Nothing Special   »   [go: up one dir, main page]

WO2010140704A1 - S-(3-アミノプロピル)チオ硫酸またはその金属塩の使用 - Google Patents

S-(3-アミノプロピル)チオ硫酸またはその金属塩の使用 Download PDF

Info

Publication number
WO2010140704A1
WO2010140704A1 PCT/JP2010/059588 JP2010059588W WO2010140704A1 WO 2010140704 A1 WO2010140704 A1 WO 2010140704A1 JP 2010059588 W JP2010059588 W JP 2010059588W WO 2010140704 A1 WO2010140704 A1 WO 2010140704A1
Authority
WO
WIPO (PCT)
Prior art keywords
weight
rubber
aminopropyl
parts
vulcanized rubber
Prior art date
Application number
PCT/JP2010/059588
Other languages
English (en)
French (fr)
Inventor
オズトゥルクオルハン
上北泰生
竹内謙一
Original Assignee
住友化学株式会社
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 住友化学株式会社 filed Critical 住友化学株式会社
Priority to BRPI1013761A priority Critical patent/BRPI1013761A2/pt
Priority to CN201080024118.8A priority patent/CN102449054B/zh
Priority to KR1020117031177A priority patent/KR101784018B1/ko
Priority to RU2011153413/05A priority patent/RU2528996C2/ru
Priority to US13/375,859 priority patent/US8664432B2/en
Priority to EP10783486.3A priority patent/EP2439237B1/en
Publication of WO2010140704A1 publication Critical patent/WO2010140704A1/ja

Abstract

加硫ゴムが有する粘弾性特性を改善させるためのS-(3-アミノプロピル)チオ硫酸および/またはその金属塩の使用。

Description

S−(3−アミノプロピル)チオ硫酸またはその金属塩の使用
 本発明は、S−(3−アミノプロピル)チオ硫酸またはその金属塩の使用に関する。
 近年、環境保護の要請から、自動車の燃費向上(すなわち、低燃費化)が求められている。そして、自動車用タイヤの分野において、粘弾性特性を改善させることにより、自動車の燃費が向上することが知られている(日本ゴム協会編「ゴム技術入門」丸善株式会社、124頁参照)。
 本発明は、
<1> 加硫ゴムが有する粘弾性特性を改善させるためのS−(3−アミノプロピル)チオ硫酸および/またはその金属塩の使用;
<2> S−(3−アミノプロピル)チオ硫酸の金属塩における金属イオンが、リチウムイオン、ナトリウムイオン、カリウムイオン、セシウムイオン、コバルトイオン、銅イオンまたは亜鉛イオンである<1>に記載の使用;
<3> S−(3−アミノプロピル)チオ硫酸の金属塩における金属イオンが、リチウムイオン、ナトリウムイオンまたはカリウムイオンである<1>に記載の使用;
<4> S−(3−アミノプロピル)チオ硫酸の金属塩が、式(2)
(HN−(CH−SSO ・Mn+      (2)
(式中、Mn+は金属イオンを表わし、nはその価数を表わす。)
で示される3−アミノプロピルチオスルファートである<1>に記載の使用;
<5> 金属イオンが、リチウムイオン、ナトリウムイオン、カリウムイオン、セシウムイオン、コバルトイオン、銅イオンまたは亜鉛イオンである<4>に記載の使用;
<6> 金属イオンが、リチウムイオン、ナトリウムイオンまたはカリウムイオンである<4>に記載の使用;を提供するものである。
 本発明において、”粘弾性特性を改善させる”とは、”加硫ゴムの損失係数(tanδ)を改変させる”ことを意味する。
 本発明に用いるS−(3−アミノプロピル)チオ硫酸は、式(1)
N−(CH−SSOH     (1)
で示される化合物であり、その金属塩は、式(2)
(HN−(CH−SSO ・Mn+      (2)
(式中、Mn+は金属イオンを表し、nはその価数を表す。)
で示される3−アミノプロピルチオスルファートである。
 S−(3−アミノプロピル)チオ硫酸の金属塩は任意の公知の方法により製造することができる。具体的には、3−ハロプロピルアミンとチオ硫酸ナトリウムとを反応させる方法、フタルイミドのカリウム塩と1,3−ジハロプロパンとを反応させて、得られた化合物とチオ硫酸ナトリウムとを反応させ、次いで、得られた化合物を加水分解する方法が挙げられる。S−(3−アミノプロピル)チオ硫酸は、S−(3−アミノプロピル)チオ硫酸の金属塩とプロトン酸とを反応させることにより製造することができる。
 本発明では、S−(3−アミノプロピル)チオ硫酸とその金属塩の混合物を用いることもできる。かかる混合物は、S−(3−アミノプロピル)チオ硫酸とその金属塩とを混合する方法、金属アルカリ(上記Mで示される金属を含有する水酸化物、炭酸塩および炭酸水素塩等)を用いてS−(3−アミノプロピル)チオ硫酸の一部を金属塩化する方法、プロトン酸を用いてS−(3−アミノプロピル)チオ硫酸の金属塩の一部を中和する方法により製造することができる。このようにして製造したS−(3−アミノプロピル)チオ硫酸またはその金属塩は、濃縮、晶析等の操作により、反応混合物から取り出すことができ、取り出されたS−(3−アミノプロピル)チオ硫酸またはその金属塩は、通常0.1%~5%程度の水分を含む。本発明では、S−(3−アミノプロピル)チオ硫酸のみを用いることができ、また、S−(3−アミノプロピル)チオ硫酸の金属塩のみを用いることもできる。また、複数種のS−(3−アミノプロピル)チオ硫酸の金属塩を併用することもでき、また、S−(3−アミノプロピル)チオ硫酸と、その金属塩を併用することもできる。
 Mn+で示される金属イオンとしては、リチウムイオン、ナトリウムイオン、カリウムイオン、セシウムイオン、コバルトイオン、銅イオンおよび亜鉛イオンが好ましく、リチウムイオン、ナトリウムイオンおよびカリウムイオンがより好ましい。nは金属イオンの価数を表わし、当該金属において可能な範囲であれば、限定されない。金属イオンが、リチウムイオン、ナトリウムイオン、カリウムイオン、セシウムイオンのようなアルカリ金属イオンの場合、nは通常1であり、金属イオンがコバルトイオンの場合、nは通常2または3である。金属イオンが、銅イオンの場合、nは通常1~3の整数であり、金属イオンが、亜鉛イオンの場合、nは通常2である。上記製法によれば、通常、S−(3−アミノプロピル)チオ硫酸のナトリウム塩が得られるが、カチオン交換反応を行うことにより、ナトリウム塩以外の金属塩に変換することができる。
 S−(3−アミノプロピル)チオ硫酸およびその金属塩のメディアン径は、好ましくは0.05~100μmの範囲であり、より好ましくは1~100μmの範囲である。かかるメディアン径は、レーザー回析法にて測定することができる。
 本発明は、加硫ゴムが有する粘弾性特性を改善させるためのS−(3−アミノプロピル)チオ硫酸および/またはその金属塩の使用であり、S−(3−アミノプロピル)チオ硫酸および/またはその金属塩を加硫ゴムの製造時に配合することにより通常実施される。
 加硫ゴムは、通常、ゴム成分、充填剤および硫黄成分を含む。
 S−(3−アミノプロピル)チオ硫酸またはその金属塩の使用量は、加硫ゴム中のゴム成分100重量部に対して、0.1~10重量部の範囲が好ましく、0.3~3重量部の範囲がより好ましい。
<ゴム成分>
 ゴム成分としては、天然ゴム、エポキシ化天然ゴム、脱蛋白天然ゴムおよびその他の変性天然ゴムのほか、ポリイソプレンゴム(IR)、スチレン・ブタジエン共重合ゴム(SBR)、ポリブタジエンゴム(BR)、アクリロニトリル・ブタジエン共重合ゴム(NBR)、イソプレン・イソブチレン共重合ゴム(IIR)、エチレン・プロピレン−ジエン共重合ゴム(EPDM)、ハロゲン化ブチルゴム(HR)等の各種の合成ゴムが挙げられる。なかでも、天然ゴム、スチレン・ブタジエン共重合ゴム、ポリブタジエンゴム等の高不飽和性ゴムが好ましく用いられ、天然ゴムが特に好ましい。天然ゴムとスチレン・ブタジエン共重合ゴムとの併用、天然ゴムとポリブタジエンゴムとの併用等の数種のゴム成分を組み合わせることも有効である。
 天然ゴムとしては、RSS#1、RSS#3、TSR20、SIR20等のグレードの天然ゴムが挙げられる。エポキシ化天然ゴムとしては、エポキシ化度10~60モル%のものが好ましく、具体的には、クンプーラン ガスリー社製ENR25やENR50が挙げられる。脱蛋白天然ゴムとしては、総窒素含有率が0.3重量%以下である脱蛋白天然ゴムが好ましい。変性天然ゴムとしては、天然ゴムに、N,N−ジエチルアミノエチルアクリレート等のN,N−ジアルキルアミノエチルアクリレート、4−ビニルピリジン、2−ヒドロキシアクリレート等を予め反応させて得られる、極性基を含有する変性天然ゴムが好ましい。
 SBRとしては、日本ゴム協会編「ゴム工業便覧<第四版>」第210~211頁に記載されている乳化重合SBRおよび溶液重合SBRが挙げられる。トレッド用ゴム組成物としては、溶液重合SBRが好ましく、日本ゼオン社製「ニッポール(登録商標)NS116」等の4,4’−ビス−(ジアルキルアミノ)ベンゾフェノンを用いて分子末端を変性した溶液重合SBR、JSR社製「SL574」等のハロゲン化スズ化合物を用いて分子末端を変性した溶液重合SBR、旭化成社製「E10」、「E15」等シラン変性溶液重合SBRの市販品や、ラクタム化合物、アミド化合物、尿素系化合物、N,N−ジアルキルアクリルアミド化合物、イソシアネート化合物、イミド化合物、アルコキシ基を有するシラン化合物(トリアルコキシシラン化合物等)またはアミノシラン化合物を用いて、または、スズ化合物とアルコキシ基を有するシラン化合物との併用や、アルキルアクリルアミド化合物とアルコキシ基を有するシラン化合物との併用等の異なる複数の化合物を用いて、分子末端を変性して得られる、分子末端に窒素、スズ、ケイ素のいずれか、または、それら複数の元素を有する溶液重合SBRが、特に好ましい。また、乳化重合SBRまたは溶液重合SBRに、プロセスオイルやアロマオイル等のオイルを添加した油展SBRは、トレッド用ゴム組成物等として好ましく用いることができる。
