US20070251924A1 - Method and apparatus for rebuilding gas turbine engines - Google Patents
Method and apparatus for rebuilding gas turbine engines Download PDFInfo
- Publication number
- US20070251924A1 US20070251924A1 US11/608,369 US60836906A US2007251924A1 US 20070251924 A1 US20070251924 A1 US 20070251924A1 US 60836906 A US60836906 A US 60836906A US 2007251924 A1 US2007251924 A1 US 2007251924A1
- Authority
- US
- United States
- Prior art keywords
- swet
- box
- protective gas
- gas
- welding chamber
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Abandoned
Abstract
A method for repairing a component within a SWET box is provided. The method includes providing a SWET box that has a divided interior volume that defines a welding chamber within the interior that is smaller than a total volume of the interior SWET box, positioning a component to be repaired within the welding chamber, introducing protective gas into the SWET box, and controlling the flow of protective gas into the SWET box to facilitate minimizing the consumption of the protective gas within the SWET box.
Description
- This invention relates generally to gas turbine engines, and more specifically to the repair of turbine blades used in gas turbine engines.
- In at least some gas turbine engines, turbine blades used within the engine are cast to an approximate final shape. Portions of the turbine blades, including, but not limited to, a root portion, are then shaped to a final desired form by a shaping technique, such as grinding. The finished turbine blades are assembled into a turbine disk or rotor, such that a “dovetail” formed on each turbine blade engages a complimentarily shaped slot on the turbine disk.
- Known turbine blades may be constructed from a high-temperature, high-strength alloy that is adapted to withstand the temperatures and stresses imposed on the parts of a turbine assembly. Because of the high cost of materials, casting operations, and finishing operations, at least some known turbine blades, after being in service, are refurbished to restore the original aerodynamic contours of portions of the blades. At least some known turbine blade repairs, such as those utilized in restoring blade tips, require building up the surface being repaired with a weld bead, and then grinding the surface back to its original contour.
- One known technique for building up the blade material by welding is known as superalloy welding at elevated temperatures (SWET) in which tungsten inert gas (TIG) welding is combined with a pre-heating box, referred to as a SWET box. More specifically, in one known method, argon gas is supplied to the SWET box to provide a protective atmosphere for the blades being welded. The argon atmosphere facilitates reducing an amount of contamination within the weld and reducing the amount of cracking within the weld. More specifically, during use a sufficient volume of argon is provided to protect the blade and for good weld quality, and it is not unusual that the argon flow to the SWET box is set excessively high just to facilitate protecting the blades during welding. However, this technique not only unnecessarily increases argon consumption and its associated costs, but also the unnecessarily high gas flow increases the noise level in the area of the SWET box.
- In one aspect, a method for repairing a component within a SWET box is provided. The method includes providing a SWET box that has a divided interior volume that defines a welding chamber within the interior that is smaller than a total volume of the interior SWET box, positioning a component to be repaired within the welding chamber, introducing protective gas into the SWET box, and controlling the flow of protective gas into the SWET box to facilitate minimizing the consumption of the protective gas within the SWET box.
- In another aspect, a liner assembly for a SWET box is provided. The liner assembly includes an enclosure configured to be received in a heating chamber of the SWET box. The enclosure includes a rear wall, a front wall opposite the rear wall, a pair of opposed end walls, and a dividing wall defining a welding chamber therein. A gas delivery system is provided for supplying a protective gas into the SWET box and the enclosure. A lid is coupled to the SWET box and extends over the heating chamber and the enclosure, encasing the heating chamber and the enclosure.
- In another aspect, a SWET box is provided that includes a heating chamber and an enclosure configured to be received in the heating chamber. The enclosure includes a rear wall, a front wall opposite the rear wall, a pair of opposed end walls, and a dividing wall defining a welding chamber therein. A gas delivery system is provided for supplying a protective gas into the heating chamber and the enclosure. A lid is coupled to the heating chamber and extends over the heating chamber and the enclosure.
