JP2829813B2 - Metallic coating composition and method for forming metallic coating film - Google Patents
Metallic coating composition and method for forming metallic coating filmInfo
- Publication number
- JP2829813B2 JP2829813B2 JP11398993A JP11398993A JP2829813B2 JP 2829813 B2 JP2829813 B2 JP 2829813B2 JP 11398993 A JP11398993 A JP 11398993A JP 11398993 A JP11398993 A JP 11398993A JP 2829813 B2 JP2829813 B2 JP 2829813B2
- Authority
- JP
- Japan
- Prior art keywords
- pigment
- weight
- parts
- coating
- titanium dioxide
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Lifetime
Description
【0001】[0001]
【産業上の利用分野】本発明は、例えば自動車、自転
車、家電製品およびその部品等を対象とする工業塗装用
として好適な光輝性を有するメタリック塗料組成物と工
業的に有利なメタリック塗膜の形成法に関する。BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a metallic coating composition having a luster suitable for industrial coating of, for example, automobiles, bicycles, home electric appliances and parts thereof, and an industrially advantageous metallic coating film. It relates to the forming method.
【0002】[0002]
【従来の技術】従来、塗膜にパール調光沢感の光輝性を
付与するための塗料成分としてマイカ顔料が汎用されて
おり、塗膜の形成は該マイカ顔料を含む塗料を着色した
カラー中塗り塗膜上に塗布し、さらにクリヤーコートを
形成する3コート系の多層塗膜形成法によっておこなわ
れていた。ところが、この塗装系はマイカ顔料特有の低
い隠蔽性と干渉性のために色ムラを生じる欠点があっ
た。2. Description of the Related Art Conventionally, mica pigments have been widely used as a coating component for imparting pearly luster to a coating film, and the formation of the coating film is a color intermediate coating obtained by coloring a coating containing the mica pigment. It has been carried out by a three-coat multi-layer coating method in which a clear coat is formed on the coating film. However, this coating system has a drawback of causing color unevenness due to low hiding power and interference characteristic of mica pigment.
【0003】このようなマイカ顔料の欠点を補う隠蔽性
能に優れた塗料として、鱗片状アルミニウム顔料と着色
顔料を組み合わせた組成のものが提案されている。例え
ば特開平2−132171号公報には、ルチル型二酸化
チタン(A)と少なくとも80重量%が1〜32μm の
粒子径を有するリン片状アルミニウム粉(B)を合計で
少なくとも80重量%含有し、且つ(A)/(B)の割
合が99/1〜90/10(重量比)の範囲からなる顔
料組成物を樹脂固形分100重量部に対して10〜20
0重量部の範囲で含有させた被覆用組成物が開示されて
いる。しかしながら、この組成ではマイカ顔料が配合さ
れていず、二酸化チタン顔料の配合量も多いため、鱗片
状アルミニウム粉のもつ光輝性を付与することができな
いうえ、アルミニウム粉末のグレー色感により色調に濁
りを与える現象を招く。[0003] As a paint excellent in concealing performance to compensate for such a disadvantage of the mica pigment, a paint having a combination of a flaky aluminum pigment and a coloring pigment has been proposed. For example, JP-A-2-132171 discloses that rutile-type titanium dioxide (A) and at least 80% by weight of at least 80% by weight of flaky aluminum powder (B) having a particle diameter of 1 to 32 μm are contained in total, The pigment composition having a ratio of (A) / (B) in the range of 99/1 to 90/10 (weight ratio) is used in an amount of 10 to 20 with respect to 100 parts by weight of the resin solid content.
A coating composition contained in a range of 0 parts by weight is disclosed. However, in this composition, the mica pigment is not blended, and the blending amount of the titanium dioxide pigment is large, so that the glitteriness of the flaky aluminum powder cannot be imparted and the color tone becomes cloudy due to the gray color of the aluminum powder. Cause a phenomenon to give.
【0004】特開平2−142862号公報には、前記
の問題点を解消する光輝性塗料として、メタリック顔料
の表面に、二重結合を有する一種以上のカルボン酸を熱
重合した少なくとも1個の二重結合と2個のカルボキシ
ル基を有するカルボン酸を介して着色顔料を化学吸着さ
せてなる一次着色メタリック顔料を含有させた組成の塗
料が開示されている。この着色顔料を担持した着色メタ
リック塗料は、優れた下地隠蔽性を発揮するが色調とし
て黒味感(アルミニウム顔料の持つグレーな色調が残る
色感)が残留する難点があり、パール調の乳白感や虹彩
感を得ることができない。[0004] Japanese Patent Application Laid-Open No. 2-142882 discloses a glittering paint which solves the above-mentioned problems. At least one carboxylic acid obtained by thermally polymerizing one or more carboxylic acids having a double bond on the surface of a metallic pigment is disclosed. A paint having a composition containing a primary colored metallic pigment obtained by chemically adsorbing a colored pigment via a carboxylic acid having a heavy bond and two carboxyl groups is disclosed. The colored metallic paint carrying this colored pigment exhibits excellent underground concealing properties, but has a drawback in that the color tone remains black (the color tone in which the gray color of an aluminum pigment remains), and it has a pearly milky feeling. Or a feeling of iris cannot be obtained.
【0005】一方、光輝感のあるメタリック塗膜の形成
方法としては、クリヤコートとしてメタリック塗料中の
アルミニウム粉末粒径と同等以上の粒径を有するカラー
アルミニウム粉末を混合したクリヤ塗料を用い、メタリ
ック塗装面にウエットオンウエットで2コート形成する
メタリック塗装法が提案されている(特開昭52−144041
号公報)。しかし、この塗装手段を用いた場合にも黒味
感が残る色調を抑制することは困難である。On the other hand, as a method of forming a metallic coating film having a brilliant feeling, a metallic paint is used as a clear coat, in which a color paint having a particle size equal to or more than that of the aluminum powder in the metallic paint is mixed. A metallic coating method has been proposed in which two coats are formed on a surface by wet-on-wet (Japanese Patent Application Laid-Open No. 52-144041).
No.). However, even when this coating means is used, it is difficult to suppress a color tone in which blackness remains.
