WO2016148045A1 - Steel sheet for hot pressing and method for producing same - Google Patents
Steel sheet for hot pressing and method for producing same Download PDFInfo
- Publication number
- WO2016148045A1 WO2016148045A1 PCT/JP2016/057710 JP2016057710W WO2016148045A1 WO 2016148045 A1 WO2016148045 A1 WO 2016148045A1 JP 2016057710 W JP2016057710 W JP 2016057710W WO 2016148045 A1 WO2016148045 A1 WO 2016148045A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- steel sheet
- less
- hot pressing
- steel
- hot
- Prior art date
Abstract
Description
C:0.15%以上、0.40%以下、
Si:1.00%以上、2.00%以下、
Mn:1.50%以上、3.00%以下、
Ti:(N×48/14)%以上、0.10%以下、
B:0.0005%以上、0.0050%以下、
Al:0%超、0.10%以下、
P:0%超、0.05%以下、
S:0%超、0.01%以下、および
N:0%超、0.010%以下
を含有し、残部が鉄および不可避不純物からなり、
転位密度が10×1014/m2以上であり、かつ
全組織に占めるパーライトの面積率が30%以上であり、更に
引張強さが1100MPa以下であるところに特徴を有する。 The hot-press steel sheet of the present invention that has solved the above-mentioned problems is in mass%,
C: 0.15% or more, 0.40% or less,
Si: 1.00% or more, 2.00% or less,
Mn: 1.50% or more, 3.00% or less,
Ti: (N × 48/14)% or more, 0.10% or less,
B: 0.0005% or more, 0.0050% or less,
Al: more than 0%, 0.10% or less,
P: more than 0%, 0.05% or less,
S: more than 0%, 0.01% or less, and N: more than 0%, 0.010% or less, the balance consisting of iron and inevitable impurities,
The dislocation density is 10 × 10 14 / m 2 or more, the area ratio of pearlite in the entire structure is 30% or more, and the tensile strength is 1100 MPa or less.
(i)MoとCrのうちの少なくとも1種の元素を、合計で、0%超、0.50%以下
(ii)CuとNiのうちの少なくとも1種の元素を、合計で、0%超、0.50%以下
(iii)Nb、VおよびZrよりなる群から選択される少なくとも1種の元素を、合計で、0%超、0.10%以下 The steel sheet may further contain one or more of the following (i) to (iii) by mass%.
(I) At least one element of Mo and Cr in total exceeding 0% and 0.50% or less (ii) At least one element in Cu and Ni totaling more than 0% , 0.50% or less (iii) at least one element selected from the group consisting of Nb, V and Zr in total, more than 0% and 0.10% or less
前述の通りSiを比較的多く含有させることによって、部材強度が安定して得られる。しかしSiや後述するMn等の合金元素が多く含まれると、マルテンサイトやベイナイトといった硬質なミクロ組織が増加しやすく鋼板強度が上昇する。引張強さの抑えられた鋼板を得るには、上記マルテンサイトやベイナイトなどの硬質な相が極力少ないミクロ組織とする必要がある。この観点から、本発明ではパーライトを積極的に含有させることとした。また、フェライトが多くパーライトが少ない場合、引張強さは抑えられるが次の様な問題がある。即ち、パーライトが少なくなると炭化物が局所的に集まるようになり、加熱中の逆変態での炭素の拡散が遅くなる。昇温速度が一定の場合、拡散時間の遅れを加熱温度で補う必要がある。その結果、熱間プレスにより一定以上の強度を確保するための最低加熱温度を高める必要がある。この最低加熱温度が高くなると、前述の通り鋼板表面の酸化や亜鉛めっき層の消失が生じやすくなる。この観点からも、パーライトを積極的に含有させる必要がある。 The area ratio of pearlite in the entire structure is 30% or more. By containing a relatively large amount of Si as described above, the member strength can be stably obtained. However, when a large amount of alloy elements such as Si and Mn described later are contained, the hard microstructure such as martensite and bainite tends to increase, and the steel sheet strength increases. In order to obtain a steel sheet with reduced tensile strength, it is necessary to have a microstructure with as few hard phases as possible such as martensite and bainite. From this viewpoint, in the present invention, pearlite is positively included. Further, when there is a large amount of ferrite and a small amount of pearlite, the tensile strength is suppressed, but there are the following problems. That is, when the amount of pearlite decreases, carbides gather locally, and the diffusion of carbon in the reverse transformation during heating becomes slow. When the heating rate is constant, it is necessary to compensate for the delay in diffusion time with the heating temperature. As a result, it is necessary to increase the minimum heating temperature for securing a certain strength or higher by hot pressing. When this minimum heating temperature becomes high, the oxidation of the steel plate surface and the disappearance of the galvanized layer are likely to occur as described above. Also from this viewpoint, it is necessary to actively contain pearlite.
