KR102583105B1 - Clear coat composition - Google Patents
Clear coat composition Download PDFInfo
- Publication number
- KR102583105B1 KR102583105B1 KR1020210057261A KR20210057261A KR102583105B1 KR 102583105 B1 KR102583105 B1 KR 102583105B1 KR 1020210057261 A KR1020210057261 A KR 1020210057261A KR 20210057261 A KR20210057261 A KR 20210057261A KR 102583105 B1 KR102583105 B1 KR 102583105B1
- Authority
- KR
- South Korea
- Prior art keywords
- polyester resin
- weight
- coating film
- above range
- composition
- Prior art date
Abstract
본 발명은 제1 폴리에스터 수지, 제2 폴리에스터 수지, 실리콘 변성 폴리에스터 수지 및 멜라민 수지를 포함하고, 상기 제1 폴리에스터 수지는 수산기가가 200 내지 300 mgKOH/g이고, 유리전이온도가 15 내지 30 ℃이며, 상기 제2 폴리에스터 수지는 수산기가가 80 내지 180 mgKOH/g이고, 유리전이온도가 1 내지 10 ℃인, 클리어 코트 조성물에 관한 것이다.The present invention includes a first polyester resin, a second polyester resin, a silicone-modified polyester resin, and a melamine resin, wherein the first polyester resin has a hydroxyl value of 200 to 300 mgKOH/g and a glass transition temperature of 15. to 30°C, and the second polyester resin has a hydroxyl value of 80 to 180 mgKOH/g and a glass transition temperature of 1 to 10°C.
Description
본 발명은 반응성이 우수하여 핀홀 특성이 개선되어 제조된 도막의 외관 특성이 우수하고 내스크래치성 등의 기계적 물성도 우수한 클리어 코트 조성물에 관한 것이다.The present invention relates to a clear coat composition that has excellent reactivity and improved pinhole properties, so that the manufactured coating film has excellent appearance properties and excellent mechanical properties such as scratch resistance.
자동차의 차체는, 외관 특성을 향상시키고 외부 환경으로부터 표면을 보호하기 위해, 전착 도장, 중도 도장, 베이스 도장 및 클리어 도장 등의 복수 코팅 공정이 수행된다. 구체적으로, 차체에 전착 도료의 도포 및 경화, 중도 도료의 도포 및 경화를 실시한 후, 중도 코팅층 상에 베이스 코트와 클리어 코트를 연속적으로 도장한 후 건조 및 경화시키는 것이 보편적이다. 상술한 바와 같이, 베이스 코트와 클리어 코트는 베이스 코트 조성물의 도포 및 건조 후 클리어 코트 조성물을 도포하고, 140~150 ℃에서 클리어 코트와 베이스 코트를 함께 경화시키는 것이 일반적이다. The car body is subjected to multiple coating processes, such as electrodeposition coating, intermediate coating, base coating, and clear coating, in order to improve the exterior characteristics and protect the surface from the external environment. Specifically, it is common to apply and cure an electrodeposited paint and an intermediate paint on a car body, and then continuously apply a base coat and a clear coat on the intermediate coating layer, followed by drying and curing. As described above, it is common to apply the base coat and clear coat after applying and drying the base coat composition, and then curing the clear coat and base coat together at 140 to 150 ° C.
한편, 종래 클리어 코트 조성물은 폴리에스터 수지, 아크릴 수지, 멜라민 경화제 등을 포함하여 우레탄 경화 시스템 기반으로 한다. 또한, 상술한 바와 같은 종래 클리어 코트 조성물은 제조된 도막의 외관 특성이 우수하고, 내스크래치성이 우수하여 널리 이용되고 있다. 구체적으로, 한국 공개특허 제2014-0125415호(특허문헌 1)에는 히드록실기 함유 폴리에스테르 수지 및 히드록실기와 반응하는 가교제로 멜라민 수지를 포함하는 1액형 도료 조성물을 개시하고 있습니다.Meanwhile, conventional clear coat compositions are based on a urethane curing system including polyester resin, acrylic resin, melamine curing agent, etc. In addition, the conventional clear coat composition as described above is widely used because the produced coating film has excellent appearance characteristics and excellent scratch resistance. Specifically, Korean Patent Publication No. 2014-0125415 (Patent Document 1) discloses a one-component paint composition containing a hydroxyl group-containing polyester resin and a melamine resin as a crosslinking agent that reacts with the hydroxyl group.