【0006】[0006]
【発明が解決しようとする課題】本発明者らは、従来の
光輝性メタリック塗料における上記の問題点を解消する
ために顔料成分の組成を中心に鋭意研究を重ねた結果、
二酸化チタン顔料およびその他の着色顔料、顔料担持鱗
片状アルミニウム顔料およびパール顔料を特定の比率で
配合した組成の塗料は黒味感を抑制した美麗な乳白色の
ある光輝性の塗膜を現出し、またその複合塗膜は2コー
ト1ベーク塗装工程で効率よく形成できることを確認し
た。SUMMARY OF THE INVENTION The present inventors have conducted intensive studies on the composition of the pigment component in order to solve the above-mentioned problems in the conventional glittering metallic paint.
A paint having a composition in which a titanium dioxide pigment and other color pigments, a pigment-carrying flaky aluminum pigment and a pearl pigment are blended in a specific ratio, produces a beautiful milky-white glittering coating with suppressed blackness, and It was confirmed that the composite coating film could be efficiently formed in a two-coat one-bake coating process.
【0007】本発明は前記の知見に基づいて開発された
もので、その目的は、黒味感の色調を抑えた美麗なパー
ル調乳白感ならびに虹彩感を呈し、かつ下地隠蔽性能に
優れた塗膜形成が可能なメタリック塗料組成物とその工
業的な塗膜形成方法を提供することにある。The present invention has been developed on the basis of the above-mentioned findings, and its object is to provide a beautiful pearly milky whiteness and iris with a suppressed blackness color tone and a coating excellent in base layer hiding performance. An object of the present invention is to provide a metallic coating composition capable of forming a film and an industrial coating film forming method therefor.
【0008】[0008]
【課題を解決するための手段】上記の目的を達成するた
めの本発明によるメタリック塗料組成物は、(A)二酸
化チタン顔料、(B)顔料担持鱗片状アルミニウム顔
料、(C)二酸化チタン以外の着色顔料、(D)パール
顔料および(E)塗膜形成樹脂を組成成分とし、これら
成分を(A)/(B)が2/8から6/4(重量比)、
〔(A)+(B)〕/(C)が99/1〜80/20
(重量比)、〔(A)+(B)+(C)〕100重量部
に対し(D)が20〜60重量部、(E)の樹脂固形分
100重量部に対する顔料成分[(A)〜(D)]の合計量が1
0〜60重量部の各量比で含有することを構成上の特徴
とする。In order to achieve the above object, the present invention provides a metallic coating composition comprising (A) a titanium dioxide pigment, (B) a flake-like aluminum pigment carrying a pigment, and (C) a pigment other than titanium dioxide. Coloring pigment, (D) pearl pigment and (E) coating film forming resin are used as composition components, and these components are (A) / (B) in 2/8 to 6/4 (weight ratio),
[(A) + (B)] / (C) is 99/1 to 80/20
(D) is 20 to 60 parts by weight based on 100 parts by weight of ((A) + (B) + (C)), and the pigment component [(A) is based on 100 parts by weight of the resin solid content of (E). ~ (D)] is 1
It is characterized in that it is contained in each amount ratio of 0 to 60 parts by weight.
【0009】本発明を構成する顔料成分のうち、(A)
二酸化チタン顔料としては平均粒径0.2〜0.5μm
のルチル型二酸化チタン粉末が用いられる。しかし、平
均粒径が0.02〜0.05μm の範囲にある超微粒子
二酸化チタン顔料は着色力が弱いため、隠蔽性の点で本
発明の目的には適さない。Among the pigment components constituting the present invention, (A)
Average particle size 0.2-0.5μm as titanium dioxide pigment
Rutile-type titanium dioxide powder is used. However, ultrafine titanium dioxide pigment having an average particle size in the range of 0.02 to 0.05 μm has a weak coloring power and is not suitable for the purpose of the present invention in terms of hiding properties.
【0010】(B)成分の顔料担持鱗片状アルミニウム
顔料は、鱗片状アルミニウム顔料の表面に有機系または
無機系の着色顔料を化学的に吸着させたメタリック顔料
で、粒径が1〜50μm 、好ましくは5〜44μm の範
囲の粉末として使用される。担持される着色顔料は従来
から塗料用に常用されているもので、例えば有機系とし
てはアゾレーキ系顔料、不溶性アゾ系顔料、縮合アゾ系
顔料、フタロシアニン系顔料、インジゴ系顔料、ペリノ
ン系顔料、ペリレン系顔料、フタロン系顔料、ジオキサ
ジン系顔料、キナクリドン系顔料、イソインドリノン系
顔料、金属錯体顔料等を挙げることができ、無機系とし
ては黄鉛、黄色酸化鉄、ベンガラ、カーボンブラック、
二酸化チタン等が挙げられる。The pigment-bearing flaky aluminum pigment of the component (B) is a metallic pigment obtained by chemically adsorbing an organic or inorganic coloring pigment on the surface of the flaky aluminum pigment, and has a particle diameter of 1 to 50 μm, preferably Is used as a powder in the range of 5-44 .mu.m. The color pigments to be carried are those conventionally used for paints, for example, as organic type, azo lake type pigment, insoluble azo type pigment, condensed azo type pigment, phthalocyanine type pigment, indigo type pigment, perinone type pigment, perylene Pigments, phthalone pigments, dioxazine pigments, quinacridone pigments, isoindolinone pigments, metal complex pigments, and the like.Inorganic pigments such as graphite, yellow iron oxide, red iron oxide, carbon black,
Titanium dioxide and the like can be mentioned.
【0011】上記の顔料担持鱗片状アルミニウム顔料
(B)は、二重結合を有する1種以上のカルボン酸を熱
重合した1個以上の二重結合と2個のカルボキシル基を
有するカルボン酸とフレーク状のアルミニウム顔料を有
機溶媒中で撹拌し、冷却後に濾過して得た熱重合カルボ
ン酸処理アルミニウム顔料と着色顔料とを分散粉砕した
のち有機溶媒を除去する工程によって製造することがで
き、さらに必要に応じてラジカル重合性不飽和カルボン
酸およびラジカル重合性二重結合を3個以上有するモノ
マーからなるポリマーによって被覆させることもでき
る。これら顔料は、商品名“フレンドカラーF500G
R,F500BL,F500RG,F701BG”〔昭
和アルミパウダー(株)製〕等としても市販されてい
る。The above-mentioned pigment-bearing flaky aluminum pigment (B) is obtained by thermally polymerizing one or more carboxylic acids having a double bond, a carboxylic acid having at least one double bond and two carboxyl groups, and a flake. A heat-polymerized carboxylic acid-treated aluminum pigment obtained by stirring an aluminum pigment in a form of an organic solvent, cooling and filtering, and then dispersing and pulverizing the pigment and then removing the organic solvent can be produced. According to the above, it can be coated with a polymer comprising a monomer having three or more radically polymerizable unsaturated carboxylic acids and radically polymerizable double bonds. These pigments are available under the trade name “Friend Color F500G”
R, F500BL, F500RG, F701BG "(manufactured by Showa Aluminum Powder Co., Ltd.) and the like.