ミクロ組織の転位密度を高めることによって、加熱時のオーステナイト化を促進させることができる。加熱時のオーステナイト化を促進できると、部材強度を確保するための加熱温度を低くすることが可能となり、結果として、鋼板表面の酸化や亜鉛めっき層の消失を抑制することができる。 The dislocation density of the steel sheet is 10 × 10 14 / m 2 or more. By increasing the dislocation density of the microstructure, austenitization during heating can be promoted. If the austenitization at the time of heating can be promoted, the heating temperature for securing the member strength can be lowered, and as a result, the oxidation of the steel sheet surface and the disappearance of the galvanized layer can be suppressed.
Cは、熱間プレスして得られる部材の強度確保のために重要な元素である。部材強度としてミクロビッカース硬さで400Hv以上を達成するには、C量を0.15%以上とする必要がある。C量は、好ましくは0.18%以上、より好ましくは0.20%以上である。一方、C量が0.40%を超えると溶接部の強度が低下する。C量は、好ましくは0.38%以下、より好ましくは0.35%以下である。 C: 0.15% or more and 0.40% or less C is an important element for securing the strength of a member obtained by hot pressing. In order to achieve a member strength of 400 Hv or more in micro Vickers hardness, the C content needs to be 0.15% or more. The amount of C is preferably 0.18% or more, more preferably 0.20% or more. On the other hand, if the amount of C exceeds 0.40%, the strength of the welded portion decreases. The amount of C is preferably 0.38% or less, more preferably 0.35% or less.
Mnは、安定した部材強度を得るために有効な元素である。詳細にはMnは、熱間プレスにおいて、加熱から熱間プレス開始までの間のフェライトなどの軟質層の生成を抑制したり、熱間プレス中および熱間プレス後の冷却過程でのフェライトなどの軟質層やベイナイト相の生成を抑制して、安定した部材強度を得るのに有効な元素である。この効果を発揮させるため、Mn量を1.50%以上とする必要がある。Mn量は、好ましくは1.60%以上、より好ましくは1.80%以上、更に好ましくは2.00%以上である。一方、Mn量が過剰であると、熱間プレス前の鋼板強度が著しく上昇するため、Mn量は3.00%以下とする。Mn量は、好ましくは2.50%以下、より好ましくは2.30%以下である。 Mn: 1.50% or more and 3.00% or less Mn is an element effective for obtaining stable member strength. Specifically, Mn suppresses the formation of a soft layer such as ferrite during the hot press to the start of hot press, or the like during the cooling process during and after the hot press. It is an effective element for obtaining a stable member strength by suppressing the formation of a soft layer or a bainite phase. In order to exhibit this effect, it is necessary to make the amount of Mn 1.50% or more. The amount of Mn is preferably 1.60% or more, more preferably 1.80% or more, and still more preferably 2.00% or more. On the other hand, if the amount of Mn is excessive, the strength of the steel plate before hot pressing is remarkably increased, so the amount of Mn is set to 3.00% or less. The amount of Mn is preferably 2.50% or less, more preferably 2.30% or less.
