウ
チ等の包装材料として有用である。
The resin composition of the present invention comprises the above-described EVOH
(A) and an olefin polymer (B) having a functional group selected from the group consisting of a carboxylic acid derivative group, a silicon-containing functional group, an epoxy group, a sulfonate group, and a phosphonate group at the terminal, and the component (A) The weight ratio of component to component (B) is preferably from 99: 1 to 1:99, more preferably from 95: 5 to 5:99. When it is desired to further exhibit the properties of the component (A), for example, gas barrier properties and solvent resistance, the ratio of (A) :( B) is preferably from 95: 5 to 50:50. When it is desired to exhibit characteristics such as hot water resistance and mechanical properties more strongly, (A) :( B) is preferably from 5:95 to 50:50. When a propylene-based polymer is used as the base polymer of the component (B), as will be apparent from Examples described later,
Since the hot water resistance is improved, it is extremely useful as a field requiring hot water resistance, for example, as a retort packaging material. When an ethylene-based polymer is used as the base polymer of the component (B), the impact resistance is improved as will be apparent from the examples described later, and thus the field requiring impact resistance is required. For example, it is useful as a packaging material for bottles, tubes, cups, pouches and the like.

【0034】本発明の樹脂組成物は、周知の溶融成形方
法(T−ダイ押出、インフレ−ション押出、ブロ−成
形、射出成形、プレス成形)で容易に成形可能であり、
フィルム、シ−ト、チュ−ブ、ボトル、繊維、棒、管な
ど任意の成形品に成形することができる。
The resin composition of the present invention can be easily molded by well-known melt molding methods (T-die extrusion, inflation extrusion, blow molding, injection molding, press molding).
It can be formed into an arbitrary molded product such as a film, a sheet, a tube, a bottle, a fiber, a rod, and a tube.

【0035】また、本発明の樹脂組成物は、EVOH層
と熱可塑性樹脂(ポリオレフィン等)層とを有する多層
構造体、例えばEVOH層/熱可塑性樹脂層からなる多
層構造体、熱可塑性樹脂層/EVOH層/熱可塑性樹脂
層からなる多層構造体からフィルム、シ−ト、チュ−
ブ、ボトル等を製造する際に発生するスクラップに本発
明に使用する成分(B)を配合して使用する態様も含ま
れる。また本発明の樹脂組成物は、他の熱可塑性樹脂、
例えば前記した成分(B)のベ−スポリマ−のオレフィ
ン系重合体、さらにはポリエステル(ポリエチレンエチ
レンテレフタレ−ト、ポリブチレンテレフタレ−ト
等)、ポリアミド、ポリカ−ボネ−ト、ポリ塩化ビニ
ル、ポリウレタン、ポリアセタ−ル、EVOH等との多
層構造体として好適に用いられる。多層構造体は共押
出、共射出、押出コ−ティング等公知の方法で成形さ
れ、またこれらの成形品のスクラップを再使用すること
もできるし、またスクラップを再使用する場合、本発明
の樹脂組成物をスクラップ中に配合すること、あるいは
本発明で用いる成分(B)をスクラップ中に配合するこ
ともできる。
Further, the resin composition of the present invention is a multilayer structure having an EVOH layer and a thermoplastic resin (polyolefin or the like) layer, for example, a multilayer structure comprising an EVOH layer / thermoplastic resin layer, a thermoplastic resin layer / From multilayer structure consisting of EVOH layer / thermoplastic resin layer to film, sheet, tube
The present invention also includes an embodiment in which the component (B) used in the present invention is blended and used with scrap generated in the production of plastics, bottles and the like. Further, the resin composition of the present invention, other thermoplastic resin,
For example, the olefin polymer of the base polymer of the component (B) described above, further, polyester (polyethylene ethylene terephthalate, polybutylene terephthalate, etc.), polyamide, polycarbonate, polyvinyl chloride, It is suitably used as a multilayer structure with polyurethane, polyacetal, EVOH and the like. The multilayer structure is formed by a known method such as co-extrusion, co-injection, extrusion coating, etc., and the scrap of these molded products can be reused. When the scrap is reused, the resin of the present invention is used. The composition can be compounded in scrap, or the component (B) used in the present invention can be compounded in scrap.