【0012】二酸化チタン以外の着色顔料(C)には、
塗料用として用いられる各種の有機系、無機系のものが
使用でき、種類や成分に制約はない。したがって、担持
用着色顔料として例示した上記の着色顔料のうち二酸化
チタンを除いたものが使用し得る。The coloring pigments (C) other than titanium dioxide include:
Various organic and inorganic materials used for paints can be used, and there are no restrictions on the types and components. Therefore, among the above-mentioned coloring pigments exemplified as the supporting coloring pigment, those excluding titanium dioxide can be used.
【0013】パール顔料(D)は、マイカの表面に二酸
化チタンを被覆した性状の顔料成分で、粒径が1〜44
μm の範囲にある粉末が使用される。とくに粒径が10
〜40μm で、薄層の二酸化チタンでコーティングされ
たホワイトマイカまたは同コーティング層が比較的厚い
干渉マイカが好適に用いられる。このほか、耐水性を高
めるために他の金属酸化物等で被覆処理したものであっ
ても使用することができる。The pearl pigment (D) is a pigment component having a mica surface coated with titanium dioxide and having a particle diameter of 1 to 44.
Powders in the μm range are used. Especially when the particle size is 10
White mica having a thickness of 4040 μm and coated with a thin layer of titanium dioxide or interference mica having a relatively thick coating layer is preferably used. In addition, those coated with another metal oxide or the like in order to enhance water resistance can also be used.
【0014】塗膜形成用のビヒクルとなる(E)成分の
樹脂としては、アクリル樹脂、ポリエステル樹脂、アル
キッド樹脂、弗素樹脂などが適用され、通常、アミノ樹
脂やブロックイソシアネートなどの架橋剤と混合して使
用に供される。また、これら樹脂は1種に限らず2種以
上を組み合わせて使用することもできる。このほか、常
温乾燥により硬化することができる2液型ポリウレタン
樹脂やシリコーン樹脂なども用いられる。Acrylic resin, polyester resin, alkyd resin, fluorine resin and the like are applied as the resin of the component (E) to be a vehicle for forming a coating film, and are usually mixed with a crosslinking agent such as an amino resin or a blocked isocyanate. Provided for use. Further, these resins are not limited to one kind, and two or more kinds can be used in combination. In addition, a two-component polyurethane resin or silicone resin that can be cured by drying at room temperature is also used.
【0015】上記(A)〜(E)の組成成分と併せ、こ
れらの成分を重量比で(A)/(B)を2/8〜6/
4、〔(A)+(B)〕/(C)を99/1〜80/2
0の割合とし、〔(A)+(B)+(C)〕100重量
部当たり(D)を20〜60重量部、(E)の樹脂固形
分100重量部に対する顔料成分[(A)〜(D)]の合計量が
10〜60重量部の量比で含有させることは発明構成上
の重要な要件であり、この量比範囲を外れると形成塗膜
に目的とする黒味感を抑えた美麗なパール調乳白感と虹
彩感を呈する光輝性を発現し、かつ隠蔽性に優れた塗膜
を形成することができなくなる。In combination with the above-mentioned components (A) to (E), these components are converted by weight ratio of (A) / (B) to 2/8 to 6 /
4, [(A) + (B)] / (C) is 99/1 to 80/2
The ratio of (D) is 20 to 60 parts by weight per 100 parts by weight of [(A) + (B) + (C)], and the pigment component [(A) to 100 parts by weight of the resin solid content of (E)]. (D)] is an important requirement in the constitution of the invention to be contained in an amount ratio of 10 to 60 parts by weight, and when the amount ratio is out of this range, the desired blackness of the formed coating film is suppressed. It is impossible to form a coating film exhibiting a brilliant pearly milky white feeling and an iris feeling and exhibiting excellent hiding properties.
【0016】すなわち、(A)に対する(B)の割合が
2/8(80重量%)を越えるとメタリック感が強調さ
れ過ぎてパール調の乳白感が消失し、また(B)の比率
が6/4(40重量%)を下廻ると二酸化チタンの白濁
感が強くなって、虹彩感や光輝感が消失する。〔(A)
+(B)〕に対する(C)の割合が99/1(1重量
%)未満では淡い彩色しかできない関係で色調の選択が
限定され、逆に80/20(20重量%)を越えると濃
彩色になり過ぎてパール調乳白色に乏しい色調となる。
〔(A)+(B)+(C)〕成分の100重量部に対し
て(D)のパール顔料が20重量部未満の配合比率であ
ると虹彩感が減退し、60重量部を上廻ると下地隠蔽性
能が低下して多層塗布工程を採る必要が生じる。また、
(E)の樹脂固形分に対して〔(A)+(B)+(C)
+(D)〕の全顔料成分の配合量が10重量部未満では
隠蔽力が不足し、60重量部を越えると臨界PWCに近
づいて塗膜の平滑性が損なわれ、外観不良を招く。That is, when the ratio of (B) to (A) exceeds 2/8 (80% by weight), the metallic feeling is overemphasized and the pearly milky feeling disappears, and the ratio of (B) is 6%. If the ratio is less than / 4 (40% by weight), the opacity of titanium dioxide becomes strong, and the iris and glitter are lost. [(A)
When the ratio of (C) to + (B)] is less than 99/1 (1% by weight), only a light color can be obtained, so that selection of color tone is limited, and when it exceeds 80/20 (20% by weight), dark color It becomes too pearly milky white color.