 BRとしては、シス−1,4−結合が90%以上の高シスBRやシス結合が35%前後の低シスBR等の溶液重合BRが挙げられ、高ビニル含量の低シスBRが好ましい。日本ゼオン製「Nipol(登録商標)BR 1250H」等のスズ変性BRや、4,4‘−ビス−(ジアルキルアミノ)ベンゾフェノン、ハロゲン化スズ化合物、ラクタム化合物、アミド化合物、尿素系化合物、N,N−ジアルキルアクリルアミド化合物、イソシアネート化合物、イミド化合物、アルコキシ基を有するシラン化合物(トリアルコキシシラン化合物等)またはアミノシラン化合物を用いて、または、スズ化合物とアルコキシ基を有するシラン化合物との併用や、アルキルアクリルアミド化合物とアルコキシ基を有するシラン化合物との併用等の異なる複数の化合物を用いて、分子末端を変性して得られる、分子末端に窒素、スズ、ケイ素のいずれか、または、それら複数の元素を有する溶液重合BRが、特に好ましい。これらBRは、トレッド用ゴム組成物やサイドウォール用ゴム組成物として好ましく用いることができ、通常は、SBRおよび/または天然ゴムとブレンドして使用される。ブレンド比率は、トレッド用ゴム組成物においては、総ゴム重量に対して、SBRおよび/または天然ゴムが60~100重量%、BRが0~40重量%であることが好ましく、サイドウォール用ゴム組成物においては、総ゴム重量に対して、SBRおよび/または天然ゴムが10~70重量%、BRが90~30重量%であることが好ましく、総ゴム重量に対して、天然ゴムが40~60重量%、BRが60~40重量%であるブレンドが特に好ましい。この場合、変性SBRと非変性SBRとのブレンドや、変性BRと非変性BRとのブレンドも好ましい。
<充填剤>
 充填剤としては、ゴム分野で通常使用されているカーボンブラック、シリカ、タルク、クレイ、水酸化アルミニウムおよび酸化チタンが挙げられ、カーボンブラックおよびシリカが好ましく、カーボンブラックが特に好ましい。カーボンブラックとしては、日本ゴム協会編「ゴム工業便覧<第四版>」494頁に記載されるものが挙げられ、HAF(High Abrasion Furnace)、SAF(Super Abrasion Furnace)、ISAF(Intermediate SAF)、FEF(Fast Extrusion Furnace)、MAF、GPF(General Purpose Furnace)、SRF(Semi−Reinforcing Furnace)等のカーボンブラックが好ましい。タイヤトレッド用ゴム組成物には、CTAB(Cetyl Trimethyl Ammonium Bromide)表面積が40~250m/gであり、窒素吸着比表面積が20~200m/gであり、且つ、粒子径10~50nmであるカーボンブラックが好ましく用いられ、CTAB表面積70~180m/gであるカーボンブラックがより好ましい。その具体例としては、ASTMの規格において、N110、N220、N234、N299、N326、N330、N330T、N339、N343およびN351が挙げられる。カーボンブラックの表面に、シリカを0.1~50重量%付着させた表面処理カーボンブラックも好ましい。カーボンブラックとシリカとの併用等の数種の充填剤を組み合わせることも有効であり、タイヤトレッド用ゴム組成物には、カーボンブラック単独あるいはカーボンブラックとシリカの両方を用いることが好ましい。カーカス、サイドウォール用ゴム組成物には、CTAB表面積が20~60m/gであり、且つ、粒子径が40~100nmであるカーボンブラックが好ましく用いられ、その具体例としては、ASTMの規格において、N330、N339、N343、N351,N550、N568、N582、N630、N642、N660、N662、N754およびN762が挙げられる。充填剤の使用量は限定されないが、ゴム成分100重量部に対して、5~100重量部の範囲が好ましい。カーボンブラックのみを充填剤として使用する場合、カーボンブラックの使用量は、30~80重量部の範囲がより好ましく、トレッド部材用途においてカーボンブラックとシリカとを併用する場合には、カーボンブラックの使用量は、5~50重量部の範囲が好ましい。
 シリカとしては、CTAB比表面積50~180m/gであるシリカおよび窒素吸着比表面積50~300m/gであるシリカが挙げられ、東ソー・シリカ(株)社製「AQ」、「AQ−N」、デグッサ社製「ウルトラジル(登録商標)VN3」、「ウルトラジル(登録商標)360」、「ウルトラジル(登録商標)7000」、ローディア社製「ゼオシル(登録商標)115GR」、「ゼオシル(登録商標)1115MP」、「ゼオシル(登録商標)1205MP」、「ゼオシル(登録商標)Z85MP」、日本シリカ社製「ニップシール(登録商標)AQ」等の市販品が好ましく用いられる。また、pHが6~8であるシリカやナトリウムを0.2~1.5重量%含むシリカ、真円度が1~1.3の真球状シリカ、ジメチルシリコーンオイル等のシリコーンオイルやエトキシシリル基を含有する有機ケイ素化合物、エタノールやポリエチレングリコール等のアルコールで表面処理したシリカ、二種類以上の異なった窒素吸着比表面面積を有するシリカを配合することも好ましい。
 充填剤の使用量は限定されない。乗用車用トレッド用ゴム組成物には、シリカが好ましく用いられ、ゴム成分100重量部に対して、シリカの使用量は、10~120重量部の範囲が好ましい。シリカを配合する場合、ゴム成分100重量部に対して、5~50重量部のカーボンブラックを配合することが好ましく、カーボンブラックに対するシリカの配合比率(シリカ/カーボンブラック)は0.7/1~1/0.1が特に好ましい。
 充填剤としてシリカを用いる場合、ビス(3−トリエトキシシリルプロピル)テトラスルフィド(デグッサ社製「Si−69」)、ビス(3−トリエトキシシリルプロピル)ジスルフィド(デグッサ社製「Si−75」)、ビス(3−ジエトキシメチルシリルプロピル)テトラスルフィド、ビス(3−ジエトキシメチルシリルプロピル)ジスルフィド、オクタンチオ酸S−[3−(トリエトキシシリル)プロピル]エステル(ジェネラルエレクトロニックシリコンズ社製「NXTシラン」)、オクタンチオ酸S−[3−{(2−メチル−1,3−プロパンジアルコキシ)エトキシシリル}プロピル]エステルおよびオクタンチオ酸S−[3−{(2−メチル−1,3−プロパンジアルコキシ)メチルシリル}プロピル]エステルフェニルトリエトキシシラン、メチルトリメトキシシラン、メチルトリエトキシシラン、メチルトリアセトキシシラン、メチルトリブトキシシラン、エチルトリメトキシシラン、エチルトリエトキシシラン、イソブチルトリメトキシシラン、イソブチルトリエトキシシラン、n−オクチルトリメトキシシラン、n−オクチルトリエトキシシラン、ビニルトリメトキシシラン、ビニルトリエトキシシラン、ビニルトリ(メトキシエトキシ)シラン、フェニルトリメトキシシラン、フェニルトリエトキシシラン、フェニルトリアセトキシシラン、3−メタクリロキシプロピルトリメトキシシラン、3−メタクリロキシプロピルトリエトキシシラン、3−アミノプロピルトリメトキシシラン、3−アミノプロピルトリエトキシシラン、N−(2−アミノエチル)−3−アミノプロピルトリメトキシシラン、N−(2−アミノエチル)−3−アミノプロピルトリエトキシシラン、(3−グリシドキシプロピル)トリメトキシシラン、(3−グリシドキシプロピル)トリエトキシシラン、2−(3,4−エポキシシクロヘキシル)エチルトリメトキシシラン、2−(3,4−エポキシシクロヘキシル)エチルトリエトキシシラン、3−イソシアナートプロピルトリメトキシシランおよび3−イソシアナートプロピルトリエトキシシランからなる群から選択される1種以上のシランカップリング剤等のシリカと結合可能なケイ素等の元素またはアルコシキシラン等の官能基を有する化合物を併用することが好ましく、ビス(3−トリエトキシシリルプロピル)テトラスルフィド(デグッサ社製「Si−69」)、ビス(3−トリエトキシシリルプロピル)ジスルフィド(デグッサ社製「Si−75」)、3−オクタノイルチオプロピルトリエトキシシラン(ジェネラルエレクトロニックシリコンズ社製「NXTシラン」)が特に好ましい。これらの化合物の配合段階は限定されないが、シリカと同じ段階でゴムに配合することが好ましく、配合量は、シリカに対して、好ましくは2~10重量%、より好ましくは7~9重量%である。配合時の温度は、80~200℃の範囲が好ましく、より好ましくは110~180℃の範囲である。充填剤としてシリカを用いる場合、シリカと結合可能なケイ素等の元素またはアルコシキシラン等の官能基を有する化合物およびシリカに加えて、エタノール、ブタノール、オクタノール等の1価アルコールやエチレングリコール、ジエチレングリコール、トリエチレングリコール、ポリエチレングリコール、ポリプロピレングリコール、ペンタエリスリトール、ポリエーテルポリオール等の2価以上のアルコール、N−アルキルアミン、アミノ酸、分子末端がカルボキシル変性またはアミン変性された液状ポリブタジエン等を配合することも好ましい。
 水酸化アルミニウムとしては、窒素吸着比表面積5~250m/gである水酸化アルミニウムおよびDOP給油量50~100ml/100gである水酸化アルミニウムが挙げられる。
<硫黄成分>
 硫黄成分としては、粉末硫黄、沈降硫黄、コロイド硫黄、不溶性硫黄および高分散性硫黄が挙げられる。粉末硫黄が好ましく、ベルト用部材等の硫黄量が多いタイヤ部材の場合には不溶性硫黄が好ましい。かかる硫黄成分は、S−(3−アミノプロピル)チオ硫酸、その金属塩および後述の加硫促進剤は含まない。硫黄成分の使用量は、ゴム成分100重量部に対して、0.3~5重量部であることが好ましく、0.5~3重量部であることがより好ましい。
<酸化亜鉛および加硫促進剤>
 S−(3−アミノプロピル)チオ硫酸および/またはその金属塩とゴム成分と充填剤と硫黄成分以外に、酸化亜鉛や加硫促進剤を、加硫ゴムに配合し、混練することが好ましい。酸化亜鉛の使用量は、ゴム成分100重量部に対して、1~15重量部であることが好ましく、3~8重量部であることがより好ましい。
 加硫促進剤としては、ゴム工業便覧<第四版>(平成6年1月20日社団法人 日本ゴム協会発行)第412~413頁に記載されているチアゾール系加硫促進剤、スルフェンアミド系加硫促進剤およびグアニジン系加硫促進剤が挙げられる。