그러나, 종래 클리어 코트 조성물은 도장 후 건조 시간이 짧거나, 클리어 코트 건조 후 경화를 위한 오븐까지의 이동 거리가 짧거나, 차체 간 거리가 짧은 경우 제조된 도막의 외관 특성, 특히 핀홀 불량, 광택 불량 등의 문제가 있었다.However, conventional clear coat compositions have a short drying time after painting, a short travel distance to the oven for curing after drying the clear coat, or a short distance between car bodies, resulting in poor appearance characteristics of the manufactured paint film, especially poor pinholes and poor gloss. There was a problem, etc.
따라서, 반응성이 우수하여 도장 후 건조 시간이 짧거나 클리어 코트 건조 후 경화를 위한 오븐까지의 이동 거리가 짧거나, 차체 간 거리가 짧은 경우도 제조된 도막의 외관 특성이 우수하고 내스크래치성 등의 기계적 물성도 우수한 클리어 코트 조성물에 대한 연구개발이 필요한 실정이다.Therefore, even in cases where the drying time after painting is short due to excellent reactivity, the travel distance to the oven for curing after clear coat drying is short, or the distance between car bodies is short, the produced coating film has excellent appearance characteristics and scratch resistance, etc. There is a need for research and development on clear coat compositions with excellent mechanical properties.
본 발명은 반응성이 우수하여 도장 후 건조 시간이 짧거나 클리어 코트 건조 후 경화를 위한 오븐까지의 이동 거리가 짧거나, 차체 간 거리가 짧은 경우도 제조된 도막의 외관 특성이 우수하고 내스크래치성 등의 기계적 물성도 우수한 클리어 코트 조성물을 제공하고자 한다.The present invention has excellent reactivity, so even when the drying time after painting is short, the distance to the oven for curing after drying the clear coat is short, or the distance between car bodies is short, the produced coating film has excellent appearance characteristics, scratch resistance, etc. The aim is to provide a clear coat composition with excellent mechanical properties.
본 발명은 제1 폴리에스터 수지, 제2 폴리에스터 수지, 실리콘 변성 폴리에스터 수지 및 멜라민 수지를 포함하고,The present invention includes a first polyester resin, a second polyester resin, a silicone-modified polyester resin, and a melamine resin,
상기 제1 폴리에스터 수지는 수산기가가 200 내지 300 mgKOH/g이고, 유리전이온도가 15 내지 30 ℃이며,The first polyester resin has a hydroxyl value of 200 to 300 mgKOH/g and a glass transition temperature of 15 to 30 ℃,
상기 제2 폴리에스터 수지는 수산기가가 80 내지 180 mgKOH/g이고, 유리전이온도가 1 내지 10 ℃인, 클리어 코트 조성물을 제공한다.The second polyester resin has a hydroxyl value of 80 to 180 mgKOH/g and a glass transition temperature of 1 to 10° C., providing a clear coat composition.
또한, 본 발명은 상기 클리어 코트 조성물; 및 경화제;를 포함하는, 클리어 도료 키트를 제공한다.In addition, the present invention relates to the clear coat composition; and a hardener. A clear paint kit is provided.
본 발명에 따른 클리어 코트 조성물은 반응성이 우수하여 도장 후 건조 시간이 짧거나 클리어 코트 건조 후 경화를 위한 오븐까지의 이동 거리가 짧거나, 차체 간 거리가 짧은 경우도 제조된 도막의 핀홀이 발생하지 않고 광택 저하가 발생하지 않아 외관 특성이 우수하다. 또한, 상기 클리어 코트 조성물로부터 제조된 도막은 경도, 부착성, 내스크래치성 등의 기계적 물성도 우수하여 차체 도장용으로 유용하게 사용할 수 있다.The clear coat composition according to the present invention has excellent reactivity, so pinholes in the manufactured paint film do not occur even when the drying time after painting is short, the distance to the oven for curing after drying the clear coat is short, or the distance between car bodies is short. The appearance characteristics are excellent as there is no loss of gloss. In addition, the coating film prepared from the clear coat composition has excellent mechanical properties such as hardness, adhesion, and scratch resistance, and can be usefully used for car body painting.
이하, 본 발명을 상세하게 설명한다.Hereinafter, the present invention will be described in detail.
본 명세서에서 사용된 "중량평균분자량"은 당업계에 알려진 통상의 방법에 의해 측정된 것이며, 예를 들어 GPC(gel permeation chromatograph) 방법 등으로 측정할 수 있다. The “weight average molecular weight” used in this specification is measured by a common method known in the art, and can be measured, for example, by a GPC (gel permeation chromatograph) method.