Tiは、鋼板中のNを固定してBによる焼入れ性を確保するために重要な元素である。そのためTi量は少なくとも、鋼板中のNを全てTiNとして固定する量が必要となる。またTiは、ミクロ組織を微細化する効果があり、部材の靭性を改善する効果も有する。これらの観点から、Ti量は(N×48/14)%以上とする。前記Nは鋼板中の質量%でのN量をいう。Ti量は、好ましくは0.02%以上、より好ましくは0.03%以上である。一方、Ti量が過剰になると、鋼板強度が著しく上昇するため、Ti量は0.10%以下とする。Ti量は、好ましくは0.08%以下、より好ましくは0.06%以下である。 Ti: (N × 48/14)% or more and 0.10% or less Ti is an important element for securing N in the steel sheet and ensuring hardenability by B. Therefore, at least the amount of Ti is required to fix all N in the steel plate as TiN. Ti also has the effect of refining the microstructure and has the effect of improving the toughness of the member. From these viewpoints, the Ti amount is set to (N × 48/14)% or more. Said N means the amount of N in the mass% in a steel plate. The amount of Ti is preferably 0.02% or more, more preferably 0.03% or more. On the other hand, if the Ti amount is excessive, the steel sheet strength is remarkably increased, so the Ti amount is 0.10% or less. The amount of Ti is preferably 0.08% or less, more preferably 0.06% or less.
Bは、鋼板の焼入れ性を向上させるために重要な元素である。特には、Bを含有させ焼入れ性を向上させることによって、部材強度を安定して得ることができる。該効果を発揮させるには、Bを0.0005%以上含有させる必要がある。B量は、好ましくは0.0010%以上、より好ましくは0.0015%以上である。一方、B量が過剰になると、粗大な鉄ボロン化合物が析出し、靭性が低下する。よってB量は0.0050%以下とする。B量は、好ましくは0.0040%以下、より好ましくは0.0035%以下である。 B: 0.0005% or more and 0.0050% or less B is an important element for improving the hardenability of the steel sheet. In particular, the strength of the member can be stably obtained by containing B and improving the hardenability. In order to exhibit this effect, it is necessary to contain B 0.0005% or more. The amount of B is preferably 0.0010% or more, more preferably 0.0015% or more. On the other hand, when the amount of B becomes excessive, a coarse iron boron compound precipitates and toughness falls. Therefore, the B content is 0.0050% or less. The amount of B is preferably 0.0040% or less, more preferably 0.0035% or less.
Alは、脱酸に必要な元素である。この観点から、0%超、更には0.01%以上含みうる。しかし、Al量が過剰になると鋼板のAc3点が上昇する。鋼板のAc3点が高まると、熱間プレス時の加熱温度を高める必要が生じ、前述の通り鋼板表面の酸化や亜鉛めっき層の消失が生じやすくなる。よってAl量は0.10%以下とする。Al量は、好ましくは0.08%以下、より好ましくは0.06%以下である。 Al: more than 0% and 0.10% or less Al is an element necessary for deoxidation. In this respect, it may contain more than 0%, further 0.01% or more. However, when the amount of Al becomes excessive, the Ac 3 point of the steel plate rises. When the Ac 3 point of the steel plate is increased, it is necessary to increase the heating temperature during hot pressing, and as described above, oxidation of the steel plate surface and disappearance of the galvanized layer are likely to occur. Therefore, the Al content is 0.10% or less. The amount of Al is preferably 0.08% or less, more preferably 0.06% or less.
MoとCrは、焼入れ性の向上に寄与する元素である。該効果を発揮させるには、MoとCrのうちの少なくとも1種の元素を、合計で0%超含有させることが好ましく、より好ましくは合計で0.01%以上である。上記「合計で」とは、単独の場合は単独量を示し、複数元素を含む場合は合計量であることを意味する。以下同じである。 At least one element of Mo and Cr: in total, more than 0% and 0.50% or less Mo and Cr are elements that contribute to the improvement of hardenability. In order to exert the effect, it is preferable to contain at least one element of Mo and Cr in total exceeding 0%, and more preferably 0.01% or more in total. The above “in total” means a single amount when used alone, and means a total amount when plural elements are included. The same applies hereinafter.