【0036】多層構造体を得る場合、本発明の樹脂組成
物層と熱可塑性樹脂層に接着性樹脂層を介在させること
が両層を強固に接着せしめることができるので好ましい
場合が多い。ここで接着性樹脂としては、両層を強固に
接着するものであれば、特に限定されるものではない
が、不飽和カルボン酸またはその無水物(無水マレイン
酸など)をオレフィン系重合体または共重合体[ポリエ
チレン{低密度ポリエチレン、直線状低密度ポリエチレ
ン(LLDPE)、超低密度ポリエチレン(SLDP
E)}、エチレン−酢酸ビニル共重合体、エチレン−
(メタ)アクリル酸共重合体、エチレン−(メタ)アク
リル酸エステル(メチルエステルまたはエチルエステ
ル)共重合体、ポリプロピレンなど]にグラフトしたも
の、水素化スチレン−ブタジエン共重合体の酸無水物
(例無水マレイン酸)変性物、液状ブタジエンの酸無水
物変性物、エチレン−プロピレン−ジエン共重合体の酸
無水物変性物等のジエン系重合体酸無水物変性物等が好
適に用いられる。
In the case of obtaining a multilayer structure, it is often preferable to interpose an adhesive resin layer between the resin composition layer of the present invention and the thermoplastic resin layer because both layers can be firmly bonded. Here, the adhesive resin is not particularly limited as long as it strongly adheres both layers, but the unsaturated carboxylic acid or its anhydride (maleic anhydride or the like) may be an olefin polymer or a copolymer. Polymers [Polyethylene @ low density polyethylene, linear low density polyethylene (LLDPE), ultra low density polyethylene (SLDP)
E)}, ethylene-vinyl acetate copolymer, ethylene-
(Meth) acrylic acid copolymer, ethylene- (meth) acrylic acid ester (methyl ester or ethyl ester) copolymer, polypropylene, etc.], and hydrogenated styrene-butadiene copolymer acid anhydride (eg, Modified products of maleic anhydride), modified acid anhydrides of liquid butadiene, modified acid anhydrides of diene polymers such as modified acid anhydrides of ethylene-propylene-diene copolymer and the like are preferably used.

【0037】多層構造体の層構成としては、樹脂組成物
層/熱可塑性樹脂層、樹脂組成物層/熱可塑性樹脂層/
樹脂組成物層、熱可塑性樹脂層/樹脂組成物層/熱可塑
性樹脂層、熱可塑性樹脂層/樹脂組成物層/スクラップ
回収層/熱可塑性樹脂層、熱可塑性樹脂層/スクラップ
回収層/樹脂組成物層/スクラップ回収層/熱可塑性樹
脂層、あるいはこれらの層の少なくとも一つの層間に前
記した接着性樹脂層を介在させたものが挙げられる。
The layer structure of the multilayer structure is as follows: resin composition layer / thermoplastic resin layer, resin composition layer / thermoplastic resin layer /
Resin composition layer, thermoplastic resin layer / resin composition layer / thermoplastic resin layer, thermoplastic resin layer / resin composition layer / scrap collecting layer / thermoplastic resin layer, thermoplastic resin layer / scrap collecting layer / resin composition Material layer / scrap recovery layer / thermoplastic resin layer, or those in which the above-mentioned adhesive resin layer is interposed between at least one of these layers.

【0038】前記した本発明の樹脂組成物より得た成形
物、多層構造体は、ガスバリア−性の要求される食品、
医薬、医療器材、衣料などの包装材料として特に有用で
ある。
Molded articles and multilayer structures obtained from the above-mentioned resin composition of the present invention can be used for foods requiring gas barrier properties,
It is particularly useful as a packaging material for pharmaceuticals, medical equipment, clothing, and the like.

【0039】[0039]

【実施例】以下、実施例により本発明をさらに詳しく説
明するが、これらの実施例によって本発明は何ら限定さ
れるものではない。なお、以下の合成例および実施例に
おいて特に断りのない限り、比率は重量比を、「%」は
「重量%」を意味する。またメルトインデックス(以下
MIと略す)は断りのない限り190℃で荷重2160
gで測定したものである。また固有粘度はフェノ−ル8
5重量%および水15重量%の混合溶媒(以下含水フェ
ノ−ルと略記する)中30℃における極限粘度である。
ポリオレフィン中の二重結合量は、重パラキシレンを溶
媒として用い、270MHz1H−NMRにより定量し
た。ポリオレフィン中のナトリウム、リンおよび硫黄含
量はX線蛍光分析により測定した。またポリオレフィン
中のトリメトキシシリル基の量はNMRにより測定し
た。
The present invention will be described in more detail with reference to the following Examples, which should not be construed as limiting the invention thereto. In the following Synthesis Examples and Examples, unless otherwise specified, the ratio means the weight ratio, and “%” means “% by weight”. The melt index (hereinafter abbreviated as MI) was measured at 190 ° C. under a load of 2160 unless otherwise noted.
g. The intrinsic viscosity is phenol 8
It is the intrinsic viscosity at 30 ° C. in a mixed solvent of 5% by weight and 15% by weight of water (hereinafter abbreviated as hydrated phenol).
The amount of double bonds in the polyolefin was determined by 270 MHz 1H-NMR using heavy para-xylene as a solvent. The sodium, phosphorus and sulfur contents in the polyolefin were measured by X-ray fluorescence analysis. The amount of trimethoxysilyl groups in the polyolefin was measured by NMR.