 具体的には、N−シクロヘキシル−2−ベンゾチアゾリルスルフェンアミド(CBS)、N−tert−ブチル−2−ベンゾチアゾリルスルフェンアミド(BBS)、N,N−ジシクロヘキシル−2−ベンゾチアゾリルスルフェンアミド(DCBS)、2−メルカプトベンゾチアゾール(MBT)、ジベンゾチアジルジスルフィド(MBTS)およびジフェニルグアニジン(DPG)が挙げられる。また、公知の加硫剤であるモルフォリンジスルフィドを用いることもできる。充填剤としてカーボンブラックを用いる場合には、N−シクロヘキシル−2−ベンゾチアゾリルスルフェンアミド(CBS)、N−tert−ブチル−2−ベンゾチアゾリルスルフェンアミド(BBS)、N,N−ジシクロヘキシル−2−ベンゾチアゾリルスルフェンアミド(DCBS)およびジベンゾチアジルジスルフィド(MBTS)のいずれかとジフェニルグアニジン(DPG)との併用が好ましく、充填剤としてシリカとカーボンブラックとを併用する場合には、N−シクロヘキシル−2−ベンゾチアゾリルスルフェンアミド(CBS)、N−tert−ブチル−2−ベンゾチアゾリルスルフェンアミド(BBS)、N,N−ジシクロヘキシル−2−ベンゾチアゾリルスルフェンアミド(DCBS)およびジベンゾチアジルジスルフィド(MBTS)のいずれかとジフェニルグアニジン(DPG)との併用が好ましい。かかる加硫促進剤は、S−(3−アミノプロピル)チオ硫酸およびその金属塩を含まない。
 硫黄と加硫促進剤との比率は制限されないが、加硫促進剤に対する硫黄の重量比(硫黄/加硫促進剤)が、2/1~1/2の範囲であることが好ましい。また、天然ゴムを主成分として含むゴム部材の耐熱性を向上させる方法である、硫黄/加硫促進剤の重量比を1以下にするEV加硫は、耐熱性向上が特に必要な用途においては、本発明でも好ましく用いられる。
<加硫ゴムの製造>
 一般に、加硫ゴムを製造する場合、その製造は基本的に3つの工程で行われる。すなわち、ゴム成分、充填剤、および必要に応じて酸化亜鉛を比較的高温で配合し、混練する第1の工程、第1の工程で得られた混練物に、硫黄成分および必要に応じて加硫促進剤等を比較的低温で配合し、混練する第2の工程、および、比較的高温で、第2の工程で得られた混練物の加硫処理を行う第3の工程により、加硫ゴムを得る。
 第1の工程は、好ましくは200℃以下で行われ、より好ましくは120~180℃で行われる。第2の工程は、好ましくは60~120℃で行われる。
 S−(3−アミノプロピル)チオ硫酸および/またはその金属塩は、第2の工程で用いてもよいが、充填剤や酸化亜鉛とともに、第1の工程で用いることが好ましい。S−(3−アミノプロピル)チオ硫酸および/またはその金属塩を第1の工程で用いる場合、第1の工程は80~200℃の範囲で行うことが好ましく、110~180℃の範囲で行うことがより好ましい。S−(3−アミノプロピル)チオ硫酸および/またはその金属塩を第2の工程で用いる場合、第2の工程は50~100℃の範囲で行うことが好ましい。
 S−(3−アミノプロピル)チオ硫酸および/またはその金属塩は、予め担持剤と配合しておくことも可能である。かかる担持剤としては先に例示した充填剤および日本ゴム協会編「ゴム工業便覧<第四版>」第510~513頁に記載されている「無機充てん剤、補強剤」が挙げられ、なかでも、カーボンブラック、シリカ、焼成クレイおよび水酸化アルミニウムが好ましい。かかる担持剤の使用量は限定されないが、S−(3−アミノプロピル)チオ硫酸および/またはその金属塩100重量部に対して、10~1000重量部の範囲が好ましい。
 ゴム分野において従来用いられている粘弾性特性を改善させる剤を配合し混錬することも可能である。かかる剤としては、N,N’−ビス(2−メチル−2−ニトロプロピル)−1,6−ヘキサンジアミン(住友化学社製「スミファイン(登録商標)1162」)、特開昭63−23942号公報記載のジチオウラシル化合物、特開昭60−82406号公報記載の5−ニトロソ−8−ヒドロキシキノリン(NQ−58)等のニトロソキノリン化合物、田岡化学製「タッキロール(登録商標)AP、V−200」、ペンウォールト社製「バルタック2、3、4、5、7、710」等の特開2009−138148号公報記載のアルキルフェノール・塩化硫黄縮合物、ビス(3−トリエトキシシリルプロピル)テトラスルフィド(デグッサ社製「Si−69」)、ビス(3−トリエトキシシリルプロピル)ジスルフィド(デグッサ社製「Si−75」)、ビス(3−ジエトキシメチルシリルプロピル)テトラスルフィド、ビス(3−ジエトキシメチルシリルプロピル)ジスルフィド、オクタンチオ酸S−[3−(トリエトキシシリル)プロピル]エステル、オクタンチオ酸S−[3−{(2−メチル−1,3−プロパンジアルコキシ)エトキシシリル}プロピル]エステルおよびオクタンチオ酸S−[3−{(2−メチル−1,3−プロパンジアルコキシ)メチルシリル}プロピル]エステルフェニルトリエトキシシラン、メチルトリメトキシシラン、メチルトリエトキシシラン、メチルトリアセトキシシラン、メチルトリブトキシシラン、エチルトリメトキシシラン、エチルトリエトキシシラン、イソブチルトリメトキシシラン、イソブチルトリエトキシシラン、n−オクチルトリメトキシシラン、n−オクチルトリエトキシシラン、ビニルトリメトキシシラン、ビニルトリエトキシシラン、ビニルトリ(メトキシエトキシ)シラン、フェニルトリメトキシシラン、フェニルトリエトキシシラン、フェニルトリアセトキシシラン、3−メタクリロキシプロピルトリメトキシシラン、3−メタクリロキシプロピルトリエトキシシラン、3−アミノプロピルトリメトキシシラン、3−アミノプロピルトリエトキシシラン、N−(2−アミノエチル)−3−アミノプロピルトリメトキシシラン、N−(2−アミノエチル)−3−アミノプロピルトリエトキシシラン、(3−グリシドキシプロピル)トリメトキシシラン、(3−グリシドキシプロピル)トリエトキシシラン、2−(3,4−エポキシシクロヘキシル)エチルトリメトキシシラン、2−(3,4−エポキシシクロヘキシル)エチルトリエトキシシラン、3−イソシアナートプロピルトリメトキシシラン、3−イソシアナートプロピルトリエトキシシラン等のシランカップリング剤、1,6−ビス(N,N’−ジベンジルチオカルバモイルジチオ)ヘキサン(バイエル社製「KA9188」)、1,6−ヘキサメチレンジチオサルフェート2ナトリウム塩2水和物、1,3−ビスシトラコンイミドメチルベンゼン(フレキシス社製「パーカリンク900」)、1−ベンゾイル−2−フェニルヒドラジド、1−または3−ヒドロキシ−N’−(1−メチルエチリデン)−2−ナフトエ酸ヒドラジド、特開2004−91505号公報記載の1−又は3−ヒドロキシ−N’−(1−メチルプロピリデン)−2−ナフトエン酸ヒドラジド、1−又は3−ヒドロキシ−N’−(1,3−ジメチルブチリデン)−2−ナフトエ酸ヒドラジドおよび1−または3−ヒドロキシ−N’−(2−フリルメチレン)−2−ナフトエ酸ヒドラジド等のカルボン酸ヒドラジド誘導体、特開2000−190704号公報記載の3−ヒドロキシ−N’−(1,3−ジメチルブチリデン)−2−ナフトエ酸ヒドラジド、3−ヒドロキシ−N’−(1,3−ジフェニルエチリデン)−2−ナフトエ酸ヒドラジドおよび3−ヒドロキシ−N’−(1−メチルエチリデン)−2−ナフトエ酸ヒドラジド、特開2006−328310号公報記載のビスメルカプトオキサジアゾール化合物、特開2009−40898号公報記載のピリチオン塩化合物、特開2006−249361号公報記載の水酸化コバルト化合物が挙げられる。
 なかでも、N,N’−ビス(2−メチル−2−ニトロプロピル)−1,6−ヘキサンジアミン(住友化学社製「スミファイン(登録商標)1162」)、5−ニトロソ−8−ヒドロキシキノリン(NQ−58)、ビス(3−トリエトキシシリルプロピル)テトラスルフィド(デグッサ社製「Si−69」)、ビス(3−トリエトキシシリルプロピル)ジスルフィド(デグッサ社製「Si−75」)、1,6−ビス(N,N’−ジベンジルチオカルバモイルジチオ)−ヘキサン(バイエル社製「KA9188」)、ヘキサメチレンビスチオサルフェート2ナトリウム塩2水和物、1,3−ビスシトラコンイミドメチルベンゼン(フレキシス社製「パーカリンク900」)、田岡化学製「タッキロール(登録商標)AP、V−200」等のアルキルフェノール・塩化硫黄縮合物が好ましい。これら粘弾性特性を改善させる剤の使用量は、ゴム成分100重量部に対して、0.1~10重量部であることが好ましい。
 酸化亜鉛は、第1の工程で配合することが好ましく、加硫促進剤は第2の工程で配合することが好ましい。
 ゴム分野で従来から用いられている各種の配合剤を配合し、混練することも可能である。かかる配合剤としては、老化防止剤;オイル;ステアリン酸等の脂肪酸類;日鉄化学(株)のクマロン樹脂NG4(軟化点81~100℃)、神戸油化学工業(株)のプロセスレジンAC5(軟化点75℃)等のクマロン・インデン樹脂;テルペン樹脂、テルペン・フェノール樹脂、芳香族変性テルペン樹脂等のテルペン系樹脂;三菱瓦斯化学(株)「ニカノール(登録商標)A70」(軟化点70~90℃)等のロジン誘導体;水素添加ロジン誘導体;ノボラック型アルキルフェノール系樹脂;レゾール型アルキルフェノール系樹脂;C5系石油樹脂;液状ポリブタジエン;が挙げられる。これら配合剤は、第1の工程で配合してもよいし、第2の工程で配合してもよい。
 上記のオイルとしては、プロセスオイル、植物油脂が挙げられる。プロセスオイルとしては、パラフィン系プロセスオイル、ナフテン系プロセスオイル、芳香族系プロセスオイルが挙げられる。
 上記の老化防止剤としては、日本ゴム協会編「ゴム工業便覧<第四版>」第436~443頁に記載されるものが挙げられる。なかでも、N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン(6PPD)、アニリンとアセトンの反応生成物(TMDQ)、ポリ(2,2,4−トリメチル−1,2−)ジヒドロキノリン)(松原産業社製「アンチオキシダントFR」)、合成ワックス(パラフィンワックス等)、植物性ワックスが好ましく用いられる。
 ゴム分野で従来から用いられているモルフォリンジスルフィド等の加硫剤を配合し、混練することも可能である。これらは第2の工程で配合することが好ましい。
 また、しゃく解剤やリターダーを配合し、混練してもよく、さらには、一般の各種ゴム薬品や軟化剤等を必要に応じて配合し、混練してもよい。
 リターダーとしては、無水フタル酸、安息香酸、サリチル酸、N−ニトロソジフェニルアミン、N−(シクロヘキシルチオ)−フタルイミド(CTP)、スルホンアミド誘導体、ジフェニルウレア、ビス(トリデシル)ペンタエリスリトール−ジホスファイトが挙げられ、N−(シクロヘキシルチオ)−フタルイミド(CTP)が好ましい。
 リターダーは、第1の工程で配合し、混錬してもよいが、第2の工程で配合し、混錬することが好ましい。リターダーの使用量は限定されないが、ゴム成分100重量部に対して、0.01~1重量部の範囲が好ましく、0.05~0.5重量部の範囲がより好ましい。
 次に、第2の工程で得られた混練物を加硫処理する第3の工程について説明する。
 加硫処理は、120~180℃で行われることが好ましい。加硫処理は、通常、常圧または加圧下で行われる。
 本発明の使用は、通常、第2の工程で得られた混練物を第3の工程での加硫処理に供する前に、該混練物を特定の状態に加工する工程を含む。
