USH1949H1 - Hydrogenated elastomer primed polyolefin film - Google Patents
Hydrogenated elastomer primed polyolefin film Download PDFInfo
- Publication number
- USH1949H1 USH1949H1 US08/595,094 US59509496A USH1949H US H1949 H1 USH1949 H1 US H1949H1 US 59509496 A US59509496 A US 59509496A US H1949 H USH1949 H US H1949H
- Authority
- US
- United States
- Prior art keywords
- block copolymer
- styrene
- process according
- weight percent
- film
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Abandoned
Abstract
Description
TABLE 1 | ||||||||
Materials | A | B | C | D | E | F | G | H |
G16521 | 7 | 7 | 0 | 0 | 0 | 0 | 0 | 0 |
FG19012 | 0 | 0 | 7 | 7 | 0 | 0 | 0 | 0 |
B52-53 | 0 | 0 | 0 | 0 | 7 | 7 | 0 | 0 |
Bayprene4 | 0 | 0 | 0 | 0 | 0 | 0 | 3.5 | 3.5 |
Nipol5 | 0 | 0 | 0 | 0 | 0 | 0 | 3.5 | 3.5 |
Toluene6 | 93 | 0 | 93 | 0 | 93 | 0 | 93 | 0 |
XPS68477 | 0 | 93 | 0 | 93 | 0 | 93 | 0 | 93 |
1KRATON ® R G1652 elastomeric ABA block copolymer; 7,200 MW polymerized styrene end-blocks; mid-block hydrogenated 1-2 addition polymerization butadiene; 28 weight % styrene SEBS | ||||||||
2KRATON ® G1652 maleated to give about 2 weight percent functional component. | ||||||||
3KRATON ® G1652 maleated to give about 5 weight percent functional component. | ||||||||
4Neoprene rubber. | ||||||||
5Neoprene rubber. | ||||||||
6Aromatic solvent. | ||||||||
7Developmental non-aromatic hydrocarbon containing predominantly methylcyclohexane and other aliphatic hydrocarbons. |
TABLE 2 | ||||||
avg1 | ||||||
I.D. | (pli) | solvent | primer | % primer fail4 | ||
A(tsu)2 | 4.36 | TOL | G1652 | 3 | ||
A(tsd)3 | 4.18 | TOL | G1652 | 30 | ||
B(tsu) | 4.34 | XPS | G1652 | |||
B(tsd) | 4.06 | XPS | G1652 | |||
C(tsu) | 5.12 | TOL | FG1901 | 0 | ||
C(tsd) | 5.12 | TOL | FG1901 | 0 | ||
D(tsu) | 4.34 | XPS | FG1901 | 1 | ||
D(tsd) | 4.12 | XPS | FG1901 | 0 | ||
E(tsu) | 4.2 | TOL | B52-5 | 0 | ||
E(tsd) | 4.9 | TOL | B52-5 | |||
F(tsu) | 4.7 | XPS | B52-5 | |||
F(tsd) | 5 | XPS | B52-5 | |||
G(tsu) | 2.04 | TOL | NEOPR | 70 | ||
G(tsd) | 2.28 | TOL | NEOPR | 38 | ||
H5 | XP | NEOPR | ||||
1An average of the five “T” peel Instron readings (pli). A high reading indicates good adhesion of the primer to the biaxially-oriented polypropylene backing, and a low number indicates poor adhesion. The actual reading on the ½-inch wide film was multiplied by 2 to give the number reported. | ||||||
2Indicates treated side up, i.e. this tests the adhesion of the primer to the 30 micron corona discharge-treated surface. | ||||||
3Treated side down; this tests the adhesion of the primer to the side of the biaxially oriented polypropylene film not corona discharge treated. | ||||||
4Against polypropylene film | ||||||
5Could not be run since material would not dissolve in non-aromatic solvent. |
D1107 | 100 | parts | ||
Wingtack ® 95 | 100 | parts | ||
IRGANOX ® 1010 | 1 | part | ||
TABLE 3 | |||||||||
Materials | A | B | C | D | E | F | G8 | ||
G16521 | 7 | 7 | |||||||
FG19012 | 7 | 7 | |||||||
B52-53 | 7 | ||||||||
Bayprene4 | 3.5 | ||||||||
Nipol5 | 3.5 | ||||||||
Toluene6 | 93 | — | 93 | — | 93 | 93 | |||
XPS 68477 | — | 93 | — | 93 | — | — | |||
1KRATON ® R G1652 elastomeric ABA block copolymer; 28% styrene SEBS; mid-block hydrogenated 1-2 addition polymerization butadiene | |||||||||
2KRATON ® G1652 maleated to give about 2 weight percent functional component. | |||||||||
3KRATON ® G1652 maleated to give about 5 weight percent functional component. | |||||||||
4Neoprene rubber. | |||||||||
5Neoprene rubber. | |||||||||
6Aromatic solvent. | |||||||||
7Commercial non-aromatic hydrocarbon containing predominantly methyl-cyclohexane. | |||||||||
8No primer. |
TABLE 4 |
“T” Peel Results |
avg1 | ||||
(pli) | solvent | primer | ||
A (treated, 40 dynes) | 3.9 | TOL | G1652 | ||
A (treated, 56 dynes) | 2.9 | TOL | G1652 | ||
A (not treated) | 4.3 | TOL | G1652 | ||
B (treated, 40 dynes) | 4.1 | XPS | G1652 | ||
B (treated, 56 dynes) | 3.8 | XPS | G1652 | ||
B (not treated) | 5.6 | XPS | G1652 | ||
C (treated, 40 dynes) | 5.8 | TOL | FG1901 | ||
C (treated, 56 dynes) | 5.4 | TOL | FG1901 | ||
C (not treated) | 5.7 | TOL | FG1901 | ||
D (treated, 40 dynes) | 5.4 | XPS | FG1901 | ||
D (treated, 56 dynes) | 5.7 | XPS | FG1901 | ||
D (not treated) | 4.3 | XPS | FG1901 | ||
E (treated, 40 dynes) | 5.5 | TOL | B52-5 | ||
E (treated, 56 dynes) | 5.8 | TOL | B52-5 | ||
E (not treated) | 3.3 | TOL | B52-5 | ||
F (treated, 40 dynes) | 3 | TOL | neopr | ||
F (treated, 56 dynes) | 3 | TOL | neopr | ||
F (not treated) | 2.9 | TOL | neopr | ||
G (treated, 40 dynes) | 5.6 | NA | None | ||
1An average of the five “T” peel Instron readings as in Example 1. A high reading indicates good adhesion of the primer to the biaxially-oriented polypropylene backing chemical and a low number indicates poor adhesion. |
Claims (10)