WELDING INSTRUCTIONS FOR TOOLHOLDERS


M ATERIA L
MICROALLOYED HEAT-TREATABLE STEEL 34MnCrB4+Ti

Chemical composition C 0,33-0,37


(in %) Mn 1,35-1,50
Cr 0,20-0,50
B 0,0015-0,0050
Ti 0,020-0,060
Si 0,15-0,30
Al 0,015-0,060
S 0,02-0,035
Cu 0,00-0,25
Mo 0,00-0,06
P 0,000-0,045

P R E - W E L D H E AT T R E AT M E N T R E C O M M E N D AT I O N F O R E L E C T R O D E S
INERT GAS WELDING (MAGC/MAGM)
Before welding, preheat the holder or welding bar to a
temperature of approximately 250°C to prevent crack DIN 8559 SG 3
formation. Please dry the electrodes for two hours at DIN 8575 SGMo
300°C before starting the welding process
AWS A 5.18 ER 70S-6

CURRENT SOURCE AWS A 5.28 ER 80S-G


SFA-5.18 ER 70S-6
Direct current (DC)
SFA-5.28 ER 80S-G
B.S. 2901 A30

WELDING WELDING WITHOUT INERT GAS

Multiple layer welding DIN 8529 EY 42 65 Mn B


DIN 8529 EY 4664 Mo B
Do not heat over 350°C to avoid tensile DIN 8529 EY 4664 Mo
strength 1450-1600 N/mm2 loss. DIN 8575 E Mo B 29
DIN 8575 E Mo B 26
In order to reduce welding stress, the AWS A 5.1 E 7018DIN 8575
material should be allowed to cool down AWS A 5.5 E 7015-A 1
slowly. AWS A 5.45 E 7018-A 1
SFA-5.1 E 7018
SFA-5.5 E 7015-A 1
SFA-5.5 E 7018-A 1
B.S. 639 E 5154 B
B.S. 249 Mo BH
B.S. 2493 Mo BHJ