CuとNiは、部材の耐遅れ破壊特性の改善に寄与する元素であり、必要に応じて含有させることができる。上記効果を発揮させるには、CuとNiのうちの少なくとも1種の元素を、合計で0%超含有させることが好ましく、より好ましくは合計で0.05%以上である。しかし、これらの元素が過剰に含まれると、鋼板の表面疵、最終的には部材の表面疵の発生要因となる。よって、CuとNiのうちの少なくとも1種の元素は、合計で0.50%以下とすることが好ましく、より好ましくは合計で0.30%以下である。 At least one element of Cu and Ni: in total, more than 0% and 0.50% or less Cu and Ni are elements that contribute to the improvement of delayed fracture resistance of the member, and are included as necessary be able to. In order to exert the above effect, it is preferable to contain at least one element of Cu and Ni in total exceeding 0%, and more preferably 0.05% or more in total. However, when these elements are excessively contained, it causes generation of surface flaws on the steel sheet and finally surface flaws on the member. Accordingly, at least one element of Cu and Ni is preferably 0.50% or less in total, and more preferably 0.30% or less in total.
Nb、VおよびZrは、Tiと同様にミクロ組織を微細化する効果を有している。よって、例えばTiの含有量をNの固定に必要な最小限とし、これらの元素でミクロ組織の微細化を実現することもできる。特に高温でのオーステナイト粒の成長抑制には、これらの元素がより効果的である。この観点から、Nb、VおよびZrよりなる群から選択される少なくとも1種の元素は、合計で0.005%以上含有させることが好ましく、より好ましくは合計で0.010%以上である。一方、これらの元素が過剰に含まれると、熱間プレス前の鋼板強度が上昇する。よってNb、VおよびZrよりなる群から選択される少なくとも1種の元素の含有量は、合計で0.10%以下とすることが好ましく、より好ましくは合計で0.050%以下である。 A total of at least one element selected from the group consisting of Nb, V and Zr is more than 0% and not more than 0.10%. Nb, V and Zr have the effect of refining the microstructure like Ti. Have. Therefore, for example, the content of Ti can be made the minimum necessary for fixing N, and refinement of the microstructure can be realized with these elements. In particular, these elements are more effective in suppressing the growth of austenite grains at high temperatures. In this respect, at least one element selected from the group consisting of Nb, V and Zr is preferably contained in a total amount of 0.005% or more, and more preferably in a total of 0.010% or more. On the other hand, when these elements are excessively contained, the steel plate strength before hot pressing increases. Therefore, the content of at least one element selected from the group consisting of Nb, V and Zr is preferably 0.10% or less in total, and more preferably 0.050% or less in total.
(a)550℃以上で巻き取る工程;および、
(b)20%以上の冷延率で冷間圧延を行う工程;
を順に含むようにする。以下、各工程について詳述する。 After the above hot rolling,
(A) a step of winding at 550 ° C. or higher; and
(B) a step of cold rolling at a cold rolling rate of 20% or more;
In order. Hereinafter, each process is explained in full detail.
鋼板をコイルに巻き取る温度を、550℃以上とすることによって、規定量のパーライトを確保することができる。この様に巻取温度を高めることによって、熱延鋼板の強度を低下させ、後述の冷延率を高めることもできる。前記巻取温度は、好ましくは580℃以上、より好ましくは630℃以上である。尚、巻取温度の上限は、鋼板表面の酸化による劣化の観点から750℃程度である。 (A) Step of winding at 550 ° C. or higher A specified amount of pearlite can be secured by setting the temperature at which the steel sheet is wound around the coil to 550 ° C. or higher. By increasing the coiling temperature in this way, the strength of the hot-rolled steel sheet can be reduced and the cold rolling rate described later can be increased. The winding temperature is preferably 580 ° C. or higher, more preferably 630 ° C. or higher. In addition, the upper limit of coiling temperature is about 750 degreeC from a viewpoint of deterioration by the oxidation of the steel plate surface.