【0040】合成例1 二重結合を末端に有するポリプロピレンの合成:セパラ
ブルフラスコにポリプロピレン{MI(230℃、荷重
2160g)0.3g/10分}200gを仕込み、真
空下でバス温を250℃で1時間加熱後、さらにバス温
を340℃に昇温後2時間加熱を行なった。冷却後、ポ
リプロピレンを取り出し、粉砕することにより、二重結
合量0.031meq/g、MI80g/10分の末端
に二重結合を有するポリプロピレンを得た。
Synthesis Example 1 Synthesis of polypropylene having a double bond at the terminal: 200 g of polypropylene {MI (230 ° C., load 2160 g) 0.3 g / 10 minutes} 200 g was charged into a separable flask, and the bath temperature was raised to 250 ° C. under vacuum. After heating for 1 hour, the bath temperature was further raised to 340 ° C., and then heating was performed for 2 hours. After cooling, the polypropylene was taken out and pulverized to obtain a polypropylene having a double bond amount of 0.031 meq / g and MI having a double bond at a terminal of 80 g / 10 min.

【0041】合成例2 カルボン酸無水物基を末端に有するポリプロピレンの合
成:冷却器および撹拌機付きのセパラブルフラスコに合
成例1で得られたポリプロピレン20重量部、無水マレ
イン酸50重量部を仕込み、窒素置換を行なった後、2
10℃で4時間反応を行なった。得られたポリマーをセ
トンのにより良く洗浄後、乾燥することによって無水マ
レイン酸基量0.026meq/g、MI80g/10
分のポリプロピレンを得た。
Synthesis Example 2 Synthesis of Polypropylene Having Carboxylic Anhydride Group at the Terminal: A separable flask equipped with a condenser and a stirrer was charged with 20 parts by weight of the polypropylene obtained in Synthesis Example 1 and 50 parts by weight of maleic anhydride. , After purging with nitrogen, 2
The reaction was performed at 10 ° C. for 4 hours. The resulting polymer was washed well with seton and dried to obtain a maleic anhydride group content of 0.026 meq / g and MI of 80 g / 10.
Minutes of polypropylene.

【0042】合成例3 末端に二重結合を有する低密度ポリエチレンの合成:窒
素シール付きフィーダーおよびベントを有するセグメン
ト型25φ二軸押出機(D/L=25)を用い、低密度
ポリエチレン(MI=0.3g/10分)をスクリュー
回転数200rpm、スクリュー部温度390℃、ダイ
温度270℃、吐出量1.2Kg/hで熱分解すること
により、二重結合量0.03meq/g、MI10g/
10分の末端に二重結合を有するポリエチレンを得た。
Synthesis Example 3 Synthesis of low-density polyethylene having a double bond at a terminal: Using a segment type 25φ twin-screw extruder (D / L = 25) having a feeder with a nitrogen seal and a vent, a low-density polyethylene (MI = 0.3 g / 10 min) by thermal decomposition at a screw rotation speed of 200 rpm, a screw temperature of 390 ° C., a die temperature of 270 ° C., and a discharge rate of 1.2 kg / h.
A polyethylene having a double bond at the terminal for 10 minutes was obtained.