If the proportion of the pearl pigment of (D) is less than 20 parts by weight with respect to 100 parts by weight of the ((A) + (B) + (C)) component, the iris is reduced and exceeds 60 parts by weight. Then, the underlying layer concealing performance is lowered, and it is necessary to adopt a multilayer coating process. Also,
[(A) + (B) + (C)]
+ (D)] if the blending amount of all the pigment components is less than 10 parts by weight, the hiding power is insufficient, and if it exceeds 60 parts by weight, it approaches the critical PWC and the smoothness of the coating film is impaired, leading to poor appearance.
【0017】より好ましい成分配合比は、(A)/
(B)が2/8〜4/6(重量比)、〔(A)+
(B)〕/(C)が95/5〜85/15(重量比)、
〔(A)+(B)+(C)〕100重量部当たり(D)
40〜50重量部、(E)の樹脂固形分100重量部当
たり顔料成分[(A)〜(D)]の合計量が15〜40重量部の
範囲にある。A more preferable compounding ratio is (A) /
(B) is 2/8 to 4/6 (weight ratio), [(A) +
(B)] / (C) is 95/5 to 85/15 (weight ratio),
[(A) + (B) + (C)] per 100 parts by weight (D)
The total amount of the pigment components [(A) to (D)] is in the range of 15 to 40 parts by weight per 40 to 50 parts by weight and 100 parts by weight of the resin solid content of (E).
【0018】本発明のメタリック塗料組成物は上記の各
成分を主体に構成されるが、従来の塗料組成物に常用さ
れている各種の添加剤を任意に配合することができる。
添加剤としては、例えばドデシルベンゼンスルホン酸等
の硬化触媒、ベンゾトリアゾール系の紫外線吸収剤、ベ
ンゾフェノール系の酸化防止剤、シリコーンや有機高分
子等の表面調整剤、タレ止め剤、増粘剤などが適宜に使
用される。これらの成分は、通常、塗膜形成用樹脂10
0重量部に対し5重量部以下の配合量で塗料や塗膜の性
能を改善することができる。Although the metallic coating composition of the present invention is mainly composed of the above-mentioned components, various additives commonly used in conventional coating compositions can be arbitrarily compounded.
Examples of the additive include a curing catalyst such as dodecylbenzenesulfonic acid, a benzotriazole-based ultraviolet absorber, a benzophenol-based antioxidant, a surface conditioner such as silicone and an organic polymer, a sagging agent, and a thickener. Is used as appropriate. These components are usually contained in the film-forming resin 10.
The performance of paints and coatings can be improved with a blending amount of 5 parts by weight or less with respect to 0 parts by weight.
【0019】上記の成分組成からなる本発明のメタリッ
ク塗料系は、有機溶媒型が一般的であるが、これに限ら
れるものではなく非水分散液型、水溶液型、分散液型な
ど各種の形態として塗料構成することができる。塗装に
際しては、有機溶剤、水等の溶媒で塗装適性粘度に希釈
して用いるが、塗装時の固形分は10〜50重量%が好
ましい。The metallic coating system of the present invention having the above-mentioned component composition is generally of the organic solvent type, but is not limited thereto, and may be of various types such as non-aqueous dispersion type, aqueous solution type and dispersion type. Can be composed as a paint. At the time of coating, the mixture is diluted with a solvent such as an organic solvent or water to a viscosity suitable for coating, and the solid content at the time of coating is preferably 10 to 50% by weight.
【0020】本発明によるメタリック塗膜の形成法は、
(A)二酸化チタン顔料、(B)顔料担持鱗片状アルミ
ニウム顔料、(C)二酸化チタン以外の着色顔料、
(D)パール顔料、(E)塗膜形成樹脂を組成成分と
し、これら成分を(A)/(B)が2/8〜6/4(重
量比)、〔(A)+(B)〕/(C)が99/1〜80
/20(重量比)、〔(A)+(B)+(C)〕100
重量部に対し(D)が20〜60重量部、(E)の樹脂
固形分100重量部に対する顔料成分[(A)〜(D)]の合計
量が10〜60重量部の各量比で含有する上記のメタリ
ック塗料を被塗基材面にベースコートしたのち、クリヤ
ー塗料をトップコートし、ベースコートおよびトップコ
ートを同時に硬化させるプロセスからなる。The method for forming a metallic coating film according to the present invention comprises:
(A) titanium dioxide pigment, (B) pigment-bearing flaky aluminum pigment, (C) coloring pigment other than titanium dioxide,
(D) Pearl pigment and (E) a film-forming resin are used as composition components, and these components are (A) / (B) in a ratio of 2/8 to 6/4 (weight ratio), [(A) + (B)]. / (C) is 99/1 to 80
/ 20 (weight ratio), [(A) + (B) + (C)] 100
(D) is 20 to 60 parts by weight with respect to 100 parts by weight of the resin solid content of (E), and the total amount of the pigment components [(A) to (D)] is 10 to 60 parts by weight. After a base coat is applied to the surface of the base material to be coated, the clear paint is top-coated, and the base coat and the top coat are simultaneously cured.
【0021】塗布対象となる被塗基材は、鉄、アルミニ
ウム、銅もしくはこれらの合金を含む金属類を始めとし
て、ガラス、セメント、コンクリートなどの無機材料、
ポリエチレン、ポリプロピレン、エチレン−酢酸ビニル
共重合体、ポリアミド、ポリアクリル、ポリエステル、
エチレン−ポリビニルアルコール共重合体、塩化ビニル
樹脂、塩化ビニリデン樹脂、ポリカーボネート、ポリウ
レタン等の樹脂成形品および各種FRPなどのプラスチ
ック材料、木材、繊維材料が該当する。なお、これら被
塗基材に予め適宜なアンダーコートやプレコート処理を
施すことは任意である。The substrate to be coated includes inorganic materials such as metals such as iron, aluminum, copper and their alloys, glass, cement, concrete, and the like.
Polyethylene, polypropylene, ethylene-vinyl acetate copolymer, polyamide, polyacryl, polyester,
Resin molded products such as ethylene-polyvinyl alcohol copolymer, vinyl chloride resin, vinylidene chloride resin, polycarbonate, and polyurethane, and plastic materials such as various FRPs, wood, and fiber materials are applicable. It is optional to apply an appropriate undercoat or precoat treatment to these substrates in advance.