또한, "유리전이온도"는 당업계에 알려진 통상의 방법에 의해 측정된 것이며, 예를 들어 시차주사열량분석법(differential scanning calorimetry, DSC) 등으로 측정할 수 있다. In addition, “glass transition temperature” is measured by a common method known in the art, and can be measured, for example, by differential scanning calorimetry (DSC).
"산가" 및 "수산기가"와 같은 작용기가는 당업계에 잘 알려진 방법에 의해 측정할 수 있으며, 예를 들어 적정(titration) 방법 등으로 측정한 값을 나타낼 수 있다.Functional values such as “acid value” and “hydroxyl value” can be measured by methods well known in the art, and can represent values measured by, for example, titration methods.
클리어 코트 조성물clear coat composition
본 발명에 따른 클리어 코트 조성물은 제1 폴리에스터 수지, 제2 폴리에스터 수지, 실리콘 변성 폴리에스터 수지 및 멜라민 수지를 포함한다. 이때, 제1 폴리에스터 수지는 제2 폴리에스터 수지보다 수산기가(OHv) 및 유리전이온도가 높다. 상기 클리어 코트 조성물이 상술한 바와 같이 유리전이온도 및 수산기가가 상이한 2종의 폴리에스터 수지를 포함함으로써, 조성물의 건조 속도 및 가교 밀도를 조절하여 제조된 도막의 외관 특성 및 경도, 부착성, 내스크래치성 등의 기계적 물성을 향상시키는 효과를 수득할 수 있다.The clear coat composition according to the present invention includes a first polyester resin, a second polyester resin, a silicone-modified polyester resin, and a melamine resin. At this time, the first polyester resin has a higher hydroxyl value (OHv) and glass transition temperature than the second polyester resin. As the clear coat composition contains two types of polyester resins with different glass transition temperatures and hydroxyl values as described above, the appearance characteristics, hardness, adhesion, and resistance of the coating film produced by controlling the drying speed and crosslinking density of the composition The effect of improving mechanical properties such as scratchability can be obtained.
제1 폴리에스터 수지1st polyester resin
제1 폴리에스터 수지는 조성물에 주수지로서, 도막 형성성을 부여하는 역할을 한다.The first polyester resin serves as the main resin in the composition and provides film forming properties.
상기 제1 폴리에스터 수지는 공지된 방법에 따라 직접 합성된 것을 사용하거나, 시판되는 제품을 사용할 수 있다. 예를 들어, 상기 제1 폴리에스터 수지는 제1 카르복실산과 제1 폴리올을 반응시켜 제조할 수 있다. The first polyester resin can be directly synthesized according to a known method, or a commercially available product can be used. For example, the first polyester resin can be produced by reacting a first carboxylic acid and a first polyol.
이때, 상기 제1 카르복실산은 예를 들어, 아디프산(AA), 이소프탈산(IPA), 트리말레트산 무수물(TMA), 지환족산, 프탈산 무수물, 이소프탈산, 테레프탈산, 숙신산, 아디프산, 푸마르산, 말레산 무수물, 테트라하이드로프탈산 무수물(HHPA), 헥사히드로프탈산 무수물 및 이들의 유도체로 이루어진 군으로부터 선택된 1종 이상일 수 있다. At this time, the first carboxylic acid is, for example, adipic acid (AA), isophthalic acid (IPA), trimaltic anhydride (TMA), cycloaliphatic acid, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, It may be one or more selected from the group consisting of fumaric acid, maleic anhydride, tetrahydrophthalic anhydride (HHPA), hexahydrophthalic anhydride, and derivatives thereof.
상기 제1 폴리올은 예를 들어, 메톡시폴리에틸렌 글리콜, 1,6-헥산디올(1,6-HD), 네오펜틸글리콜(NPG), 트리메틸올 프로판(TMP), 에틸렌글리콜, 프로필렌글리콜, 디에틸렌글리콜, 부탄디올 1,4-헥산디올 및 3-메틸펜탄디올로 이루어진 군으로부터 선택된 1종 이상일 수 있다.The first polyol is, for example, methoxypolyethylene glycol, 1,6-hexanediol (1,6-HD), neopentyl glycol (NPG), trimethylol propane (TMP), ethylene glycol, propylene glycol, diethylene. It may be one or more selected from the group consisting of glycol, butanediol, 1,4-hexanediol, and 3-methylpentanediol.