-
FIG. 1 is a schematic cross sectional view of a SWET box; -
FIG. 2 is a schematic cross sectional view of a turbine blade being repaired within the SWET box shown inFIG. 1 . -
FIG. 3 is a schematic cross sectional view of the SWET box shown inFIG. 1 with a liner assembly; -
FIG. 4 is a perspective view of the enclosure of the liner assembly shown inFIG. 3 ; -
FIG. 5 is a perspective view of the SWET box lid shown inFIG. 3 ; -
FIG. 6 is a perspective view of the first gas delivery system shown inFIG. 3 ; -
FIG. 7 is a perspective view of the blade holder shown inFIG. 3 . -
FIG. 1 is a schematic cross sectional view of aconventional SWET box 10 that may be used in superalloy welding at elevated temperatures (SWET). SWETbox 10 includes aheating chamber 12 that has aback wall 14, an opposed front wall (not shown), and opposedends box 10 also includes afloor 20 and aremovable lid 22. Though shown as being substantially rectangular in shape inFIG. 1 ,SWET box 10 may be non-rectangular. For example, in one embodiment, one or bothends SWET box 10 has an elliptical cross-sectional profile when viewed from the top along sight line A-A. Aheat source 26 is mounted inback wall 14. Typically, in SWET welding,heat source 26 includes one or more quartz lamps, however, other known heating methods may be used.Fluid inlets 28 are provided infloor 20 for introducing protective to create a protective atmosphere insideSWET box 10. -
FIG. 2 is a schematic view of a turbine blade being repaired inSWET box 10. Blade 30 includes adove tail 32 and anairfoil 34 that extends radially outward fromdove tail 32 to anairfoil tip 36 that is being repaired.Blade 30 is retained in afixture 40 that is positioned on aplatform 42 at the bottom ofheating chamber 12.Platform 42 rests onSWET box floor 20 such thatfluid inlets 28 remain un-obstructed. During use,blade 30 is heated byheat source 26, and a protective gas, such as argon, is supplied toSWET box 10 throughfluid inlets 28. A weld repair is made to blade 30 in the presence of the protective gas. - As used herein, the terms “repair” and “repairing”, may include any repair/inspection process. For example, repair processes may include various known repair techniques including welding, grinding, and/or machining. The above examples are intended as exemplary only, and thus are not intended to limit in any way the definition and/or meaning of the terms “repair” and repairing”. In addition, as used herein the term “component” may include any object to which a repair process is applied. Furthermore, although the invention is described herein in association with a gas turbine engine, and more specifically for use with a turbine blade for a gas turbine engine, it should be understood that the present invention may be applicable to any component and/or any repair process. Accordingly, practice of the present invention is not limited to the repair of turbine blades or other components of gas turbine engines.
- During SWET welding,
SWET box 10 is filled with the protective gas to facilitate enhancing the quality of the weld while minimizing contamination and cracks within the weld. More specifically, to ensure the entire volume ofSWET box 10 is filled with protective gas during welding, and increased gas flow rate is used to ensure that the volume of gas is maintained. The higher gas flow rate creates a higher noise level in the vicinity ofSWET box 10. -
FIG. 3 is a schematic cross sectional view ofSWET box 10 including aliner assembly 50 for reducing the amount of protective gas supplied toSWET box 10 and the amount of noise generated in the vicinity ofSWET box 10.Assembly 50 includes anenclosure 52 and alid 54. A firstgas delivery system 56 is positioned adjacent afloor 58 ofenclosure 52, and a secondgas delivery system 60 is coupled throughlid 54. Ablade holder 62 is positioned above firstgas delivery system 56, and a layer of ametallic mesh material 66 is packed around firstgas delivery system 56 to facilitate diffusing and reducing noise generated as the flow of protective gas entersSWET box 10. In the example embodiment,metallic mesh 66 is a steel, wool-like structure, and may be fabricated from any metallic material capable of withstanding the fabricating temperatures which develop during welding withinSWET box 10. In the embodiment, the temperature withinSWET box 10 may reach at least about 900 degrees Celsius. -