 ここで、該混練物を「特定の状態に加工する工程」とは、タイヤの分野においては、該混練物を、「スチールコードに被覆する工程」「カーカス繊維コードに被覆する工程」「トレッド用部材の形状に加工する工程」等が挙げられる。また、これらの工程によりそれぞれ得られるベルト、カーカス、インナーライナー、サイドウォール、トレッド(キャップトレッドまたはアンダートレッド)等の各部材は、通常、その他の部材とともに、タイヤの分野で通常行われる方法により、さらにタイヤの形状に成型される工程、すなわち該混練物をタイヤに組み込む工程を経て、該混練物を含む生タイヤの状態で第3の工程での加硫処理に供される。かかる加硫処理は、通常、加圧下で行われる。
 トラック、バス、ライトトラック、建設用車両等の大型タイヤに適したトレッド部材に好適なゴム配合におけるゴム成分としては、天然ゴム単独または天然ゴムを主成分とする、SBRおよび/またはBRと天然ゴムとのブレンドが好ましい。また、充填剤としては、カーボンブラック単独またはシリカを主成分とするシリカとカーボンブラックとのブレンドが好ましく用いられる。さらに、N,N’−ビス(2−メチル−2−ニトロプロピル)−1,6−ヘキサンジアミン(住友化学社製「スミファイン(登録商標)1162」)、5−ニトロソ−8−ヒドロキシキノリン(NQ−58)、ビス(3−トリエトキシシリルプロピル)テトラスルフィド(Si−69)、ビス(3−トリエトキシシリルプロピル)ジスルフィド(Si−75)、1,6−ビス(N,N’−ジベンジルチオカルバモイルジチオ)−ヘキサン(バイエル社製「KA9188」)、ヘキサメチレンビスチオサルフェート2ナトリウム塩2水和物、1,3−ビスシトラコンイミドメチルベンゼン(フレキシス社製「パーカリンク900」)、田岡化学製「タッキロール(登録商標)AP、V−200」等のアルキルフェノール・塩化硫黄縮合物、等の粘弾性改良剤を併用することが好ましい。
 乗用車用タイヤに適したトレッド部材に好適なゴム配合におけるゴム成分としては、ケイ素化合物で分子末端を変性した溶液重合SBR単独、または、前記末端変性の溶液重合SBRを主成分とする、非変性の溶液重合SBR、乳化重合SBR、天然ゴムおよびBRからなる群から選ばれる少なくとも1種のゴムと前記末端変性の溶液重合SBRとのブレンドが好ましい。また、充填剤としては、シリカを主成分とするシリカとカーボンブラックとのブレンドが好ましく用いられる。さらに、N,N’−ビス(2−メチル−2−ニトロプロピル)−1,6−ヘキサンジアミン(住友化学社製「スミファイン(登録商標)1162」)、5−ニトロソ−8−ヒドロキシキノリン(NQ−58)、ビス(3−トリエトキシシリルプロピル)テトラスルフィド(Si−69)、ビス(3−トリエトキシシリルプロピル)ジスルフィド(Si−75)、1,6−ビス(N,N’−ジベンジルチオカルバモイルジチオ)−ヘキサン(バイエル社製「KA9188」)、ヘキサメチレンビスチオサルフェート2ナトリウム塩2水和物、1,3−ビスシトラコンイミドメチルベンゼン(フレキシス社製「パーカリンク900」)、田岡化学製「タッキロール(登録商標)AP、V−200」等のアルキルフェノール・塩化硫黄縮合物、等の粘弾性改良剤を併用することが好ましい。
 サイドウォール部材に好適なゴム配合におけるゴム成分としては、BRを主成分とする、非変性の溶液重合SBR、乳化重合SBRおよび天然ゴムからなる群から選ばれる少なくとも1種のゴムとBRとのブレンドが好ましい。また、充填剤としては、カーボンブラック単独またはカーボンブラックを主成分とするシリカとカーボンブラックとのブレンドが好ましく用いられる。さらに、N,N’−ビス(2−メチル−2−ニトロプロピル)−1,6−ヘキサンジアミン(住友化学社製「スミファイン(登録商標)1162」)、5−ニトロソ−8−ヒドロキシキノリン(NQ−58)、ビス(3−トリエトキシシリルプロピル)テトラスルフィド(Si−69)、ビス(3−トリエトキシシリルプロピル)ジスルフィド(Si−75)、1,6−ビス(N,N’−ジベンジルチオカルバモイルジチオ)−ヘキサン(バイエル社製「KA9188」)、ヘキサメチレンビスチオサルフェート2ナトリウム塩2水和物、1,3−ビスシトラコンイミドメチルベンゼン(フレキシス社製「パーカリンク900」)、田岡化学製「タッキロール(登録商標)AP、V−200」等のアルキルフェノール・塩化硫黄縮合物、等の粘弾性改良剤を併用することが好ましい。
 カーカス、ベルト部材に好適なゴム配合におけるゴム成分としては、天然ゴム単独、または、天然ゴムを主成分とするBRと天然ゴムとのブレンドが好ましい。また、充填剤としては、カーボンブラック単独、または、カーボンブラックを主成分とするシリカとカーボンブラックとのブレンドが好ましく用いられる。さらに、N,N’−ビス(2−メチル−2−ニトロプロピル)−1,6−ヘキサンジアミン(住友化学社製「スミファイン(登録商標)1162」)、5−ニトロソ−8−ヒドロキシキノリン(NQ−58)、ビス(3−トリエトキシシリルプロピル)テトラスルフィド(Si−69)、ビス(3−トリエトキシシリルプロピル)ジスルフィド(Si−75)、1,6−ビス(N,N’−ジベンジルチオカルバモイルジチオ)−ヘキサン(バイエル社製「KA9188」)、ヘキサメチレンビスチオサルフェート2ナトリウム塩2水和物、1,3−ビスシトラコンイミドメチルベンゼン(フレキシス社製「パーカリンク900」)、田岡化学製「タッキロール(登録商標)AP、V−200」等のアルキルフェノール・塩化硫黄縮合物、等の粘弾性改良剤を併用することが好ましい。
 かくして得られる加硫ゴムを用いて、通常の方法によって空気入りタイヤが製造される。すなわち、上記加硫処理前の段階のゴム組成物をトレッド用部材に押出し加工し、タイヤ成形機上で通常の方法により貼り付け成形し、生タイヤが成形され、この生タイヤを加硫機中で加熱加圧することにより、タイヤが得られる。
 このようにして得られるタイヤが装着された自動車の燃費は向上し、低燃費化が達成できる。
 以下、実施例により本発明をさらに詳細に説明するが、本発明はこれら実施例に限定されるものではない。
製造例1<S−(3−アミノプロピル)チオ硫酸のナトリウム塩の製造>
 反応容器内の気体を窒素ガスに置換した。該反応容器に、3−ブロモプロピルアミン臭素酸塩25g(0.11モル)、チオ硫酸ナトリウム・五水和物28.42g(0.11モル)、メタノール125mlおよび水125mlを仕込み、得られた混合物を70℃で4.5時間還流した。反応混合物を放冷し、減圧下でメタノールを除去した。得られた残渣に、水酸化ナトリウム4.56gを加え、得られた混合物を室温で30分間攪拌した。減圧下で溶媒を完全に除去した後、残渣にエタノール200mlを加えて1時間還流した。熱ろ過により副生成物である臭化ナトリウムを除去した。ろ液を減圧下で、結晶が析出するまで濃縮し、その後静置した。結晶をろ過により取り出し、エタノール、次いでヘキサンで洗浄した。得られた結晶を真空乾燥して、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を得た。
H−NMR(270.05MHz,MeOD)δppm:3.1(2H,t,J=6.3Hz),2.8(2H,t,J=6.2Hz),1.9−2.0(2H,m)
 得られたS−(3−アミノプロピル)チオ硫酸のナトリウム塩のメディアン径(50%D)を、島津製作所製SALD−2000J型を用い、レーザー回折法(測定操作は下記のとおり)により測定したところ、メディアン径(50%D)は66.7μmであった。得られたS−(3−アミノプロピル)チオ硫酸のナトリウム塩を粉砕し、そのメディアン径(50%D)が14.6μmであるS−(3−アミノプロピル)チオ硫酸のナトリウム塩を調製した。メディアン径(50%D)が14.6μmであるS−(3−アミノプロピル)チオ硫酸のナトリウム塩を実施例1で使用した。
<測定操作>
 得られたS−(3−アミノプロピル)チオ硫酸のナトリウム塩を下記の分散溶媒(トルエン)と分散剤(10重量%スルホこはく酸ジ−2−エチルヘキシルナトリウム/トルエン溶液)との混合溶液に室温で分散させ、得られた分散液に超音波を照射しながら、該分散液を5分間攪拌して試験液を得た。該試験液を回分セルに移し、1分後に測定した。(屈折率:1.70−0.20i)
 S−(3−アミノプロピル)チオ硫酸のナトリウム塩10.0gを水30mlに溶解させて得られる水溶液のpHは11~12であった。
実施例1
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、天然ゴム(RSS#1)100重量部、HAF(旭カーボン社製、商品名「旭#70」)45重量部、ステアリン酸3重量部、酸化亜鉛5重量部および上記製造例1で得たS−(3−アミノプロピル)チオ硫酸のナトリウム塩1重量部を混練配合し、ゴム組成物を得た。該工程は、各種試剤および充填剤の投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は180~200℃であった。
<第2の工程>
 オープンロール機で60~80℃の温度で、第1の工程で得られたゴム組成物と、加硫促進剤(N−シクロヘキシル−2−ベンゾチアゾールスルフェンアミド)1重量部、硫黄2重量部および老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン:商品名「アンチゲン(登録商標)6C」住友化学株式会社製)1重量部とを混練配合し、ゴム組成物を得た。
<第3の工程>
 第2の工程で得たゴム組成物を145℃で加硫処理を行い、加硫ゴムを得た。
参考例1
 実施例1において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例1と同様にして加硫ゴムを得た。
試験例1
 以下のとおり、得られた加硫ゴムの反発弾性率(レジリエンス)、引張特性および粘弾性特性を測定した。
(1)反発弾性率(レジリエンス)
 得られた加硫ゴムのレジリエンスを、リュプケタイプの試験機を用いて測定した。
(2)引張特性
 得られた加硫ゴムの引張特性を、JIS−K6251に準拠して測定した。
 引張応力(M200)は、ダンベル3号形を用いて測定した。
(3)粘弾性特性
 得られた加硫ゴムの粘弾性特性を、株式会社上島製作所製の粘弾性アナライザを用いて測定した。
 条件:温度−5℃~80℃(昇温速度:2℃/分)
    初期歪10%、動的歪2.5%、周波数10Hz
 参考例1で得た加硫ゴムを対照とした場合、実施例1で得た加硫ゴムは、レジリエンスが11%向上し、引張応力(M200)が21%向上し、粘弾性特性(60℃でのtanδ)が13%低下し、いずれの試験においても、各種物性の改善が確認された。
実施例2
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、天然ゴム(RSS#1)100重量部、HAF(旭カーボン社製、商品名「旭#70」)45重量部、ステアリン酸3重量部、酸化亜鉛5重量部およびS−(3−アミノプロピル)チオ硫酸のナトリウム塩1重量部を混練配合し、ゴム組成物を得た。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃であった。
<第2の工程>
 オープンロール機で60~80℃の温度で、第1の工程で得られたゴム組成物と、加硫促進剤(N−シクロヘキシル−2−ベンゾチアゾールスルフェンアミド(CBS))1重量部、硫黄2重量部および老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン(6PPD):商品名「アンチゲン(登録商標)6C」住友化学株式会社製)1重量部とを混練配合し、混練物を得た。
<第3の工程>
 第2の工程で得た混練物を145℃で加硫処理することにより加硫ゴムを得た。
参考例2
 実施例2において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例2と同様にして加硫ゴムを得た。
試験例2
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例2で得た加硫ゴムを対照とした場合、実施例2で得た加硫ゴムは、レジリエンスが15%向上し、引張応力(M200)が15%向上し、粘弾性特性(60℃でのtanδ)が32%低下し、いずれの試験においても、各種物性の改善が確認された。
実施例3
 実施例2において、天然ゴム(RSS#1)100重量部に代えて、天然ゴム(RSS#1)50重量部とポリブタジエンゴムBR−01(JSR社製)50重量部を用いた以外は、実施例2と同様にして加硫ゴムを得た。
参考例3
 実施例3において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例3と同様にして加硫ゴムを得た。
試験例3
 試験例1と同様に反発弾性率および粘弾性特性を測定したところ、参考例3で得た加硫ゴムを対照とした場合、実施例3で得た加硫ゴムは、レジリエンスが8%向上し、粘弾性特性(60℃でのtanδ)が20%低下し、いずれの試験においても、各種物性の改善が確認された。
実施例4
 実施例2において、天然ゴム(RSS#1)に代えて、スチレン・ブタジエン共重合ゴムSBR#1500(JSR社製)を用いた以外は、実施例2と同様にして加硫ゴムを得た。
参考例4
 実施例4において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例4と同様にして加硫ゴムを得た。
試験例4
 試験例1と同様に反発弾性率および粘弾性特性を測定したところ、参考例4で得た加硫ゴムを対照とした場合、実施例4で得た加硫ゴムは、レジリエンスが2%向上し、粘弾性特性(60℃でのtanδ)が8%低下し、いずれの試験においても各種物性の改善が確認された。
実施例5
 実施例2において、天然ゴム(RSS#1)に代えて、スチレン・ブタジエン共重合ゴムSBR#1723(JSR社製)を用いた以外は、実施例2と同様にして加硫ゴムを得た。
参考例5
 実施例5において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例5と同様にして加硫ゴムを得た。
試験例5
 試験例1と同様に反発弾性率および粘弾性特性を測定したところ、参考例5で得た加硫ゴムを対照とした場合、実施例5で得た加硫ゴムは、レジリエンスが9%向上し、粘弾性特性(60℃でのtanδ)が14%低下し、いずれの試験においても各種物性の改善が確認された。
実施例6
 実施例2において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩の使用量を0.5重量部とした以外は、実施例2と同様にして加硫ゴムを得た。
試験例6
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例2で得た加硫ゴムを対照とした場合、実施例6で得た加硫ゴムは、レジリエンスが9%向上し、引張応力(M200)が8%向上し、粘弾性特性(60℃でのtanδ)が31%低下し、いずれの試験においても各種物性の改善が確認された。
実施例7
 実施例2において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩の使用量を0.4重量部とし、加硫促進剤をN−シクロヘキシル−2−ベンゾチアゾリルスルフェンアミド(CBS)に代えてN,N−ジシクロヘキシル−2−ベンゾチアゾリルスルフェンアミド(DCBS)を用いた以外は、実施例2と同様にして加硫ゴムを得た。
参考例7
 実施例7において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例7と同様にして加硫ゴムを得た。
試験例7
 試験例1と同様に反発弾性率および粘弾性特性を測定したところ、参考例7で得た加硫ゴムを対照とした場合、実施例7で得た加硫ゴムは、レジリエンスが8%向上し、粘弾性特性(60℃でのtanδ)が20%低下し、いずれの試験においても各種物性の改善が確認された。
実施例8
 実施例2において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩の使用量を0.4重量部とした以外は、実施例2と同様にして加硫ゴムを得た。
試験例8
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例2で得た加硫ゴムを対照とした場合、実施例8で得た加硫ゴムは、レジリエンスが7%向上し、引張応力(M200)が2%向上し、粘弾性特性(60℃でのtanδ)が21%低下し、いずれの試験においても各種物性の改善が確認された。
実施例9
 実施例2において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩の使用量を0.7重量部とした以外は、実施例2と同様にして加硫ゴムを得た。
試験例9
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例2で得た加硫ゴムを対照とした場合、実施例9で得た加硫ゴムは、レジリエンスが10%向上し、引張応力(M200)が5%向上し、粘弾性特性(60℃でのtanδ)が29%低下し、いずれの試験においても各種物性の改善が確認された。
実施例10
 実施例2において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩の使用量を1.2重量部とした以外は、実施例2と同様にして加硫ゴムを得た。
試験例10
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例2で得た加硫ゴムを対照とした場合、実施例10で得た加硫ゴムは、レジリエンスが10%向上し、引張応力(M200)が8%向上し、粘弾性特性(60℃でのtanδ)が32%低下し、いずれの試験においても各種物性の改善が確認された。
実施例11
 実施例2において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩の使用量を2重量部とした以外は、実施例2と同様にして加硫ゴムを得た。
試験例11
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例2で得た加硫ゴムを対照とした場合、実施例11で得た加硫ゴムは、レジリエンスが11%向上し、引張応力(M200)が13%向上し、粘弾性特性(60℃でのtanδ)が27%低下し、いずれの試験においても各種物性の改善が確認された。
実施例12
 実施例2において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩の使用量を4重量部とした以外は、実施例2と同様にして加硫ゴムを得た。
試験例12
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例2で得た加硫ゴムを対照とした場合、実施例12で得た加硫ゴムは、レジリエンスが8%向上し、引張応力(M200)が6%向上し、粘弾性特性(60℃でのtanδ)が21%低下し、いずれの試験においても各種物性の改善が確認された。
実施例13
 実施例2において、HAF(旭カーボン社製、商品名「旭#70」)に代えてSAF(旭カーボン社製、商品名「旭#90」)を用いた以外は、実施例2と同様にして加硫ゴムを得た。
参考例13
 実施例13において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例13と同様にして加硫ゴムを得た。
試験例13
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例13で得た加硫ゴムを対照とした場合、実施例13で得た加硫ゴムは、レジリエンスが8%向上し、引張応力(M200)が12%向上し、粘弾性特性(60℃でのtanδ)が20%低下し、いずれの試験においても各種物性の改善が確認された。
実施例14
 実施例2において、HAF(旭カーボン社製、商品名「旭#70」)に代えてISAF−HM(旭カーボン社製、商品名「旭#80」)を用いた以外は、実施例2と同様にして加硫ゴムを得た。
参考例14
 実施例14において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例14と同様にして加硫ゴムを得た。
試験例14
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例14で得た加硫ゴムを対照とした場合、実施例14で得た加硫ゴムは、レジリエンスが8%向上し、引張応力(M200)が6%向上し、粘弾性特性(60℃でのtanδ)が21%低下し、いずれの試験においても各種物性の改善が確認された。
実施例15
 実施例2において、HAF(旭カーボン社製、商品名「旭#70」)に代えてISAF−LS(旭カーボン社製、商品名「SUNBLACK710」)を用いた以外は、実施例2と同様にして加硫ゴムを得た。
参考例15
 実施例15において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例15と同様にして加硫ゴムを得た。
試験例15
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例15で得た加硫ゴムを対照とした場合、実施例15で得た加硫ゴムは、レジリエンスが9%向上し、引張応力(M200)が26%向上し、粘弾性特性(60℃でのtanδ)が20%低下し、いずれの試験においても各種物性の改善が確認された。
実施例16
 実施例2において、HAF(旭カーボン社製、商品名「旭#70」)に代えてHAF−LS(旭カーボン社製、商品名「旭#70L」)を用いた以外は、実施例2と同様にして加硫ゴムを得た。
参考例16
 実施例16において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例16と同様にして加硫ゴムを得た。
試験例16