상기 제1 폴리에스터 수지는 산가(Av)가 15 내지 25 mgKOH/g, 또는 18 내지 22 mgKOH/g일 수 있다. 제1 폴리에스터 수지의 산가가 상기 범위 내인 경우, 열처리에 의한 급격한 경화가 방지되어 도막의 외관 불량을 방지하고 기포(popping)가 생기는 것을 줄이는 효과가 있다. 제1 폴리에스터 수지의 산가가 상기 범위 미만인 경우, 경화 반응 속도가 저하되어 제조된 도막의 경도와 외관 특성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 경화 반응 속도가 빨라져서 도막이 브리틀(Brittle)해져 내스크래치성이 저하되고, 친수성이 향상됨에 따라 내수성이 저하되는 문제가 발생할 수 있다.The first polyester resin may have an acid value (Av) of 15 to 25 mgKOH/g, or 18 to 22 mgKOH/g. When the acid value of the first polyester resin is within the above range, rapid hardening due to heat treatment is prevented, which has the effect of preventing poor appearance of the coating film and reducing the occurrence of bubbles (popping). If the acid value of the first polyester resin is less than the above range, the curing reaction speed is lowered, which causes a problem in that the hardness and appearance characteristics of the produced coating film are lowered, and if it exceeds the above range, the curing reaction speed is accelerated and the coating film becomes brittle. ), scratch resistance may decrease, and as hydrophilicity improves, water resistance may decrease.
또한, 상기 제1 폴리에스터 수지는 수산기가(OHv)가 200 내지 300 mgKOH/g, 또는 220 내지 280 mgKOH/g일 수 있다. 제1 폴리에스터 수지의 수산기가가 상기 범위 내인 경우, 도막의 퍼짐성을 향상시키고 우레탄 반응에 의한 내화학성을 향상시키 효과가 있다. 또한, 제1 폴리에스터 수지의 수산기가의 상기 범위 미만인 경우, 멜라민 수지와의 반응성이 부족하여 가교 밀도가 부족하여 제조된 도막의 내구성, 재도장 부착성 및 내용제성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 과경화되어 도막이 브리틀(Brittle)하게 되면서 외관 및 내스크래치성이 저하되는 문제가 발생할 수 있다.Additionally, the first polyester resin may have a hydroxyl value (OHv) of 200 to 300 mgKOH/g, or 220 to 280 mgKOH/g. When the hydroxyl value of the first polyester resin is within the above range, it is effective in improving the spreadability of the coating film and improving chemical resistance due to urethane reaction. In addition, when the hydroxyl value of the first polyester resin is less than the above range, there is a problem in that the durability, recoating adhesion, and solvent resistance of the produced coating film are reduced due to insufficient crosslinking density due to insufficient reactivity with the melamine resin. If the range is exceeded, problems may arise where the coating film becomes brittle due to overcuring and the appearance and scratch resistance deteriorate.
상기 제1 폴리에스터 수지는 유리전이온도(Tg)가 15 내지 30 ℃, 또는 18 내지 25 ℃일 수 있다. 제1 폴리에스터 수지의 유리전이온도가 상기 범위 내인 경우, 작업성(스프레이감)이 우수하고, 도막에 유연성을 부여하는 효과가 있다. 제1 폴리에스터 수지의 유리전이온도가 상기 범위 미만인 경우, 도료의 건조속도가 저하되어 도막의 기계적 물성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 건조속도가 빨라져 외관이 저하되고 도막이 브리틀(Brittle)하게 되면서 내스크래치성이 저하되는 문제가 발생할 수 있다.The first polyester resin may have a glass transition temperature (Tg) of 15 to 30 °C, or 18 to 25 °C. When the glass transition temperature of the first polyester resin is within the above range, workability (spray feel) is excellent and there is an effect of imparting flexibility to the coating film. If the glass transition temperature of the first polyester resin is less than the above range, the drying speed of the paint decreases, causing a problem in that the mechanical properties of the coating film deteriorate. If it exceeds the above range, the drying speed becomes faster, the appearance deteriorates, and the coating film becomes brittle. (Brittle), a problem of deterioration in scratch resistance may occur.
또한, 상기 제1 폴리에스터 수지는 중량평균분자량(Mw)이 800 내지 1,500 g/mol, 또는 1,000 내지 1,300 g/mol일 수 있다. 제1 폴리에스터 수지의 중량평균분자량이 상기 범위 내일 경우, 도료의 평활성 및 부드러운(SOFT) 도막을 형성하는 효과가 있다. 제1 폴리에스터 수지의 중량평균분자량이 상기 범위 미만인 경우, 분자량이 작아 제조된 도막의 기계적 물성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 분자량 증가에 따른 흐름성이 저하되어 도막이 딱딱해져 평활성이 감소하고 내스크래치성이 저하되는 문제가 발생할 수 있다.Additionally, the first polyester resin may have a weight average molecular weight (Mw) of 800 to 1,500 g/mol, or 1,000 to 1,300 g/mol. When the weight average molecular weight of the first polyester resin is within the above range, the paint has the effect of forming a smooth and soft coating film. If the weight average molecular weight of the first polyester resin is less than the above range, there is a problem that the mechanical properties of the produced coating film are deteriorated due to the small molecular weight, and if it exceeds the above range, the flowability decreases due to the increase in molecular weight, and the coating film becomes hard and becomes smooth. This may lead to problems such as decreased scratch resistance.