冷間圧延は、鋼板に転位を導入するための有効手段である。冷間圧延により規定の密度以上の転位を導入するため、冷間圧延率、即ち冷延率を20%以上とする。冷延率は、好ましくは25%以上、より好ましくは30%以上である。一方、冷延率の上限は、設備仕様に応じて適宜決定すればよく、例えば80%以下とすることができる。本発明は、鋼板の引張強さを1100MPa以下とするものであるが、該引張強さをより低い1000MPa以下に抑えるには、上記冷延率を60%未満とすることが挙げられる。 (B) Step of performing cold rolling at a cold rolling rate of 20% or more Cold rolling is an effective means for introducing dislocations into a steel sheet. In order to introduce dislocations of a specified density or higher by cold rolling, the cold rolling rate, that is, the cold rolling rate is set to 20% or more. The cold rolling rate is preferably 25% or more, more preferably 30% or more. On the other hand, the upper limit of the cold rolling rate may be determined as appropriate according to the equipment specifications, and may be, for example, 80% or less. In the present invention, the tensile strength of the steel sheet is set to 1100 MPa or less. In order to suppress the tensile strength to a lower value of 1000 MPa or less, the cold rolling rate is set to less than 60%.
焼鈍工程では、焼鈍温度:500℃以上で加熱することによって、冷間圧延後の鋼板強度の低下を図ることができる。前記焼鈍温度は、好ましくは550℃以上である。一方、焼鈍温度が640℃を超えると、冷間圧延により高めた転位密度が急速に減少する。よって焼鈍温度は640℃以下とする。焼鈍温度は、好ましくは620℃以下、より好ましくは600℃以下である。 (C) Annealing temperature: 500 ° C. or more and 640 ° C. or less, and a residence time in a temperature range of 500 ° C. or more: An annealing process performed under the condition of 500 seconds or less. The strength of the steel sheet after hot rolling can be reduced. The annealing temperature is preferably 550 ° C. or higher. On the other hand, when the annealing temperature exceeds 640 ° C., the dislocation density increased by cold rolling rapidly decreases. Therefore, annealing temperature shall be 640 degrees C or less. An annealing temperature becomes like this. Preferably it is 620 degrees C or less, More preferably, it is 600 degrees C or less.
本発明では、熱間プレス、即ちホットスタンプの条件は特に限定されず、通常、行われる方法を採用することができる。前記熱間プレスは、加熱工程、スタンピング工程および冷却工程を含む。以下、各工程について説明する。 Hot pressing In the present invention, the conditions of hot pressing, that is, hot stamping are not particularly limited, and a generally performed method can be employed. The hot press includes a heating process, a stamping process, and a cooling process. Hereinafter, each step will be described.
加熱温度:700~900℃に加熱してから熱間プレスを行う。前記加熱の方法として、炉加熱、通電加熱、誘導加熱等を採用することができる。加熱温度は、十分にオーステナイト化を図るために700℃以上とする。好ましくは750℃以上である。一方、前述の通り、この加熱温度が高すぎると、鋼板表面の酸化が生じやすく、また熱間プレス用鋼板として亜鉛めっき鋼板を用いた場合、亜鉛めっき層が消失しやすくなる。よって、上記鋼板表面の酸化や上記亜鉛めっき層の消失を抑制する観点から、加熱温度は900℃以下とする。好ましくは880℃以下である。 Heating process Heating temperature: Hot pressing is performed after heating to 700 to 900 ° C. As the heating method, furnace heating, energization heating, induction heating, or the like can be employed. The heating temperature is set to 700 ° C. or higher in order to sufficiently achieve austenitization. Preferably it is 750 degreeC or more. On the other hand, as described above, when the heating temperature is too high, the surface of the steel sheet is likely to be oxidized, and when a galvanized steel sheet is used as the steel sheet for hot pressing, the galvanized layer tends to disappear. Therefore, from the viewpoint of suppressing oxidation of the steel sheet surface and disappearance of the galvanized layer, the heating temperature is set to 900 ° C. or lower. Preferably it is 880 degrees C or less.