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例16で得た加硫ゴムを対照とした場合、実施例16で得た加硫ゴムは、レジリエンスが7%向上し、引張応力(M200)が4%向上し、粘弾性特性(60℃でのtanδ)が19%低下し、いずれの試験においても各種物性の改善が確認された。
実施例17
 実施例2において、HAF(旭カーボン社製、商品名「旭#70」)に代えてFEF(旭カーボン社製、商品名「旭#60」)を用いた以外は、実施例2と同様にして加硫ゴムを得た。
参考例17
 実施例17において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例17と同様にして加硫ゴムを得た。
試験例17
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例17で得た加硫ゴムを対照とした場合、実施例17で得た加硫ゴムは、レジリエンスが9%向上し、引張応力(M200)が3%向上し、粘弾性特性(60℃でのtanδ)が22%低下し、いずれの試験においても各種物性の改善が確認された。
実施例18
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、天然ゴム(RSS#1)100重量部、HAF(旭カーボン社製、商品名「旭#70」)45重量部、ステアリン酸3重量部、酸化亜鉛5重量部およびS−(3−アミノプロピル)チオ硫酸のナトリウム塩0.4重量部を混練配合し、ゴム組成物を得た。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃であった。
<第2の工程>
 オープンロール機で60~80℃の温度で、第1の工程により得られたゴム組成物と、加硫促進剤(N−シクロヘキシル−2−ベンゾチアゾールスルフェンアミド(CBS))1重量部、硫黄2重量部および老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン:商品名「アンチゲン(登録商標)6C」住友化学株式会社製)1重量部とN−(シクロヘキシルチオ)−フタルイミド0.1重量部とを混練配合し、ゴム組成物を得た。
<第3の工程>
 第2の工程で得たゴム組成物を145℃で加硫処理を行い、加硫ゴムを得た。
参考例18
 実施例18において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩およびN−(シクロヘキシルチオ)−フタルイミドを用いない以外は、実施例18と同様にして加硫ゴムを得た。
参考例19
 実施例18において、N−(シクロヘキシルチオ)−フタルイミドを用いない以外は、実施例18と同様にして加硫ゴムを得た。
試験例18
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例18で得た加硫ゴムを対照とした場合、実施例18で得た加硫ゴムは、レジリエンスが7%向上し、引張応力(M200)が1%向上し、粘弾性特性(60℃でのtanδ)が23%低下し、いずれの試験においても各種物性の改善が確認された。
 また、株式会社東洋精機製作所製のムーニービスコメーターを用い、JIS−K6200−1に従って加硫ゴムのスコーチタイムを測定した。その結果、参考例19で得た加硫ゴムを対照とした場合、実施例18で得た加硫ゴムは、スコーチタイム(t5)が13%向上し、物性の改善が確認された。
実施例19
 実施例18において、N−(シクロヘキシルチオ)−フタルイミドの使用量を0.2重量部とした以外は、実施例18と同様にして加硫ゴムを得た。
試験例19
 試験例1と同様に反発弾性率、引張特性および粘弾性特性を測定したところ、参考例18で得た加硫ゴムを対照とした場合、実施例19で得た加硫ゴムは、レジリエンスが6%向上し、引張応力(M200)が2%向上し、粘弾性特性(60℃でのtanδ)が28%低下し、いずれの試験においても各種物性の改善が確認された。
 また、株式会社東洋精機製作所製のムーニービスコメーターを用い、JIS−K6200−1に従って加硫ゴムのスコーチタイムを測定した。その結果、参考例19で得た加硫ゴムを対照とした場合、実施例19で得た加硫ゴムは、スコーチタイム(t5)が38%向上し、物性の改善が確認された。
実施例20
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、天然ゴム(RSS#1)100重量部、HAF(旭カーボン社製、商品名「旭#70」)45重量部、ステアリン酸3重量部、酸化亜鉛5重量部、老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン:商品名「アンチゲン(登録商標)6C」住友化学株式会社製)1重量部およびS−(3−アミノプロピル)チオ硫酸のナトリウム塩0.4重量部を混練配合し、ゴム組成物を得た。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃であった。
<第2の工程>
 オープンロール機で60~80℃の温度で、第1の工程で得られたゴム組成物と、加硫促進剤(N−シクロヘキシル−2−ベンゾチアゾールスルフェンアミド(CBS))1重量部および硫黄2重量部とを混練配合し、ゴム組成物を得た。
<第3の工程>
 第2の工程で得たゴム組成物を145℃で加硫処理を行い、加硫ゴムを得た。
参考例20
 実施例20において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例20と同様にして加硫ゴムを得た。
試験例20
 試験例1と同様に、反発弾性率、引張特性および粘弾性特性を測定したところ、参考例20で得た加硫ゴムを対照とした場合、実施例20で得た加硫ゴムは、レジリエンスが6%向上し、引張応力(M200)が3%向上し、粘弾性特性(60℃でのtanδ)が23%低下し、いずれの試験においても各種物性の改善が確認された。
実施例21
 実施例2において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩の使用量を0.4重量部とし、加硫促進剤としてN−シクロヘキシル−2−ベンゾチアゾールスルフェンアミド(CBS)に代えてN−t−ブチル−2−ベンゾチアゾールスルフェンアミド(BBS)を用いた以外は、実施例2と同様にして加硫ゴムを得た。
参考例21
 実施例21において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例21と同様にして加硫ゴムを得た。
試験例21
 試験例1と同様に、反発弾性率および粘弾性特性を測定したところ、参考例21で得た加硫ゴムを対照とした場合、実施例21で得た加硫ゴムは、レジリエンスが7%向上し、粘弾性特性(60℃でのtanδ)が16%低下し、いずれの試験においても各種物性の改善が確認された
実施例22
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、天然ゴム(RSS#1)100重量部、HAF(旭カーボン社製、商品名「旭#70」)45重量部、ステアリン酸3重量部、酸化亜鉛5重量部、芳香族系プロセスオイル(ダイアナプロセスオイルAH−12:出光興産株式会社製)5重量部およびS−(3−アミノプロピル)チオ硫酸のナトリウム塩0.4重量部を混練配合し、ゴム組成物を得た。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃であった。
<第2の工程>
 オープンロール機で60~80℃の温度で、第1の工程で得られたゴム組成物と、加硫促進剤(N−シクロヘキシル−2−ベンゾチアゾールスルフェンアミド(CBS))1重量部、硫黄2重量部および老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン:商品名「アンチゲン(登録商標)6C」住友化学株式会社製)1重量部とを混練配合し、ゴム組成物を得た。
<第3の工程>
 第2の工程で得たゴム組成物を145℃で加硫処理を行い、加硫ゴムを得た。
参考例22
 実施例22において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例22と同様にして加硫ゴムを得た。
試験例22
 試験例1と同様に、反発弾性率、引張特性および粘弾性特性を測定したところ、参考例22で得た加硫ゴムを対照とした場合、実施例22で得た加硫ゴムは、レジリエンスが8%向上し、引張応力(M200)が6%向上し、粘弾性特性(60℃でのtanδ)が19%低下し、いずれの試験においても各種物性の改善が確認された
実施例23
 実施例22において、芳香族系プロセスオイル剤に代えて、ナフテン系プロセスオイル(ダイアナプロセスオイルNM−280:出光興産株式会社製)を用いた以外は、実施例22と同様にして加硫ゴムを得た。
参考例23
 実施例23において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例23と同様にして加硫ゴムを得た。
試験例23
 試験例1と同様に、反発弾性率、引張特性および粘弾性特性を測定したところ、参考例23で得た加硫ゴムを対照とした場合、実施例23で得た加硫ゴムは、レジリエンスが4%向上し、引張応力(M200)が5%向上し、粘弾性特性(60℃でのtanδ)が16%低下し、いずれの試験においても各種物性の改善が確認された
実施例24
 実施例22において、芳香族系プロセスオイルに代えて、パラフィン系プロセスオイル(ダイアナプロセスオイルPW−90:出光興産株式会社製)を用いた以外は、実施例22と同様にして加硫ゴムを得た。
参考例24
 実施例24において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例24と同様にして加硫ゴムを得た。
試験例24
 試験例1と同様に、反発弾性率、引張特性および粘弾性特性を測定したところ、参考例24で得た加硫ゴムを対照とした場合、実施例24で得た加硫ゴムは、レジリエンスが6%向上し、引張応力(M200)が3%向上し、粘弾性特性(60℃でのtanδ)が19%低下し、いずれの試験においても各種物性の改善が確認された
実施例25
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、天然ゴム(RSS#1)100重量部、HAF(旭カーボン社製、商品名「旭#70」)45重量部、ステアリン酸3重量部、酸化亜鉛5重量部およびS−(3−アミノプロピル)チオ硫酸のナトリウム塩0.4重量部を混練配合し、ゴム組成物を得た。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃であった。
<第2の工程>