【0022】塗装は被塗基材に直接おこなうこともでき
るが、例えば自動車の塗装等においては、通常、表面化
成処理後に電着塗料などによる下塗りおよび中塗り塗装
し、塗膜が硬化した後に塗装する。塗装操作は霧化式塗
装機を用い、エアスプレー塗装、静電塗装などによって
おこなわれる。ベースコートの塗膜は、10〜25μm
の乾燥膜厚範囲で形成することが好ましい。10μm 未
満の膜厚では下地隠蔽性が減退して色ムラを生ずる原因
となる。The coating can be carried out directly on the substrate to be coated. For example, in the case of coating an automobile, for example, undercoating and intermediate coating with an electrodeposition paint or the like after a surface chemical conversion treatment, and coating after the coating film is cured I do. The coating operation is performed by air spray coating, electrostatic coating or the like using an atomizing type coating machine. Base coat film is 10-25 μm
It is preferable to form the film in the range of the dry film thickness. If the film thickness is less than 10 μm, the base concealing property is reduced, causing color unevenness.
【0023】ついで、ベースコート上に上塗りのクリヤ
ー塗料をトップコートとして塗装する。クリヤー塗料と
しては一般に常用される透明性樹脂が使用されるが、必
要に応じ透明性を損ねない範囲で着色顔料や各種添加成
分を配合してもよい。ベースコートとトップコートは2
コート1ベーク方式により同時に硬化させて複合塗膜を
形成する。形成するトップコートの好ましい乾燥膜厚
は、30〜60μm である。Next, a clear top coating is applied as a top coat on the base coat. As the clear paint, a transparent resin generally used is generally used, but if necessary, a coloring pigment or various additive components may be blended as long as the transparency is not impaired. Base coat and top coat are 2
The coating is simultaneously cured by a coat 1 baking method to form a composite coating film. The preferred dry film thickness of the formed top coat is 30 to 60 μm.
【0024】[0024]
【作用】本発明のメタリック塗料組成物によれば、特定
比率で配合された(A)〜(D)の顔料成分が形成塗膜
に独特の光輝性を与える作用を営む。すなわち、顔料担
持鱗片状アルミニウム顔料(B)の表面に介在する着色
顔料はアルミニウム顔料固有のフリップフロップによる
濁り色感を和らげ、優れた色調の光輝性を現出すると共
に下地に対する十分な隠蔽性能を発揮する。同時に二酸
化チタン顔料(A)は高い隠蔽力を付与しつつパール顔
料と併用することによりパール調の乳白感を創出し、パ
ール顔料(D)は顔料担持鱗片状アルミニウム顔料
(B)では発現できない虹彩感を現出するために機能す
る。このような各成分の機能が総合して、黒味感を抑え
ながら二酸化チタン顔料以外の着色顔料(C)の色相に
沿う独特のパール調乳白感と虹彩感を呈する極めて美麗
な光輝性のメタリック系塗膜を形成する。更に、この成
分組成において顔料担持鱗片状アルミニウム顔料の着色
顔料を変えることにより多様の色感を創出することがで
きるから、色調の選択巾が著しく拡大する効果も得られ
る。According to the metallic coating composition of the present invention, the pigment components (A) to (D) blended in a specific ratio have an effect of giving the formed coating film a unique glitter. In other words, the coloring pigment interposed on the surface of the pigment-carrying flake-like aluminum pigment (B) reduces the turbid color due to the flip-flop inherent to the aluminum pigment, exhibits excellent brilliant color tone, and has sufficient concealment performance against the base. Demonstrate. At the same time, the titanium dioxide pigment (A) creates a pearly milky feeling by being used in combination with the pearl pigment while imparting a high hiding power, and the pearl pigment (D) is an iris that cannot be exhibited by the pigment-carrying flaky aluminum pigment (B). It works to create a feeling. The function of each of these components is combined to give a unique pearly milky whiteness and iris along the hue of the coloring pigment (C) other than the titanium dioxide pigment while suppressing the blackness, and an extremely beautiful brilliant metallic. A system coating is formed. Further, by changing the color pigment of the pigment-supporting flaky aluminum pigment in this component composition, various color sensations can be created, so that the effect of remarkably expanding the color tone selection range can be obtained.
【0025】また、本発明に係るメタリック塗膜の形成
法によれば、上記したメタリック塗料の成分組成による
光輝性と下地隠蔽性能の機能に基づき、ベースコートと
トップコートの2コート1ベーク塗装により常に色ムラ
のない正常な光輝性のメタリック塗膜を形成することが
できるから、塗装工程の簡素化が可能となる。Further, according to the method for forming a metallic coating film according to the present invention, the base coat and the top coat are always subjected to two-coat one-bake coating on the basis of the functions of the brilliancy and the base concealing performance by the component composition of the metallic paint described above. Since a normal glittering metallic coating film without color unevenness can be formed, the coating process can be simplified.
【0026】[0026]
【実施例】以下、本発明の実施例を比較例と対比して説
明する。適用したメタリック塗料組成物を構成する
(A)〜(E)の具体的成分は下記のとおりである。な
お、表1〜3の成分表示は下記の記号で示した。また、
配合量は固形分の重量部で示し、(A)、(B)、
(C)および(D)の配合量は各顔料成分のみの重量部
として表示した。Hereinafter, examples of the present invention will be described in comparison with comparative examples. The specific components (A) to (E) constituting the applied metallic coating composition are as follows. The components shown in Tables 1 to 3 are indicated by the following symbols. Also,
The amount is shown in parts by weight of the solid content, and (A), (B),
The amounts of (C) and (D) were expressed as parts by weight of each pigment component alone.
【0027】(A)二酸化チタン顔料;次のように調製
した二酸化チタンペーストを用いた。 (A-1)商品名“タイペークCR−95”〔石原産業
(株)製〕40.0重量部とアクリル樹脂ワニス37.