【0043】合成例4 末端にカルボン酸塩基を有する低密度ポリエチレンの合
成:撹拌機および冷却器を有するセパラブルフラスコに
合成例3の末端に二重結合を有するポリエチレン100
重量部、3−メルカプトプロピオン酸20重量部および
キシレン200重量部を仕込み、窒素置換を行った。1
30℃に加熱後、別途調製した3%アゾビスイソブチロ
ニトリル/キシレン溶液20重量部を滴下した。反応溶
液を冷却後、ゲル状ポリエチレンをアセトンにより良く
洗浄し、0.2%水酸化ナトリウム/メタノール溶液に
より中和後、メタノールにより洗浄、さらに乾燥するこ
とにより、ナトリウム含量量0.55%、MI7g/1
0分の末端にカルボン酸塩基を有するポリオレフィンを
得た。
Synthesis Example 4 Synthesis of low-density polyethylene having a carboxylic acid group at the end: in a separable flask having a stirrer and a cooler, polyethylene 100 having a double bond at the end of Synthesis Example 3
Parts by weight, 20 parts by weight of 3-mercaptopropionic acid, and 200 parts by weight of xylene were charged and subjected to nitrogen replacement. 1
After heating to 30 ° C., 20 parts by weight of a separately prepared 3% azobisisobutyronitrile / xylene solution was added dropwise. After cooling the reaction solution, the gel polyethylene was thoroughly washed with acetone, neutralized with a 0.2% sodium hydroxide / methanol solution, washed with methanol, and further dried to obtain a sodium content of 0.55% and MI of 7 g. / 1
A polyolefin having a carboxylate group at the 0-minute end was obtained.

【0044】合成例5 末端にホスホン酸塩基を有する低密度ポリエチレンの合
成:撹拌機および冷却器を有するセパラブルフラスコに
合成例3の末端に二重結合を有するポリエチレン100
重量部、ホスホン酸ジメチルエステル25重量部および
キシレン200重量部を仕込み、窒素置換を行った。1
30℃に加熱後、別途調製した3%アゾビスイソブチロ
ニトリルのキシレン溶液20重量部を滴下した。反応溶
液を冷却後、ゲル状ポリエチレンをアセトンにより良く
洗浄、さらに乾燥した。これによって得られた、ホスホ
ン酸ジメチルエステル基を有するポリエチレンを塩化水
素雰囲気下で100℃1時間加熱後、0.2%水酸化ナ
トリウムメタノール溶液により中和後、メタノールおよ
び蒸留水により良く洗浄し、さらに乾燥することによ
り、リン含量0.75%、MI5g/10分の末端にホ
スホン酸塩基を有する低密度ポリエチレンを得た。
Synthesis Example 5 Synthesis of Low Density Polyethylene Having Phosphonate Group at Terminal: In a separable flask having a stirrer and a cooler, polyethylene 100 having a double bond at the terminal of Synthesis Example 3
Parts by weight, 25 parts by weight of dimethyl phosphonate and 200 parts by weight of xylene were charged and subjected to nitrogen replacement. 1
After heating to 30 ° C., 20 parts by weight of a separately prepared 3% azobisisobutyronitrile xylene solution was added dropwise. After cooling the reaction solution, the gel-like polyethylene was thoroughly washed with acetone and dried. The obtained polyethylene having a phosphonic acid dimethyl ester group was heated at 100 ° C. for 1 hour in a hydrogen chloride atmosphere, neutralized with a 0.2% methanol solution of sodium hydroxide, and thoroughly washed with methanol and distilled water. By further drying, low-density polyethylene having a phosphorus content of 0.75% and a phosphonate group at a terminal of 5 g / 10 min of MI was obtained.

【0045】合成例6 末端にトリメトキシシリル基を有する低密度ポリエチレ
ンの合成:撹拌機および冷却器を有するセパラブルフラ
スコに合成例3の末端に二重結合を有するポリエチレン
100重量部、ホスホン酸ジメチルエステル25重量部
およびキシレン200重量部を仕込み、窒素置換を行っ
た。130℃に加熱後、別途調製した3%アゾビスイソ
ブチロニトリル/キシレン溶液20重量部を滴下した。
反応溶液を冷却後、ゲル状ポリエチレンをアセトンによ
り良く洗浄、さらに乾燥した。これによって得られた、
ホスホン酸ジメチルエステル基を有するポリエチレンを
塩化水素雰囲気下で100℃1時間加熱後、0.2%水
酸化ナトリウムのメタノール溶液により中和後、メタノ
ールおよび蒸留水により良く洗浄し、さらに乾燥するこ
とにより、リン含量0.75%、MI5g/10分の末
端にホスホン酸塩基を有する低密度ポリエチレンを得
た。
Synthesis Example 6 Synthesis of low-density polyethylene having a trimethoxysilyl group at the end: 100 parts by weight of polyethylene having a double bond at the end of Synthesis Example 3 in a separable flask having a stirrer and a cooler, dimethyl phosphonate 25 parts by weight of the ester and 200 parts by weight of xylene were charged and the atmosphere was replaced with nitrogen. After heating to 130 ° C., 20 parts by weight of a separately prepared 3% azobisisobutyronitrile / xylene solution was added dropwise.
After cooling the reaction solution, the gel-like polyethylene was thoroughly washed with acetone and dried. This resulted in
Polyethylene having a phosphonic acid dimethyl ester group is heated in a hydrogen chloride atmosphere at 100 ° C. for 1 hour, neutralized with a methanol solution of 0.2% sodium hydroxide, thoroughly washed with methanol and distilled water, and further dried. A low-density polyethylene having a phosphonate group at the terminal with a phosphorus content of 0.75% and MI of 5 g / 10 min was obtained.