 オープンロール機で60~80℃の温度で、第1の工程で得られたゴム組成物と、加硫促進剤(N−シクロヘキシル−2−ベンゾチアゾールスルフェンアミド(CBS))1重量部、硫黄2重量部および老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン:商品名「アンチゲン(登録商標)6C」住友化学株式会社製)1重量部とを混練配合し、ゴム組成物を得た。
<第3の工程>
 第2の工程で得たゴム組成物を145℃で加硫処理を行い、加硫ゴムを得た。
参考例25
 実施例25において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例25と同様にして加硫ゴムを得た。
試験例25
 試験例1と同様に、反発弾性率、引張特性および粘弾性特性を測定したところ、参考例25で得た加硫ゴムを対照とした場合、実施例25で得た加硫ゴムは、レジリエンスが6%向上し、引張応力(M200)が3%向上し、粘弾性特性(60℃でのtanδ)が19%低下し、いずれの試験においても各種物性の改善が確認された
実施例26
 実施例25において、第1の工程における混練時のゴム温度を140~160℃にした以外は、実施例25と同様にして加硫ゴムを得た。
参考例26
 実施例26において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例26と同様にして加硫ゴムを得た。
試験例26
 試験例1と同様に、反発弾性率および粘弾性特性を測定したところ、参考例26で得た加硫ゴムを対照とした場合、実施例26で得た加硫ゴムは、レジリエンスが7%向上し、粘弾性特性(60℃でのtanδ)が14%低下し、いずれの試験においても各種物性の改善が確認された。
実施例27
 実施例25において、第1の工程における混練時のゴム温度を120~140℃にした以外は、実施例25と同様にして加硫ゴムを得た。
参考例27
 実施例27において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例27と同様にして加硫ゴムを得た。
試験例27
 試験例1と同様に、反発弾性率、引張特性および粘弾性特性を測定したところ、参考例27で得た加硫ゴムを対照とした場合、実施例27で得た加硫ゴムは、レジリエンスが6%向上し、引張応力(M200)が6%向上し、粘弾性特性(60℃でのtanδ)が23%低下し、いずれの試験においても各種物性の改善が確認された
実施例28
<第1の工程>
 サンプルミル(協立理工株式会社製 SK−M3型)を用い、S−(3−アミノプロピル)チオ硫酸のナトリウム塩とカーボンブラック(東海カーボン社製)とを、重量比40/60(S−(3−アミノプロピル)チオ硫酸のナトリウム塩/カーボンブラック)で混合、攪拌し、混合物を得た。
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、上記で得られた混合物1重量部、天然ゴム(RSS#1)100重量部、HAF(旭カーボン社製、商品名「旭#70」)45重量部、ステアリン酸3重量部および酸化亜鉛5重量部を混練配合し、ゴム組成物を得た。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃であった。
<第2の工程>
 オープンロール機で60~80℃の温度にて、第1の工程で得られたゴム組成物と、加硫促進剤(N−シクロヘキシル−2−ベンゾチアゾールスルフェンアミド(CBS))1重量部、硫黄2重量部および老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン:商品名「アンチゲン(登録商標)6C」住友化学株式会社製)1重量部とを混練配合し、ゴム組成物を得た。
<第3の工程>
 第2の工程で得たゴム組成物を145℃で加硫処理を行い、加硫ゴムを得た。
参考例28
 実施例28において、S−(3−アミノプロピル)チオ硫酸のナトリウム塩を用いない以外は、実施例28と同様にして加硫ゴムを得た。
試験例28
 試験例1と同様に、粘弾性特性を測定したところ、参考例28で得た加硫ゴムを対照とした場合、実施例28で得た加硫ゴムは、粘弾性特性(60℃でのtanδ)が18%低下し、物性の改善が確認された
製造例2<S−(3−アミノプロピル)チオ硫酸の製造>
 反応容器内の気体を窒素ガスに置換した。該反応容器に、S−(3−アミノプロピル)チオ硫酸のナトリウム塩26.0gおよび水45mlを仕込み、さらに、5mol/l塩酸を加えて、溶液のpHを5~6に調整した。減圧下で結晶が析出するまで溶液を濃縮し、その後静置した。結晶をろ過により取り出し、真空乾燥し、S−(3−アミノプロピル)チオ硫酸を得た。
H−NMR(270.05MHz,DO)δppm:3.0−3.1(4H,m),2.0−2.1(2H,m)
実施例29
 実施例1において、上記製造例1で得たS−(3−アミノプロピル)チオ硫酸のナトリウム塩1重量部に代えて、上記製造例2で得たS−(3−アミノプロピル)チオ硫酸0.4重量部を用い、第1の工程における混練時のゴム温度を160~180℃とした以外は、実施例1と同様にして加硫ゴムを得た。
参考例29
 実施例29において、S−(3−アミノプロピル)チオ硫酸を用いない以外は、実施例29と同様にして加硫ゴムを得た。
試験例29
 試験例1と同様に、粘弾性特性を測定したところ、参考例29で得た加硫ゴムを対照とした場合、実施例29で得た加硫ゴムは、レジリエンスが3%向上し、粘弾性特性(60℃でのtanδ)が23%低下し、いずれの試験においても各種物性の改善が確認された。
製造例3<S−(3−アミノプロピル)チオ硫酸とそのナトリウム塩との混合物の製造>
 反応容器内の気体を窒素ガスに置換した。該反応容器に、S−(3−アミノプロピル)チオ硫酸10.0gおよび水30mlを仕込み、さらに、1mol/l水酸化ナトリウム溶液0.6mlを加えて、溶液のpHを7~8に調整した。減圧下で溶液を濃縮し、さらに、真空乾燥して、S−(3−アミノプロピル)チオ硫酸とそのナトリウム塩との混合物を得た。
製造例4<S−(3−アミノプロピル)チオ硫酸とそのナトリウム塩との混合物の製造>
 製造例3において、1mol/l水酸化ナトリウム溶液の使用量を2.9mlとし、得られる溶液のpHを8~9に調整した以外は製造例3と同様にしてS−(3−アミノプロピル)チオ硫酸とそのナトリウム塩との混合物を得た。
製造例5<S−(3−アミノプロピル)チオ硫酸とそのナトリウム塩との混合物の製造>
 製造例3において、1mol/l水酸化ナトリウム溶液の使用量を14.6mlとし、得られる溶液のpHを9~10に調整した以外は製造例3と同様にしてS−(3−アミノプロピル)チオ硫酸とそのナトリウム塩との混合物を得た。
製造例6<S−(3−アミノプロピル)チオ硫酸とそのナトリウム塩との混合物の製造>
 製造例3において、1mol/l水酸化ナトリウム溶液の使用量を43.8mlとし、得られる溶液のpHを10~11に調整した以外は製造例3と同様にしてS−(3−アミノプロピル)チオ硫酸とそのナトリウム塩との混合物を得た。
実施例30~33
 実施例29において、S−(3−アミノプロピル)チオ硫酸に代えて、製造例3~6でそれぞれ得たS−(3−アミノプロピル)チオ硫酸とそのナトリウム塩との混合物を用いた以外は、実施例29と同様にして加硫ゴムを得た。
試験例30~33
 試験例1と同様にレジリエンスおよび粘弾性特性を測定した。参考例29で得た加硫ゴムを対照とした場合のレジリエンスと粘弾性特性(60℃でのtanδ)それぞれの変化率を表1に示す。
Figure JPOXMLDOC01-appb-T000001
 表1において、△は参考例29で得た加硫ゴムと比較してレジリエンスが向上したことを表わし、▲は参考例29で得た加硫ゴムと比較して60℃でのtanδが低下したことを表わす。いずれの試験においても各種物性の改善が確認された。
実施例34~38
 実施例8において、粉砕等により、S−(3−アミノプロピル)チオ硫酸のナトリウムのメディアン径(50%D)が表2に記載のものをそれぞれ調製し、実施例8と同様にして加硫ゴムを得た。
試験例34~38
 試験例1と同様にレジリエンスおよび粘弾性特性を測定した。参考例2で得た加硫ゴムを対照とした場合のレジリエンスと粘弾性特性(60℃でのtanδ)それぞれの変化率を表2に示す。
Figure JPOXMLDOC01-appb-T000002
 表2において、△は参考例2で得た加硫ゴムと比較してレジリエンスが向上したことを表わし、▲は参考例2で得た加硫ゴムと比較して60℃でのtanδが低下したことを表わす。いずれの試験においても各種物性の改善が確認された。
実施例39
 実施例1~38のそれぞれの第2の工程で得た混練物で、黄銅メッキ処理が施されたスチールコードを被覆することにより、ベルトが得られる。得られるベルトを用いて、通常の製造方法に従い、生タイヤを成形し、得られた生タイヤを加硫機中で加熱加圧することにより、加硫タイヤが得られる。
実施例40
 実施例1~38のそれぞれの第2の工程で得た混練物を押し出し加工し、トレッド用部材を得る。得られたトレッド用部材を用いて、通常の製造方法に従い、生タイヤを成形し、得られた生タイヤを加硫機中で加熱加圧することにより、加硫タイヤが得られる。
実施例41
 実施例1~38のそれぞれの第2の工程で得た混練物を押し出し加工して、カーカス形状に応じた形状の混練物を調製し、ポリエステル製のカーカス繊維コードの上下に貼り付けることにより、カーカスが得られる。得られたカーカスを用いて、通常の製造方法に従い、生タイヤを成形し、得られた生タイヤを加硫機中で加熱加圧することにより、加硫タイヤが得られる。
実施例42
 実施例2の第2の工程において、さらにN−(シクロヘキシルチオ)−フタルイミド(CTP)0.2重量部を混錬配合する以外は、実施例2と同様にすることにより、加硫ゴムが得られる。
実施例43
 下記の第1の工程~第3の工程により得られる加硫ゴムは、キャップトレッド用として好適である。
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、スチレン・ブタジエン共重合ゴムSBR#1502(住友化学社製)100重量部、ISAF−HM(旭カーボン社製、商品名「旭#80」)45重量部、ステアリン酸2重量部、酸化亜鉛3重量部、S−(3−アミノプロピル)チオ硫酸のナトリウム塩1重量部、老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン(6PPD):商品名「アンチゲン(登録商標)6C」住友化学株式会社製)1重量部およびワックス(日本精蝋製「OZOACE−0355」)2重量部を混練配合し、ゴム組成物を得る。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃である。
<第2の工程>
 オープンロール機で60~80℃の温度にて、第1の工程により得られたゴム組成物と、加硫促進剤(N−シクロヘキシル−2−ベンゾチアゾールスルフェンアミド(CBS))3重量部および硫黄2重量部とを混練配合し、混練物を得る。