スタンピング工程では、上記加熱工程によって加熱された鋼板にスタンピング、即ちプレス加工を施す。該スタンピングの開始温度は特に限定されない。 Stamping process In the stamping process, the steel sheet heated by the heating process is stamped, that is, pressed. The starting temperature of the stamping is not particularly limited.
冷却工程では、上記加熱工程によって加熱された鋼板、および該鋼板にスタンピングを施して得られる鋼部品を冷却する。なお、ここでの冷却は自然冷却も含み、加熱工程の直後から鋼板の冷却が開始する。 Cooling step In the cooling step, the steel plate heated by the heating step and a steel part obtained by stamping the steel plate are cooled. The cooling here includes natural cooling, and cooling of the steel sheet starts immediately after the heating step.
この実施例1では、鋼板中のSi量が、熱間プレス時の冷却速度と鋼板の硬さの関係に及ぼす影響について調べた。 Example 1
In Example 1, the influence of the amount of Si in the steel sheet on the relationship between the cooling rate during hot pressing and the hardness of the steel sheet was examined.
実施例2では、鋼板の転位密度が、熱間プレス時の加熱温度に及ぼす影響について調べた。詳細には、鋼板の転位密度が、熱間プレスにより一定以上の強度確保に必要な加熱温度、即ち、最低加熱温度に及ぼす影響について調べた。 Example 2
In Example 2, the influence of the dislocation density of the steel sheet on the heating temperature during hot pressing was examined. Specifically, the influence of the dislocation density of the steel sheet on the heating temperature necessary for ensuring a certain level of strength by hot pressing, that is, the minimum heating temperature was examined.
鋼板の転位密度はX線回折法により求めた。詳細は次の通りである。測定装置は株式会社リガク製 X線回折装置 RINT-1500を用いた。具体的にはX線源ターゲットとしてCoを使用して、線源出力40kV-200mAに設定し、受光モノクロメーターを用いて線源を単色化した。測定サンプルをディフラクトメーターに設置し、連続測定により2θ=40°~130°までのX線回折強度を測定した。 Measurement of dislocation density The dislocation density of the steel sheet was determined by the X-ray diffraction method. Details are as follows. The measuring apparatus used was an X-ray diffractometer RINT-1500 manufactured by Rigaku Corporation. Specifically, Co was used as the X-ray source target, the radiation source output was set to 40 kV-200 mA, and the radiation source was monochromatic using a light-receiving monochromator. The measurement sample was placed in a diffractometer, and the X-ray diffraction intensity from 2θ = 40 ° to 130 ° was measured by continuous measurement.
次に、各冷延鋼板を用いて、熱間プレスにより一定以上の強度確保に必要な最低加熱温度を次の様にして求めた。即ち、熱間プレス工程における加熱を模擬した熱処理として、種々の加熱温度まで冷延鋼板を加熱し、該加熱温度に到達後、保持することなく室温まで自然放冷して試験用鋼板を得た。上記熱処理は、富士電波工機株式会社製の熱間加工再現装置「サーモマスターZ」を用いて行った。また室温から上記加熱温度までの平均加熱速度は100℃/sとした。本実施例では、上記の通り冷延率が種々であるため、得られる冷延鋼板の板厚は種々である。この板厚による自然放冷速度の差を解消するため、上記熱処理には、冷間圧延後の鋼板を研削して板厚1.4mmに統一したものを用いた。 Measurement of minimum heating temperature necessary for securing a certain level of strength by hot pressing Next, using each cold-rolled steel sheet, the minimum heating temperature necessary for securing a certain level of strength by hot pressing is determined as follows. It was. That is, as a heat treatment simulating the heating in the hot pressing process, the cold-rolled steel sheet was heated to various heating temperatures, and after reaching the heating temperature, the steel sheet was naturally allowed to cool to room temperature without holding to obtain a test steel sheet. . The heat treatment was carried out using a hot working reproduction apparatus “Thermomaster Z” manufactured by Fuji Electric Koki Co., Ltd. The average heating rate from room temperature to the heating temperature was 100 ° C./s. In this example, since the cold rolling rate is various as described above, the thickness of the obtained cold rolled steel sheet is various. In order to eliminate the difference in the natural cooling rate due to the plate thickness, the heat treatment was performed by grinding the cold-rolled steel plate and unifying it to a plate thickness of 1.4 mm.