【0046】合成例7 末端にスルホン酸塩基を有する低密度ポリエチレンの合
成:撹拌機および冷却器を有するセパラブルフラスコに
合成例3の末端に二重結合を有するポリエチレン100
重量部、チオ酢酸10重量部およびキシレン200重量
部を仕込み、窒素置換を行った。100℃に加熱後、別
途調製した3%アゾビスイソブチロニトリルのキシレン
溶液20重量部を滴下した。反応溶液を冷却後、ゲル状
ポリエチレンをアセトンにより良く洗浄し、さらに乾燥
した。得られたポリマー90重量部および1%水酸化ナ
トリウムのメタノール溶液200重量部を冷却器付きフ
ラスクに仕込み、窒素置換後、60℃2時間加熱した。
得られたポリマーを蒸留水で洗浄後、2%次亜塩素酸ナ
トリウム水溶液200重量部に1日間漬け、水およびメ
タノールで良く洗浄、さらに乾燥することにより、硫黄
含量0.7%、MI6g/10分の末端にスルホン酸塩
基を有する低密度ポリエチレンを得た。
Synthesis Example 7 Synthesis of low-density polyethylene having a sulfonate group at the end: in a separable flask having a stirrer and a cooler, polyethylene 100 having a double bond at the end of Synthesis Example 3
Parts by weight, 10 parts by weight of thioacetic acid and 200 parts by weight of xylene were charged and purged with nitrogen. After heating to 100 ° C., 20 parts by weight of a separately prepared 3% azobisisobutyronitrile xylene solution was added dropwise. After cooling the reaction solution, the gel-like polyethylene was thoroughly washed with acetone and dried. 90 parts by weight of the obtained polymer and 200 parts by weight of a methanol solution of 1% sodium hydroxide were charged into a flask equipped with a condenser, and after being replaced with nitrogen, heated at 60 ° C. for 2 hours.
The obtained polymer was washed with distilled water, immersed in 200 parts by weight of a 2% aqueous sodium hypochlorite solution for 1 day, washed well with water and methanol, and further dried to obtain a sulfur content of 0.7% and MI of 6 g / 10 g. A low-density polyethylene having a sulfonate group at the end of the minute was obtained.

【0047】合成例8 末端にエポキシ基を有するポリプロピレンの合成:撹拌
基を有するセパラブルフラスコに別途粉砕した合成例1
の末端に二重結合を有するポリプロピレン20重量部、
1%m−クロロ過安息香酸の塩化メチレン溶液100重
量部を仕込み、室温で1日間撹拌した。反応終了後、ポ
リマーをアセトンで良く洗浄、さらに乾燥することによ
り、エポキシ基量0.025meq/Kg、MI80g
/10分の末端にエポキシ基を有するポリプロピレンを
得た。
Synthesis Example 8 Synthesis of polypropylene having an epoxy group at a terminal: Synthesis Example 1 separately pulverized into a separable flask having a stirring group
20 parts by weight of a polypropylene having a double bond at the end of
100 parts by weight of a 1% m-chloroperbenzoic acid solution in methylene chloride was charged and stirred at room temperature for 1 day. After completion of the reaction, the polymer was thoroughly washed with acetone and dried to obtain an epoxy group content of 0.025 meq / Kg and MI of 80 g.
A polypropylene having an epoxy group at a terminal of / 10 min was obtained.