<第3の工程>
 第2の工程で得られる混練物を145℃で加硫処理することにより加硫ゴムが得られる。
実施例44
 下記の第1の工程~第3の工程により得られる加硫ゴムは、アンダートレッド用として好適である。
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、スチレン・ブタジエン共重合ゴムSBR#1502(住友化学社製)100重量部、ISAF−HM(旭カーボン社製、商品名「旭#80」)35重量部、ステアリン酸2重量部、酸化亜鉛3重量部、S−(3−アミノプロピル)チオ硫酸のナトリウム塩1重量部、老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン(6PPD):商品名「アンチゲン(登録商標)6C」住友化学株式会社製)1重量部およびワックス(日本精蝋製「OZOACE−0355」)2重量部を混練配合し、ゴム組成物を得る。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃である。
<第2の工程>
 オープンロール機で60~80℃の温度にて、第1の工程により得られたゴム組成物と、加硫促進剤(N−シクロヘキシル−2−ベンゾチアゾールスルフェンアミド(CBS))2重量部、加硫促進剤ジフェニルグアニジン(DPG)0.5重量部、加硫促進剤ジベンゾチアジルジスルフィド(MBTS)0.8重量部および硫黄1重量部とを混練配合し、混練物を得る。
<第3の工程>
 第2の工程で得た混練物を145℃で加硫処理することにより加硫ゴムが得られる。
実施例45
 下記の第1の工程~第3の工程により得られる加硫ゴムは、ベルト用として好適である。
<第1工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、天然ゴム(RSS#1)100重量部、HAF(旭カーボン社製、商品名「旭#70」)45重量部、ステアリン酸3重量部、酸化亜鉛5重量部、S−(3−アミノプロピル)チオ硫酸のナトリウム塩1重量部、含水シリカ(東ソー・シリカ(株)社製「Nipsil(登録商標)AQ」10重量部、老化防止剤FR(松原産業社製「アンチオキシダントFR」)2重量部、レゾルシン2重量部およびナフテン酸コバルト2重量部を混練配合し、ゴム組成物を得る。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃である。
<第2の工程>
 オープンロール機で60~80℃の温度にて、第1の工程により得られたゴム組成物と、加硫促進剤(N,N−ジシクロヘキシル−2−ベンゾチアゾールスルフェンアミド(DCBS))1重量部、硫黄6重量部およびメトキシ化メチロールメラミン樹脂(住友化学社製「スミカノール507AP」)3重量部とを混練配合し、混練物を得る。
<第3の工程>
 第2の工程で得られる混練物を145℃で加硫処理することにより加硫ゴムが得られる。
実施例46
 下記の第1の工程~第3の工程により得られる加硫ゴムは、インナーライナー用として好適である。
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、ハロゲン化ブチルゴム(エクソンモービル社製「Br−IIR2255」)100重量部、GPF 60重量部、ステアリン酸1重量部、酸化亜鉛3重量部、S−(3−アミノプロピル)チオ硫酸のナトリウム塩1重量部およびパラフィンオイル(出光興産社製「ダイアナプロセスオイル」)10重量部を混練配合し、ゴム組成物を得る。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃である。
<第2の工程>
 オープンロール機で60~80℃の温度にて、第1の工程により得られたゴム組成物と、老化防止剤(アニリンとアセトンの縮合物(TMDQ))1重量部、加硫促進剤ジベンゾチアジルジスルフィド(MBTS)1重量部および硫黄2重量部とを混練配合し、混練物を得る。
<第3の工程>
 第2の工程で得られる混練物を145℃で加硫処理することにより加硫ゴムが得られる。
実施例47
 下記の第1の工程~第3の工程により得られる加硫ゴムは、サイドウォール用として好適である。
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、天然ゴム(RSS#3)40重量部、ポリブタジエンゴム(宇部興産社製「BR150B」)60部、FEF50重量部、ステアリン酸2.5重量部、酸化亜鉛3重量部、S−(3−アミノプロピル)チオ硫酸のナトリウム塩1重量部、老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン(6PPD):商品名「アンチゲン(登録商標)6C」住友化学株式会社製)2重量部、アロマチックオイル(コスモ石油社製「NC−140」)10重量部およびワックス(大内新興化学工業社製の「サンノック(登録商標)ワックス」)2重量部を混練配合し、ゴム組成物を得る。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃である。
<第2の工程>
 オープンロール機で60~80℃の温度にて、第1の工程により得られたゴム組成物と、加硫促進剤N−tert−ブチル−2−ベンゾチアゾリルスルフェンアミド(BBS)0.75重量部および硫黄1.5重量部とを混練配合し、混練物を得る。
<第3の工程>
 第2の工程で得られる混練物を145℃で加硫処理することにより加硫ゴムが得られる。
実施例48
 下記の第1の工程~第3の工程により得られる加硫ゴムは、カーカス用として好適である。
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、天然ゴム(TSR20)70重量部、スチレン・ブタジエン共重合ゴムSBR#1502(住友化学社製)30重量部、N339(三菱化学社製)60重量部、ステアリン酸2重量部、酸化亜鉛5重量部、プロセスオイル(出光興産社製「ダイアナプロセスPS32」)7重量部およびS−(3−アミノプロピル)チオ硫酸のナトリウム塩1重量部を混練配合し、ゴム組成物を得る。該工程は、各種試剤および充填剤投入後5分間、50rpmのミキサーの回転数で混練することにより実施し、その時のゴム温度は160~175℃である。
<第2の工程>
 オープンロール機で60~80℃の温度にて、第1の工程により得られたゴム組成物と、加硫促進剤(N−tert−ブチル−2−ベンゾチアゾリルスルフェンアミド(BBS))1重量部、硫黄3重量部、老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン(6PPD):商品名「アンチゲン(登録商標)6C」住友化学株式会社製)1重量部および老化防止剤(アニリンとアセトンの縮合物(TMDQ))1重量部とを混練配合し、混練物を得る。
<第3の工程>
 第2の工程で得られる混練物を145℃で加硫処理することにより加硫ゴムが得られる。
実施例49
 下記の第1の工程~第3の工程により得られる加硫ゴムは、キャップトレッド用として好適である。
<第1の工程>
 バンバリーミキサー(東洋精機製600mlラボプラストミル)を用いて、スチレン・ブタジエン共重合ゴムSBR#1500(JSR社製)100重量部、シリカ(商品名:「ウルトラシル(登録商標)VN3−G」デグッサ社製)78.4重量部、カーボンブラック(商品名「N−339」三菱化学社製)6.4重量部、シランカップリング剤(ビス(3−トリエトキシシリルプロピル)テトラスルフィド:商品名「Si−69」デグッサ社製)6.4重量部、プロセスオイル(商品名「NC−140」コスモ石油社製)47.6重量部、老化防止剤(N−フェニル−N’−1,3−ジメチルブチル−p−フェニレンジアミン(6PPD):商品名「アンチゲン(登録商標)6C」住友化学株式会社製)1.5重量部、酸化亜鉛2重量部、ステアリン酸2重量部、およびS−(3−アミノプロピル)チオ硫酸のナトリウム塩3重量部を混練配合し、ゴム組成物を得る。該工程は、70℃~120℃の温度範囲で操作され、各種試剤および充填剤投入後5分間、80rpmのミキサーの回転数で混練し、引き続き5分間、100rpmのミキサーの回転数で混練することにより実施する。
<第2の工程>
 オープンロール機で30~80℃の温度にて、第1の工程により得られるゴム組成物と、加硫促進剤(N−シクロヘキシル−2−ベンゾチアゾールスルフェンアミド(CBS))1重量部、加硫促進剤(ジフェニルグアニジン(DPG))1重量部、ワックス(商品名「サンノック(登録商標)N」大内新興化学工業社製)1.5重量部および硫黄1.4重量部とを混練配合し、混練物を得る。
<第3の工程>
 第2の工程で得られる混練物を160℃で加硫処理することにより加硫ゴムが得られる。
実施例50
 実施例49において、スチレン・ブタジエン共重合ゴムSBR#1500(JSR社製)に代えて溶液重合SBR(「アサプレン(登録商標)」旭化成ケミカルズ株式会社製)を用いる以外は実施例49と同様にして加硫ゴムが得られる。この加硫ゴムはキャップトレッドとして好適である。
実施例51
 実施例49において、スチレン・ブタジエン共重合ゴムSBR#1500(JSR社製)に代えてSBR#1712(JSR社製)を用い、プロセスオイルの使用量を21重量部に変更し、酸化亜鉛を第2の工程で配合する以外は実施例49と同様にして加硫ゴムが得られる。この加硫ゴムはキャップトレッドとして好適である。
 本発明によれば、タイヤの製造に用いられる加硫ゴムの粘弾性特性を改善させる方法が提供可能となる。

Claims (6)

  1.  加硫ゴムが有する粘弾性特性を改善させるためのS−(3−アミノプロピル)チオ硫酸および/またはその金属塩の使用。
  2.  S−(3−アミノプロピル)チオ硫酸の金属塩における金属イオンが、リチウムイオン、ナトリウムイオン、カリウムイオン、セシウムイオン、コバルトイオン、銅イオンまたは亜鉛イオンである請求項1に記載の使用。
  3.  S−(3−アミノプロピル)チオ硫酸の金属塩における金属イオンが、リチウムイオン、ナトリウムイオンまたはカリウムイオンである請求項1に記載の使用。
  4.  S−(3−アミノプロピル)チオ硫酸の金属塩が、式(2)
    (HN−(CH−SSO ・Mn+      (2)
    (式中、Mn+は金属イオンを表わし、nはその価数を表わす。)
    で示される3−アミノプロピルチオスルファートである請求項1に記載の使用。
  5.  金属イオンが、リチウムイオン、ナトリウムイオン、カリウムイオン、セシウムイオン、コバルトイオン、銅イオンまたは亜鉛イオンである請求項4に記載の使用。
  6.  金属イオンが、リチウムイオン、ナトリウムイオンまたはカリウムイオンである請求項4に記載の使用。
PCT/JP2010/059588 2009-06-04 2010-06-01 S-(3-アミノプロピル)チオ硫酸またはその金属塩の使用 WO2010140704A1 (ja)