FIG. 4 is a perspective view ofenclosure 52. In the exemplary embodiment,enclosure 52 is fabricated from a metallic material, such as steel, and includes aback wall 68, afront wall 70, afirst end wall 72, and an arcuate or curvedsecond end wall 74.First end wall 72 includes acutout 75 at an upper portion thereof, andback wall 68 includes awindow 76 extending there through and in open communication with a heat source 26 (seeFIG. 1 ) inback wall 14 ofSWET box 10. A dividingwall 78separates enclosure 52 into awelding chamber 80 and acavity 82 that is partially bounded bycurved end wall 74.Cutout 75 andcurved end wall 74 provide an operator access to manipulate a component being repaired in weldingchamber 80. Afloor 58 inwelding chamber 80 includes ahole 84 extending there through to enable the admission of a protective gas into weldingchamber 80. -
FIG. 5 is a perspective view oflid 54.Lid 54 extends over heating chamber 12 (shown inFIG. 1 ) andliner assembly 50. Secondgas delivery system 60 is coupled tolid 54 and includes aninlet tube 86, adistribution tube 88, a plurality of diffuser cups 90, and acoupling 92. When in use,inlet tube 86 is connected to a gas source (not shown) and delivers gas todistribution tube 88 viacoupling 92. Diffuser cups 90 extend downward fromlid 54 intoheating chamber 12 andliner assembly 50 to discharge the gas into an upper portion 93 (seeFIG. 3 ) ofSWET box 10. More specifically, diffuser cups 90 slow the flow of protective gas and thereby facilitate controlling the flow of gas intoSWET box 10 and facilitate reducing an amount of noise generated as the gas entersSWET box 10. When threediffuser cups 90 are used, as shown inFIG. 5 ,lid 54 is positioned onSWET box 10 such that onediffuser cup 90 extends intowelding chamber 80 and the two remaining diffuser cups 90 extend betweencurved end wall 74 and SWETbox end wall 18. In alternative embodiments more or less than three diffuser sups 90 may be utilized. -
FIG. 6 is a partial perspective view offirst delivery system 56.First distribution system 56 includes an array ofperforated tubes 94, each of which is connected to, and fed from, acommon end line 96. In use,perforated tubes 94 provide a diffuser effect that facilitates reducing the flow of gas throughperforated tubes 94 and intoSWET box 10. Moreover, supplying the protective gas throughperforated tubes 94 also facilitates reducing an amount of noise generated inSWET box 10 in comparison to the unfettered flow through fluid inlets 28 (seeFIGS. 1 and 2 ). -
FIG. 7 is a perspective view ofblade holder 62.Blade holder 62 includes aperforated base 100, astand 102 that extends upwardly frombase 100, and achannel 104 coupled to anupper end 106 ofstand 102.Channel 104 is sized to hold a component part such as a turbine blade oriented in a position to facilitate the performance of a repair operation on the component part. - In operation, and with reference to
FIG. 3 ,liner assembly 50 is placed inside theheating chamber 12 ofSWET box 10.Liner assembly 50 is positioned such thatwindow 76 ofenclosure 52 is in open communication withheat source 26 inback wall 14 ofSWET box 10. Withenclosure 52 positioned withinSWET box 10, the interior volume ofSWET box 10 is divided to form weldingchamber 80 withinenclosure 52 that is smaller than the total volume ofSWET box 10. - First
gas delivery system 56 is placed on the bottom 58 ofwelding chamber 80. Suitable plumbing is provided to connect firstgas delivery system 56 tofluid inlet 28 which is connected to a protective gas source (not shown). Firstgas delivery system 56 includes an array ofperforated tubes 94 that diffuse the protective gas and facilitate introducing the protective gas at a reduced a lower noise level in comparison to open flow throughfluid inlet 28.Metallic mesh material 66 is packed aroundperforated tubes 94 to further facilitate diffusing the protective gas and reducing the noise level. A component part to be repaired, such asturbine blade 30, is placed inchannel 104 ofblade holder 62.Blade holder 62 is then positioned in weldingchamber 80 withperforated base 100 ofblade holder 62 resting onmesh material 66 andperforated tubes 94. -
Lid 54 is positioned onSWET box 10 such that one ofdiffusers 90 extends downwardly intowelding chamber 80 and the remaining twodiffusers 90 extend downwardly into a space betweencurved end wall 74 andend wall 18 ofSWET box 10.Inlet tube 86 onlid 54 is then connected using suitable plumbing to a source of protective gas (not shown). - After positioning