【0048】実施例1 合成例2の末端にカルボン酸無水物基ポリプロピレン5
重量部とクラレ製EVAL(登録商標)−F104(エ
チレン含量32モル%、含水フェノ−ル中30℃におけ
る極限粘度0.95dl/g)45重量部を用いて、以
下の条件で溶融混練を行なった。 使用機械 :プラストグラフ ロ−タ−形状:ロ−ラ−型 回転数 :80rpm 混練温度 :220℃ 混練時間 :10分 上記の方法によって得られた樹脂組成物を、220℃で
熱プレスすることによって厚さ100ミクロンのフィル
ムにした。このフィルムを液体窒素中で破断し、破断面
を140℃のキシレンにより抽出後、走査電子顕微鏡に
より破断面を観察した。その結果、ポリプロピレンの平
均分散粒径は0.8μmで、このプレスフィルムのヘイ
ズは20%であった。このフィルム片を加圧条件下で1
10℃の熱水で30分間処理したがフィルムの形状はほ
とんど変形しなかった。
Example 1 A carboxylic anhydride-based polypropylene 5 was added to the end of Synthesis Example 2.
Using 45 parts by weight of KURARAY's EVAL (registered trademark) -F104 (ethylene content 32 mol%, intrinsic viscosity at 30 ° C. in water-containing phenol at 0.95 dl / g), melt kneading was carried out under the following conditions. Was. Machine used: Plastograph Rotor shape: Roller type Rotational speed: 80 rpm Kneading temperature: 220 ° C. Kneading time: 10 minutes The resin composition obtained by the above method is hot-pressed at 220 ° C. A 100 micron thick film was formed. This film was fractured in liquid nitrogen, and the fracture surface was extracted with xylene at 140 ° C., and the fracture surface was observed with a scanning electron microscope. As a result, the average dispersed particle size of the polypropylene was 0.8 μm, and the haze of this press film was 20%. This film piece is pressed under pressure
When treated with hot water at 10 ° C. for 30 minutes, the shape of the film was hardly deformed.

【0049】比較例1 末端にカルボン酸無水物基を有するポリプロピレン5重
量部の代わりに合成例1の末端に二重結合を有するポリ
プロピレン5重量部を用いた他は、実施例1と同様にし
てフィルムを得たところ、フィルム中の未変性ポリプロ
ピレンの平均分散粒径は5μm、フィルムのヘイズは4
0%であり、分散性、透明性共に不良であった。また1
10℃の熱水処理により一部変形した。
Comparative Example 1 The procedure of Example 1 was repeated, except that 5 parts by weight of the polypropylene having a double bond at the terminal was used instead of 5 parts by weight of the polypropylene having a carboxylic anhydride group at the terminal. When the film was obtained, the average dispersed particle size of the unmodified polypropylene in the film was 5 μm, and the haze of the film was 4 μm.
0%, and both the dispersibility and the transparency were poor. Also one
Partially deformed by hot water treatment at 10 ° C.

【0050】比較例2 クラレ製EVAL(登録商標)−F101のみを220
℃で熱プレスした後、実施例1と同様な条件で熱水処理
を行なった結果、完全に熱変形し原形をとどめない状態
になった。
Comparative Example 2 EVAL (registered trademark) -F101 manufactured by Kuraray only 220
After hot-pressing at ℃, the resultant was subjected to hot water treatment under the same conditions as in Example 1, and as a result, it was completely thermally deformed and could not remain in its original form.

【0051】実施例2 末端にカルボン酸無水物基を有するポリプロピレン5重
量部の代わりに合成例8の末端にエポキシ基を有するポ
リプロピレン5重量部を用いた他は、実施例1と同様に
してフィルムを得たところ、フィルム中の未変性ポリプ
ロピレンの平均分散粒径は1μm、フィルムのヘイズは
25%であった。
Example 2 A film was prepared in the same manner as in Example 1 except that 5 parts by weight of a polypropylene having an epoxy group at the terminal was used instead of 5 parts by weight of a polypropylene having a carboxylic anhydride group at the terminal. As a result, the average dispersed particle size of the unmodified polypropylene in the film was 1 μm, and the haze of the film was 25%.

【0052】実施例3 合成例4の末端にカルボン酸無水物基低密度ポリエチレ
ン10重量部とクラレ製EVAL(登録商標)−F10
1(エチレン含量32モル%、含水フェノ−ル中30℃
における極限粘度1.1dl/g)90重量部を用い
て、以下の条件で溶融混練を行なった。 使用機械 :ラボプラストミル(25φ) スクリュー :強混練型 回転数 :120rpm 混練温度 :220℃ 吐出量 :1Kg/h 上記の方法によって得られた樹脂組成物を、厚さ50ミ
クロンの押出しフィルムに製膜した。このフィルムを液
体窒素中で破断し、破断面を140℃のキシレンにより
抽出後、走査電子顕微鏡により破断面を観察した。その
結果、ポリプロピレンの平均分散粒径は0.5μmで、
このフィルムのヘイズは6%であった。このフィルムの
ブツは少なく、膜面の状態は良好であった。さらに上記
組成物を小型射出成形機により成形した試料片の、ノッ
チ付きIzod衝撃強度をJISK7120の方法にし
たがって測定したところ、13Kgfcm/cm↑2で
あった。
Example 3 In the synthesis example 4, 10 parts by weight of a low-density carboxylic acid anhydride group polyethylene and EVAL (registered trademark) -F10 manufactured by Kuraray were added to the terminal of Synthesis Example 4.
1 (Ethylene content 32 mol%, in water-containing phenol at 30 ° C
Was melt-kneaded under the following conditions by using 90 parts by weight of the intrinsic viscosity of 1.1 dl / g). Machine used: Labo Plastomill (25φ) Screw: Strong kneading type Rotation speed: 120 rpm Kneading temperature: 220 ° C. Discharge rate: 1 Kg / h The resin composition obtained by the above method was formed into an extruded film having a thickness of 50 μm. Filmed. This film was fractured in liquid nitrogen, and the fracture surface was extracted with xylene at 140 ° C., and the fracture surface was observed with a scanning electron microscope. As a result, the average dispersed particle size of the polypropylene was 0.5 μm,
The haze of this film was 6%. The film had few bumps, and the state of the film surface was good. Further, the notched Izod impact strength of a sample piece obtained by molding the above composition using a small injection molding machine was measured according to the method of JIS K7120, and it was 13 kgfcm / cm / 2.