実施例3では、鋼板の製造条件が、ミクロ組織や転位密度、結果として鋼板の引張強さや最低加熱温度に及ぼす影響について調べた。 Example 3
In Example 3, the influence of the manufacturing conditions of the steel sheet on the microstructure, dislocation density, and consequently the tensile strength and minimum heating temperature of the steel sheet was examined.
ミクロ組織の観察は、鋼板の板厚の1/4位置を倍率1000倍でSEM(Scanning Electron Microscope)観察し、その視野におけるパーライトの面積率を点算法により算出した。SEM写真の1視野のサイズは90μm×120μmである。点算法におけるメッシュサイズは1視野を縦20点、横20点に分割して実施した。即ち、1視野につき400点の測定を行ってパーライトの面積率を求め、合計3視野の平均値を求めた。なお、本発明におけるパーライトには擬似パーライトも含まれる。前記ミクロ組織の観察は、鋼板が製品コイルの状態では、コイル幅方向の1/4位置であって、上述の通り鋼板の板厚の1/4位置で行えばよい。または、ブランキング加工後であって熱間プレス前の鋼板の任意の位置でミクロ組織の観察を行ってもよい。 Observation of microstructure and measurement of pearlite area ratio Microstructure observation is performed by observing a 1/4 position of the thickness of the steel sheet at a magnification of 1000 times by SEM (Scanning Electron Microscope), and calculating the area ratio of pearlite in the field of view by a point calculation method. Calculated. The size of one field of view of the SEM photograph is 90 μm × 120 μm. The mesh size in the point calculation method was implemented by dividing one field of view into 20 vertical and 20 horizontal points. That is, 400 points per field of view were measured to determine the area ratio of pearlite, and the average value of a total of three fields of view was determined. The pearlite in the present invention includes pseudo pearlite. The observation of the microstructure may be performed at the 1/4 position in the coil width direction when the steel sheet is a product coil, and at the 1/4 position of the thickness of the steel sheet as described above. Alternatively, the microstructure may be observed at an arbitrary position on the steel sheet after blanking and before hot pressing.