blade 30 inSWET box 10, the protective gas is supplied andheat source 26 is activated to provide heat toheating chamber 12. In the case of turbine blade repair, argon is typically the protective gas. It is to be understood, however, thatSWET box 10 can be used with components from applications other than gas turbine engines, in which case different materials may be involved and other inert may also be used. - Protective gas is introduced into
SWET box 10 from anupper portion 93 through diffuser cups 90 onlid 54. Introduction of the protective gas through diffuser cups 90 facilitates controlling the flow of the protective gas. Protective gas is also introduced from alower portion 95 ofSWET box 10 throughperforated tubes 94 inwelding chamber 80 which concentrates the protective gas flow in weldingchamber 80.Perforated tubes 94 diffuse the protective gas and also facilitate reducing a noise level of the gas flow. Introducing the protective gas through diffuser cups 90 andperforated tubes 94, along with concentrating the gas flow in weldingchamber 80 combine to reduce the consumption of protective gas. - When a desired temperature is reached inside
SWET box 10, the repair is made. The flow of protective gas is continued during the repair to facilitate maintaining the protective atmosphere. In the case of blade tip repairs onturbine blade 30, weld beads are applied toblade tip 36 to build up the blade material so that the design contour ofblade 30 can be restored.Liner assembly 50 facilitates the production of weld beads without contaminates and without cracks within the weld beads. - The above-described SWET box liner assembly provides a cost effective and highly reliable apparatus that reduces the consumption of protective and reduces the noise level in the work place in comparison to other known SWET boxes. The liner assembly concentrates the protective gas in a reduced volume within the SWET box thereby reducing the amount of gas flow required to maintain a protective atmosphere. The introduction of the protective gas through diffusers contributes to reducing a noise level in the vicinity of the SWET box.
- Exemplary embodiments of a SWET box liner assembly are described above in detail. The liner assemblies are not limited to the specific embodiments described herein, but rather each component may be utilized independently and separately from other components described herein. Each component can also be used in combination with other SWET box systems.
- While the invention has been described in terms of various specific embodiments, those skilled in the art will recognize that the invention can be practiced with modification within the spirit and scope of the claims.
Claims (8)
1. A method for repairing a component within a SWET box, said method comprising:
providing a SWET box having a divided interior volume such that a welding chamber is defined within the interior that is smaller than a total volume of the interior SWET box;
positioning a component to be repaired within the welding chamber;
introducing protective gas into the SWET box; and
controlling the flow of protective gas into the SWET box to facilitate minimizing the consumption of the protective gas within the SWET box.
2. A method in accordance with claim 1 wherein controlling the flow of protective gas into the SWET box further comprises concentrating the flow of protective gas in the welding chamber.
3. A method in accordance with claim 1 wherein dividing the SWET box comprises positioning a compartmentalized insert in the SWET box, the insert including a welding chamber.
4. A method in accordance with claim 1 wherein introducing the protective gas into the SWET box comprises introducing the protective gas from an upper portion of the SWET box.
5. A method in accordance with claim 1 wherein controlling the flow of the protective gas into the SWET box comprises introducing the gas through diffuser cups.
6. A method in accordance with claim 2 wherein concentrating the flow of protective gas in the welding chamber comprises introducing the protective gas from an upper portion of the welding chamber and a lower portion of the welding chamber.
7. A method in accordance with claim 6 wherein introducing the protective gas from the lower portion of the welding chamber comprises introducing the gas through perforated diffusing tubes.
8-20. (canceled)