【0053】比較例3 合成例4の末端にカルボン塩基を有する低密度ポリエチ
レン10重量部の代わりに、エチレン−アクリル酸−ア
クリル酸ナトリウム共重合体(アクリル酸含量0.2モ
ル%、アクリル酸ナトリウム含量0.8モル%、MI5
g/10分)を用い、その他は実施例3と同様に試験を
行ったところ、平均分散粒径は0.7μmで、この押出
しフィルムのヘイズは10%であった。このフィルムの
ブツは多く、膜面の状態は不良であった。この組成物を
小型射出成形機により成形した試料片のノッチ付きIz
od衝撃強度は10Kgfcm/cm↑2であった。
Comparative Example 3 An ethylene-acrylic acid-sodium acrylate copolymer (acrylic acid content 0.2 mol%, sodium acrylate Content 0.8 mol%, MI5
g / 10 minutes), and the other tests were conducted in the same manner as in Example 3. As a result, the average dispersed particle size was 0.7 μm, and the haze of the extruded film was 10%. The film had many bumps, and the state of the film surface was poor. Notched Iz of a sample piece obtained by molding this composition with a small injection molding machine
The od impact strength was 10 kgfcm / cm ↑ 2.

【0054】比較例4 合成例4の末端にカルボン塩基を有する低密度ポリエチ
レン10重量部の代わりに、合成例3の末端に二重結合
を有する低密度ポリエチレンを用い、その他は実施例3
と同様に試験を行ったところ、平均分散粒径は4μm
で、このフィルムのヘイズは25%であった。この組成
物を小型射出成形機により成形した試料片のノッチ付き
Izod衝撃強度は3Kgfcm/cm↑2であった。
Comparative Example 4 The low-density polyethylene having a double bond at the terminal of Synthesis Example 3 was used instead of 10 parts by weight of the low-density polyethylene having a carboxylic acid base at the terminal of Synthesis Example 4, and the other examples were the same as those of Example 3.
When the test was carried out in the same manner as described above, the average dispersed particle size was 4 μm.
The haze of this film was 25%. The notched Izod impact strength of a sample piece obtained by molding this composition using a small injection molding machine was 3 kgfcm / cm @ 2.

【0055】比較例5 クラレ製EVAL(登録商標)−F101のみを用い実
施例3と同様に射出成形した試料片のノッチ付きIzo
d衝撃強度は2.1Kgfcm/cm↑2であった。
Comparative Example 5 Notched Izo of a sample piece injection-molded in the same manner as in Example 3 using only EVAL (registered trademark) -F101 made by Kuraray.
d Impact strength was 2.1 kgfcm / cm ↑ 2.

【0056】実施例4 合成例4の末端にカルボン塩基を有する低密度ポリエチ
レン10重量部の代わりに、合成例5の末端にホスホン
酸塩基を有する低密度ポリエチレンを用い、その他は実
施例3と同様に試験を行ったところ、平均分散粒径は
0.5μmで、このフィルムのヘイズは5%であった。
このフィルムのゲルは少なく、膜面の状態は良好であっ
た。この組成物を小型射出成形機により成形した試料片
のノッチ付きIzod衝撃強度は13Kgfcm/cm
↑2であった。
Example 4 The same procedures as in Example 3 were carried out except that 10 parts by weight of the low-density polyethylene having a carboxylic acid group at the terminal of Synthesis Example 4 was replaced with a low-density polyethylene having a phosphonate group at the terminal of Synthesis Example 5. The average dispersion particle size was 0.5 μm, and the haze of this film was 5%.
The gel of this film was small and the state of the film surface was good. A notched Izod impact strength of a sample piece obtained by molding this composition using a small injection molding machine is 13 kgfcm / cm.
It was $ 2.