3重量部をディゾルバーで予備混合し、サンドグライン
ドミルで粒度10μm 以下になるまで分散した。つい
で、メラミン樹脂ワニス7.8重量部、トリエチルアミ
ン0.3重量部および溶媒(F−1)14.6重量部を
加えてディゾルバーで20分間混合した。 (A-2)商品名“タイペークCR−95”〔石原産業
(株)製〕40.0重量部、ポリエステル樹脂(E−
3)ワニス37.3重量部、メラミン樹脂(E−4)ワ
ニス16.0重量部、トリエチルアミン0.3重量部お
よび溶媒(F−2)6.4重量部を用い、(A-1) と同様
に分散混合した。(A) Titanium dioxide pigment: A titanium dioxide paste prepared as follows was used. (A-1) 40.0 parts by weight of trade name “Taipaek CR-95” (manufactured by Ishihara Sangyo Co., Ltd.) and acrylic resin varnish
3 parts by weight were premixed with a dissolver and dispersed by a sand grind mill until the particle size became 10 μm or less. Then, 7.8 parts by weight of the melamine resin varnish, 0.3 parts by weight of triethylamine and 14.6 parts by weight of the solvent (F-1) were added and mixed with a dissolver for 20 minutes. (A-2) 40.0 parts by weight of trade name "Taipaek CR-95" (manufactured by Ishihara Sangyo Co., Ltd.), polyester resin (E-
3) Using 37.3 parts by weight of varnish, 16.0 parts by weight of melamine resin (E-4) varnish, 0.3 parts by weight of triethylamine and 6.4 parts by weight of solvent (F-2), (A-1) Similarly, they were dispersed and mixed.
【0028】(B)顔料担持鱗片状アルミニウム顔料; (B-1)商品名“フレンドカラーF500GR”〔昭和ア
ルミパウダー(株)製、固形分48%〕 (B-2)商品名“フレンドカラーF500BL”〔昭和ア
ルミパウダー(株)製、固形分48%〕 (B-3)商品名“フレンドカラーF500RG”〔昭和ア
ルミパウダー(株)製、固形分51%〕 (B-4)商品名“アルペースト7160N”〔東洋アルミ
ニウム(株)製、固形分65%〕。比較例用として用い
た顔料を担持していないアルミニウム顔料(B) Pigment-supporting flaky aluminum pigment; (B-1) Trade name "Friend Color F500GR" [manufactured by Showa Aluminum Powder Co., Ltd., solid content 48%] (B-2) Trade name "Friend Color F500BL" (Showa Aluminum Powder Co., Ltd., solid content 48%) (B-3) Trade name "Friend Color F500RG" [Showa Aluminum Powder Co., Ltd., solid content 51%] (B-4) Trade name "AL Paste 7160N "[Toyo Aluminum Co., Ltd., solid content 65%]. Aluminum pigment not carrying pigment used for comparative example
【0029】(C)着色顔料;次のように調製した原色
ペーストを用いた。 (C-1)商品名“パリオトールエロー2140HD”〔B
ASF社製〕7.8重量部とアクリル樹脂(E−1)ワ
ニス46.7重量部、メラミン樹脂(E−2)ワニス
9.7重量部、トリエチルアミン0.4重量部、溶媒
(F−1)34.4重量部を用い、(A-1) と同様に分散
混合した。 (C-2)商品名“シンカシャマゼンダRT−343D”
〔CIBAGEIGY社製〕13.4重量部、アクリル
樹脂(E−1)ワニス40.2重量部、メラミン樹脂
(E−2)ワニス8.4重量部、トリエチルアミン0.
4重量部および溶媒(F−1)37.6重量部を用い、
(A-1) と同様に分散混合した。 (C-3)商品名“シャニンブルーG−500N”〔山陽色
素(株)製〕9.0重量部、アクリル樹脂(E−1)ワ
ニス65.6重量部、メラミン樹脂(E−2)ワニス1
3.6重量部、トリエチルアミン0.5重量部および溶
媒(F−1)11.3重量部を用い、(A-1) と同様に分
散混合した。 (C-4)商品名“シャニンブルーG−500N”〔山陽色
素(株)製〕8.0重量部、ポリエステル樹脂(E−
3)ワニス57.5重量部、メラミン樹脂(E−4)ワ
ニス19.2重量部、トリエチルアミン0.5重量部お
よび溶媒(F−2)14.8重量部を用い、(A-1) と同
様に分散混合した。(C) Color pigment: A primary color paste prepared as follows was used. (C-1) Trade name "Palio Thor Yellow 2140HD" [B
ASF] 7.8 parts by weight, acrylic resin (E-1) varnish 46.7 parts by weight, melamine resin (E-2) varnish 9.7 parts by weight, triethylamine 0.4 parts by weight, solvent (F-1) Using 34.4 parts by weight, the mixture was dispersed and mixed in the same manner as in (A-1). (C-2) Product name “Shinkasha Magenta RT-343D”
[CIBAGEIGY] 13.4 parts by weight, acrylic resin (E-1) varnish 40.2 parts by weight, melamine resin (E-2) varnish 8.4 parts by weight, triethylamine 0.
Using 4 parts by weight and 37.6 parts by weight of the solvent (F-1),
It was dispersed and mixed in the same manner as (A-1). (C-3) Trade name "Shanin Blue G-500N" (manufactured by Sanyo Dyeing Co., Ltd.) 9.0 parts by weight, acrylic resin (E-1) varnish 65.6 parts by weight, melamine resin (E-2) varnish 1
3.6 parts by weight, 0.5 parts by weight of triethylamine and 11.3 parts by weight of the solvent (F-1) were dispersed and mixed in the same manner as in (A-1). (C-4) Trade name “Shanin Blue G-500N” [manufactured by Sanyo Dyeing Co., Ltd.] 8.0 parts by weight, polyester resin (E-
3) Using 57.5 parts by weight of varnish, 19.2 parts by weight of melamine resin (E-4) varnish, 0.5 parts by weight of triethylamine and 14.8 parts by weight of solvent (F-2), (A-1) Similarly, they were dispersed and mixed.