鋼板から引張試験用試験片として、JIS5号形状の試験片を切り出した。そして、島津製作所製AG-IS 250kN オートグラフ引張試験機を用い、歪み速度:10mm/minとし、JIS Z 2241に規定の方法で、鋼板の引張強さを求めた。 Measurement of tensile strength A test piece having a JIS No. 5 shape was cut out from a steel plate as a test piece for a tensile test. Then, using an AG-
Claims (6)
- 鋼板の成分が、質量%で、
C:0.15%以上、0.40%以下、
Si:1.00%以上、2.00%以下、
Mn:1.50%以上、3.00%以下、
Ti:(N×48/14)%以上、0.10%以下、
B:0.0005%以上、0.0050%以下、
Al:0%超、0.10%以下、
P:0%超、0.05%以下、
S:0%超、0.01%以下、および
N:0%超、0.010%以下
を含有し、残部が鉄および不可避不純物からなり、
転位密度が10×1014/m2以上であり、かつ
全組織に占めるパーライトの面積率が30%以上であり、更に
引張強さが1100MPa以下であることを特徴とする熱間プレス用鋼板。 The component of the steel sheet is mass%,
C: 0.15% or more, 0.40% or less,
Si: 1.00% or more, 2.00% or less,
Mn: 1.50% or more, 3.00% or less,
Ti: (N × 48/14)% or more, 0.10% or less,
B: 0.0005% or more, 0.0050% or less,
Al: more than 0%, 0.10% or less,
P: more than 0%, 0.05% or less,
S: more than 0%, 0.01% or less, and N: more than 0%, 0.010% or less, the balance consisting of iron and inevitable impurities,
A steel sheet for hot pressing, characterized in that the dislocation density is 10 × 10 14 / m 2 or more, the area ratio of pearlite in the entire structure is 30% or more, and the tensile strength is 1100 MPa or less. - 前記鋼板の成分が、更に、質量%で、下記(i)~(iii)のうちの1以上を含む請求項1に記載の熱間プレス用鋼板。
(i)MoとCrのうちの少なくとも1種の元素を、合計で、0%超、0.50%以下
(ii)CuとNiのうちの少なくとも1種の元素を、合計で、0%超、0.50%以下
(iii)Nb、VおよびZrよりなる群から選択される少なくとも1種の元素を、合計で、0%超、0.10%以下 The steel sheet for hot pressing according to claim 1, wherein the steel sheet further contains at least one of the following (i) to (iii) by mass%.
(I) At least one element of Mo and Cr in total exceeding 0% and 0.50% or less (ii) At least one element in Cu and Ni totaling more than 0% , 0.50% or less (iii) at least one element selected from the group consisting of Nb, V and Zr in total, more than 0% and 0.10% or less - 前記鋼板の少なくとも片面に亜鉛系めっき層またはアルミ系めっき層を有する請求項1に記載の熱間プレス用鋼板。 The steel plate for hot pressing according to claim 1, wherein the steel plate has a zinc-based plating layer or an aluminum-based plating layer on at least one side of the steel plate.
- 前記鋼板の少なくとも片面に亜鉛系めっき層またはアルミ系めっき層を有する請求項2に記載の熱間プレス用鋼板。 The steel sheet for hot pressing according to claim 2, wherein the steel sheet has a zinc-based plating layer or an aluminum-based plating layer on at least one side thereof.
- 請求項1~4のいずれかに記載の熱間プレス用鋼板を製造する方法であって、
前記鋼板の成分組成を満たす鋼を、
仕上圧延温度:890~950℃で熱間圧延後、
550℃以上で巻き取る工程;および
20%以上の冷延率で冷間圧延を行う工程;を順に含み、
前記冷間圧延後の鋼板の引張強さが1100MPaを超える場合は、上記冷間圧延後、更に、焼鈍温度:500℃以上640℃以下、かつ500℃以上の温度域の滞在時間:500秒以下の条件で焼鈍を行う工程を含むことを特徴とする熱間プレス用鋼板の製造方法。 A method for producing a hot-press steel sheet according to any one of claims 1 to 4,
Steel satisfying the component composition of the steel sheet,
Finish rolling temperature: After hot rolling at 890-950 ° C,
A step of winding at 550 ° C. or higher; and a step of cold rolling at a cold rolling rate of 20% or higher;
When the tensile strength of the steel sheet after the cold rolling exceeds 1100 MPa, after the cold rolling, the annealing temperature: 500 ° C. or more and 640 ° C. or less, and the residence time in the temperature range of 500 ° C. or more: 500 seconds or less The manufacturing method of the steel plate for hot press characterized by including the process of annealing on the conditions of this. - 請求項1~4のいずれかに記載の熱間プレス用鋼板を用い、加熱温度:700~900℃で加熱してから熱間プレスを行うことを特徴とする鋼部品の製造方法。
A method for producing a steel part, wherein the hot pressing steel sheet according to any one of claims 1 to 4 is used and hot pressing is performed after heating at a heating temperature of 700 to 900 ° C.