【0057】実施例5 合成例4の末端にカルボン塩基を有するポリオレフィン
10重量部の代わりに、合成例6のトリメトキシシリル
基を有する低密度ポリエチレンを用い、その他は実施例
3と同様に試験を行ったところ、平均分散粒径は1μm
で、このフィルムのヘイズは12%であった。このフィ
ルムのゲルは少なく、膜面の状態は良好であった。この
組成物を小型射出成形機により成形した試料片のノッチ
付きIzod衝撃強度は6Kgfcm/cm↑2であっ
た。
Example 5 A low-density polyethylene having a trimethoxysilyl group of Synthesis Example 6 was used in place of 10 parts by weight of the polyolefin having a carboxylic acid base at the terminal of Synthesis Example 4, and the other tests were conducted in the same manner as in Example 3. When performed, the average dispersed particle size was 1 μm.
The haze of this film was 12%. The gel of this film was small and the state of the film surface was good. The notched Izod impact strength of a sample piece obtained by molding this composition using a small injection molding machine was 6 kgfcm / cm @ 2.

【0058】実施例6 合成例4の末端にカルボン塩基を有する低密度ポリエチ
レン10重量部の代わりに、合成例7のスルホン酸塩基
を有する低密度ポリエチレンを用い、その他は実施例3
と同様に試験を行ったところ、平均分散粒径は0.5μ
mで、この押出しフィルムのヘイズは7%であった。こ
のフィルムのブツは少なく、膜面の状態は良好であっ
た。この組成物を小型射出成形機により成形した試料片
のノッチ付きIzod衝撃強度は12Kgfcm/cm
↑2であった。
Example 6 The low-density polyethylene having a sulfonate group of Synthesis Example 7 was used in place of 10 parts by weight of the low-density polyethylene having a carboxylic acid group at the terminal of Synthesis Example 4, and the other parts of Example 3 were used.
When a test was performed in the same manner as described above, the average dispersed particle size was 0.5 μm.
m, the haze of the extruded film was 7%. The film had few bumps, and the state of the film surface was good. A notched Izod impact strength of a sample piece obtained by molding this composition using a small injection molding machine is 12 kgfcm / cm.
It was $ 2.

【0059】[0059]

【発明の効果】本発明によれば、相溶性が良好で、ゲル
が少なく、しかも外観との良好なフィルムを与える樹脂
組成物が得られる。
According to the present invention, there can be obtained a resin composition which gives a film having good compatibility, little gel, and good appearance.

Claims (3)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】 エチレン−ビニルアルコ−ル系共重合体
(A)およびカルボキシル基、カルボン酸誘導体基、ケ
イ素含有基、エポキシ基、スルホン酸塩基およびホスホ
ン酸塩基からなる群より選ばれる官能基を末端に有する
オレフィン系重合体(B)からなる樹脂組成物。
1. An ethylene-vinyl alcohol-based copolymer (A) and a functional group selected from the group consisting of a carboxyl group, a carboxylic acid derivative group, a silicon-containing group, an epoxy group, a sulfonate group and a phosphonate group. A resin composition comprising the olefin-based polymer (B).
【請求項2】 請求項1記載の樹脂組成物からなるフィ2. A resin comprising the resin composition according to claim 1.
ルム。Lum.
【請求項3】 エチレン−ビニルアルコ−ル系共重合体3. An ethylene-vinyl alcohol copolymer
(A)と、カルボキシル基、カルボン酸誘導体基、ケイ(A), a carboxyl group, a carboxylic acid derivative group, and silicon
素含有基、エポキシ基、スルホン酸塩基およびホスホンElement-containing groups, epoxy groups, sulfonate groups and phosphones
酸塩基からなる群より選ばれる官能基を末端に有するオO-terminal having a functional group selected from the group consisting of acid bases
レフィン系重合体(B)とを溶融混練後、押出製膜するExtrusion film formation after melt-kneading the olefin polymer (B).
ことを特徴とする、(A)および(B)からなる樹脂組A resin set comprising (A) and (B)
成物からなるフィルムの製造方法。A method for producing a film made of a product.
JP18276893A 1993-07-23 1993-07-23 Resin composition Expired - Fee Related JP3329895B2 (en)