【0030】(D)パール顔料; (D-1)商品名“イリオジン103WII”〔メルク社製〕 (D-2)商品名“エクステリアマーリンラセット”〔マー
ル社製〕 (D-3)商品名“エクステリアマーリンスーパーブルー
〔マール社製〕(D) Pearl pigment; (D-1) Trade name “Iriodin 103WII” (manufactured by Merck) (D-2) Trade name “Exterior Marlin Russet” (manufactured by Marl) (D-3) Trade name “ Exterior Marlin Super Blue (Mal)
【0031】(E)塗膜形成樹脂; (E-1)アクリル樹脂(スチレン/メチルメタアクリレー
ト/エチルアクリレート・ヒドロキシエチルメタアクリ
レート/メタアクリル酸の共重合体, 数平均分子量2000
0,水酸基価45, 酸価15,固形分50% ) (E-2)メラミン樹脂〔商品名“ユーバン20SE”三井
東圧化学(株)製、固形分60%〕 (E-3)ポリエステル樹脂〔商品名“ベッコゾール EZ
3520−60”大日本インキ化学工業(株)製、固形
分60%〕 (E-4)メラミン樹脂〔商品名“スーパーベッカミンL−
117−60”大日本インキ化学工業(株)製、固形分
60%〕(E) Coating resin; (E-1) Acrylic resin (styrene / methyl methacrylate / ethyl acrylate / hydroxyethyl methacrylate / methacrylic acid copolymer, number average molecular weight 2000)
0, hydroxyl value 45, acid value 15, solid content 50%) (E-2) Melamine resin [trade name "Uban 20SE" manufactured by Mitsui Toatsu Chemicals, Inc., solid content 60%] (E-3) Polyester resin [Product name "Beccosol EZ
3520-60 "manufactured by Dainippon Ink and Chemicals, Inc., solid content 60%] (E-4) Melamine resin [trade name" Super Beckamine L- "
117-60 "manufactured by Dainippon Ink and Chemicals, Inc., solid content 60%]
【0032】実施例1〜10、比較例1〜11 上記(A)〜(E)の成分を表1〜3に示す組成比率で
有機溶媒F−1(トルエン/キシレン/酢酸エチル/酢
酸ブチル=70/15/10/5) または有機溶媒F−2(ソルベ
ッソ150/キシレン/酢酸ブチル=60/30/10;ソルベ
ッソ150はエクソン社製の芳香族炭化水素系溶剤)と
15分間ディスパーにより塗装適性粘度になるように撹
拌混合してメタリック塗料を作製した。Examples 1 to 10 and Comparative Examples 1 to 11 The components (A) to (E) were mixed with the organic solvent F-1 (toluene / xylene / ethyl acetate / butyl acetate) at the composition ratios shown in Tables 1 to 3. 70/15/10/5) Or organic solvent F-2 (Solvesso 150 / xylene / butyl acetate = 60/30/10; Solvesso 150 is an aromatic hydrocarbon solvent manufactured by Exxon) and dispersing for 15 minutes to suitability for coating A metallic coating was prepared by stirring and mixing to obtain a viscosity.
【0033】得られた各組成のメタリック塗料を用い、
以下の塗装工程により塗膜を形成した。リン酸亜鉛で化
成処理した厚さ0.8mmのダル鋼板基材に、カチオン電
着塗料〔日本ペイント(株)製、“パワートップU−5
0”〕を乾燥塗膜が25μm になるように塗装したの
ち、160℃で30分間焼付けた。この電着塗膜面に中
塗塗料〔日本ペイント(株)製、“オルガS−90シー
ラー”〕を乾燥塗膜が40μm になるようにエアスプレ
ー塗装し、140℃で30分間焼付けして試験板を作製
した。この試験板の表面にメタリック塗料を乾燥塗膜が
16〜20μm になるように塗装した。塗装は静電塗装
機〔ランズバーグゲマ社製、Auto REA〕を用い
霧化圧2.8kg/cm2でおこない、塗装中のブースの雰囲
気は温度25℃、湿度75%に保持した。塗装後3分間
セッティングを施したのち、アクリル樹脂系クリヤー塗
料〔日本ペイント(株)製、“スーパーラック0−10
0”〕を乾燥膜厚が約35μm になるよう塗装した。つ
いで、約10分間室温でセッティングしたのち、140
℃で30分間焼付けた。Using the obtained metallic paint of each composition,
A coating film was formed by the following coating process. A cationic electrodeposition coating [Nippon Paint Co., Ltd., "Power Top U-5"
0 "] was applied so that the dry coating film became 25 μm, and baked at 160 ° C. for 30 minutes. An intermediate coating material (“ Olga S-90 Sealer ”manufactured by Nippon Paint Co., Ltd.) was applied to the surface of the electrodeposited coating film. Was air-sprayed so that the dry film thickness was 40 μm, and baked at 140 ° C. for 30 minutes to produce a test plate, and a metallic paint was applied on the surface of the test plate so that the dry film thickness was 16 to 20 μm. Coating was performed using an electrostatic coating machine (Auto REA, manufactured by Landsberg Gemma Co., Ltd.) at an atomization pressure of 2.8 kg / cm 2 , and the atmosphere in the booth during coating was maintained at a temperature of 25 ° C. and a humidity of 75%. After setting for 3 minutes after painting, clear acrylic resin [Nippon Paint Co., Ltd., "Super Rack 0-10"
0 ″] was applied to a dry film thickness of about 35 μm. After setting at room temperature for about 10 minutes,
Bake at 300C for 30 minutes.
【0034】形成した塗膜につき、下記の基準でパール
調の乳白感と虹彩感、および隠蔽性を目視観察により判
定評価し、同時に隠蔽膜厚を測定した。 (1) 乳白感; ○ … 乳白感あり △ … 黒味がかった乳白感 × … 乳白感なし (2) 虹彩感; ○ … 鮮明な虹彩感 △ … 虹彩感弱く、メタリック感が強い × … 虹彩感なし (3) 隠蔽性; ○ … 下地の透けなし × … 下地の透けあり (4) 隠蔽膜厚;JIS K5400 7.2に定められ
た隠蔽率試験紙の上に塗装し、白黒地の境界判別ができ
なくなった時の膜厚を測定した。With respect to the formed coating film, pearly milky feeling, iris feeling and concealing property were judged and evaluated by visual observation according to the following criteria, and the concealing film thickness was measured at the same time. (1) Milky feeling; ○… Milky feeling △… Blackish milky feeling ×… No milky feeling (2) Iris feeling; ○… Clear iris feeling △… Weak iris feeling, strong metallic feeling ×… Iris feeling None (3) Opacity; ○… No undercoat is transparent ×… Undercoat is transparent (4) Concealed film thickness: Painted on opacity test paper specified in 7.2 of JIS K5400 7.2, and discrimination of boundary between black and white ground The film thickness at which no film could be formed was measured.
【0035】得られた評価結果を、用いたメタリック塗
料の成分組成と対比して表1〜3に示した。The obtained evaluation results are shown in Tables 1 to 3 in comparison with the component compositions of the used metallic paints.
【0036】[0036]
【表1】 [Table 1]
【0037】[0037]
【表2】 [Table 2]
【0038】[0038]
【表3】 [Table 3]
【0039】表1〜3を考察して明らかなように、本発
明の成分組成を有するメタリック塗料を用いて2コート
1ベーク塗装により形成した各塗膜は、黒味感のないパ
ール調の乳白感と虹彩感を呈する優れた光輝性を有して
おり、下地隠蔽力も十分であった。これに対し、本発明
のいずれかの特定要件を外れる比較例の形成塗膜は、乳
白感、虹彩感または隠蔽性の全てを満足させることはで
きなかった。なお、比較例11では全顔料成分の量が多過
ぎるため、光輝性の評価は良好であったが、塗膜の平滑
性が著しく低下することが認められた。As is apparent from a consideration of Tables 1 to 3, each coating film formed by two coats and one bake coating using the metallic paint having the component composition of the present invention has a pearly milky white having no blackish feeling. It had excellent glittering properties, giving a sense of sensation and iris, and had a sufficient background hiding power. On the other hand, the formed coating film of the comparative example which did not satisfy any of the specific requirements of the present invention could not satisfy all of the opalescent feeling, the iris feeling or the hiding property. In Comparative Example 11, the evaluation of the glitter was good because the amount of all the pigment components was too large, but it was recognized that the smoothness of the coating film was significantly reduced.
【0040】[0040]
【発明の効果】以上のとおり、本発明によれば(A)二
酸化チタン顔料、(B)顔料担持鱗片状アルミニウム顔
料、(C)二酸化チタン以外の着色顔料および(D)パ
ール顔料からなる4種類の顔料成分を特定された量比で
(E)塗膜形成樹脂に含有させることにより、従来技術
によっては得られなかった独特の美麗なパール調乳白感
と虹彩感を呈する光輝性塗膜が形成し得るメタリック塗
料組成物を提供することができる。また、本発明による
メタリック塗膜の形成法に従えば、上記成分組成の塗料
を用いて2コート1ベーク塗装系による効率的な工程で
塗装操作をおこなうことが可能となる。したがって、高
級塗色が要求される自動車車体の外面塗装をはじめ、各
種の被塗基材に高品質の光輝性塗膜を形成する目的に極
めて有用である。As described above, according to the present invention, four types of (A) titanium dioxide pigment, (B) flake aluminum pigment carrying pigment, (C) coloring pigment other than titanium dioxide, and (D) pearl pigment. (E) By adding the pigment component of (A) to the film-forming resin in a specified quantitative ratio, a glittering coating film exhibiting a unique beautiful pearl milky whiteness and iris feeling which could not be obtained by the prior art is formed. A metallic coating composition that can be used. Further, according to the method for forming a metallic coating film according to the present invention, it is possible to perform a coating operation in an efficient process using a two-coat, one-bake coating system using a coating material having the above-described composition. Therefore, it is extremely useful for the purpose of forming a high-quality brilliant coating film on various substrates to be coated, including the exterior coating of an automobile body requiring a high-grade coating color.
Claims (2)
持鱗片状アルミニウム顔料、(C)二酸化チタン以外の
着色顔料、(D)パール顔料、および(E)塗膜形成樹
脂を組成成分とし、これら成分を(A)/(B)が2/
8〜6/4(重量比)、〔(A)+(B)〕/(C)が
99/1〜80/20(重量比)、〔(A)+(B)+
(C)〕100重量部に対し(D)が20〜60重量
部、(E)の樹脂固形分100重量部に対する顔料成分
[(A)〜(D)]の合計量が10〜60重量部の各量比で含有
することを特徴とするメタリック塗料組成物。1. A composition comprising (A) a titanium dioxide pigment, (B) a flake-like aluminum pigment carrying a pigment, (C) a coloring pigment other than titanium dioxide, (D) a pearl pigment, and (E) a film-forming resin. And (A) / (B) are 2 /
8 to 6/4 (weight ratio), [(A) + (B)] / (C) is 99/1 to 80/20 (weight ratio), [(A) + (B) +
(C)] 20 to 60 parts by weight of (D) based on 100 parts by weight, and pigment component based on 100 parts by weight of resin solid content of (E).
A metallic coating composition, wherein the total amount of [(A) to (D)] is 10 to 60 parts by weight.
料、(B)顔料担持鱗片状アルミニウム顔料、(C)二
酸化チタン以外の着色顔料、(D)パール顔料、および
(E)塗膜形成樹脂を組成成分とし、これら成分を
(A)/(B)が2/8〜6/4(重量比)、〔(A)
+(B)〕/(C)が99/1〜80/20(重量
比)、〔(A)+(B)+(C)〕100重量部に対し
(D)が20〜60重量部、(E)の樹脂固形分100
重量部に対する顔料成分[(A)〜(D)]の合計量が10〜6
0重量部の各量比で含有するメタリック塗料をベースコ
ートしたのち、クリヤー塗料をトップコートし、ベース
コートおよびトップコートを同時に硬化させることを特
徴とするメタリック塗膜の形成法。2. On the surface of a substrate to be coated, (A) a titanium dioxide pigment, (B) a flaky aluminum pigment carrying a pigment, (C) a coloring pigment other than titanium dioxide, (D) a pearl pigment, and (E) a coating. The film forming resin is used as a composition component, and (A) / (B) is 2/8 to 6/4 (weight ratio), [(A)
+ (B)] / (C) is 99/1 to 80/20 (weight ratio), (D) is 20 to 60 parts by weight with respect to [(A) + (B) + (C)] 100 parts by weight, (E) 100 resin solids
The total amount of the pigment components [(A) to (D)] is 10 to 6 parts by weight.
A method for forming a metallic coating film, comprising: after a base coat of a metallic paint containing 0 parts by weight, a top coat of a clear paint, and simultaneously curing the base coat and the top coat.