상기 제1 폴리에스터 수지는 고형분 함량(NV)이 수지 총 중량에 대하여 60 내지 85 중량%, 또는 70 내지 80 중량%일 수 있다. 제1 폴리에스터 수지의 고형분 함량이 상기 범위 내일 경우, 높은 고형분에 의한 총 휘발성 유기 화합물(TVOC)의 함량을 감소시키는 효과가 있다. 제1 폴리에스터 수지의 고형분 함량이 상기 범위 미만인 경우, 조성물의 고형분 함량의 저하로 경화 반응성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 도료의 고형분이 과도하게 많아 작업성이 열세하여 제조된 도막의 외관 특성이 저하되는 문제가 발생할 수 있다.The first polyester resin may have a solid content (NV) of 60 to 85% by weight, or 70 to 80% by weight, based on the total weight of the resin. When the solid content of the first polyester resin is within the above range, there is an effect of reducing the total volatile organic compound (TVOC) content due to the high solid content. If the solid content of the first polyester resin is less than the above range, there is a problem that curing reactivity is lowered due to a decrease in the solid content of the composition, and if it exceeds the above range, the solid content of the paint is excessively high, resulting in poor workability. Problems may arise where the exterior properties of the coating film deteriorate.
또한, 상기 제1 폴리에스터 수지는 클리어 코트 조성물의 총 중량을 기준으로 20 내지 30 중량%, 또는 22 내지 28 중량%의 함량으로 포함될 수 있다. 상기 제1 폴리에스터 수지가 상기 함량 범위 내로 포함되는 경우, 외관, 내스크래치성 및 도막 평활성 향상의 효과가 있다. 조성물 내 제1 폴리에스터 수지의 함량이 상기 범위 미만인 경우, 가교 밀도가 저하되어 기계적 물성 및 외관이 저하되는 문제가 있고, 상기 범위 초과인 경우, 조성물의 점도가 과도하게 높아져 작업성 및 건조성이 저하되는 핀홀 특성이 불량해질 수 있다.Additionally, the first polyester resin may be included in an amount of 20 to 30% by weight, or 22 to 28% by weight, based on the total weight of the clear coat composition. When the first polyester resin is included within the above content range, there is an effect of improving appearance, scratch resistance, and coating film smoothness. If the content of the first polyester resin in the composition is less than the above range, the crosslink density is lowered, leading to a problem of deterioration of mechanical properties and appearance, and if it is more than the above range, the viscosity of the composition is excessively high, resulting in poor workability and drying properties. Degraded pinhole characteristics may become poor.
제2 폴리에스터 수지2nd polyester resin
제2 폴리에스터 수지는 제조된 도막의 외관 특성을 향상시키는 역할을 한다.The second polyester resin serves to improve the appearance characteristics of the manufactured coating film.
상기 제2 폴리에스터 수지는 공지된 방법에 따라 직접 합성된 것을 사용하거나, 시판되는 제품을 사용할 수 있다. 예를 들어, 상기 제2 폴리에스터 수지는 제2 카르복실산과 제2 폴리올을 반응시켜 제조할 수 있다. The second polyester resin can be directly synthesized according to a known method, or a commercially available product can be used. For example, the second polyester resin can be produced by reacting a second carboxylic acid and a second polyol.
이때, 상기 제2 카르복실산은 예를 들어, 아디프산(AA), 이소프탈산(IPA), 트리말레트산 무수물(TMA), 지환족산, 프탈산 무수물, 이소프탈산, 테레프탈산, 숙신산, 아디프산, 푸마르산, 말레산 무수물, 테트라하이드로프탈산 무수물, 헥사히드로프탈산 무수물(HHPA), 이소노난산(INA) 및 이들의 유도체로 이루어진 군으로부터 선택된 1종 이상일 수 있다. At this time, the second carboxylic acid is, for example, adipic acid (AA), isophthalic acid (IPA), trimaltic anhydride (TMA), cycloaliphatic acid, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, It may be one or more selected from the group consisting of fumaric acid, maleic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride (HHPA), isononanoic acid (INA), and derivatives thereof.
상기 제2 폴리올은 1,6-헥산디올(1,6-HD), 펜타에리스리톨(pentaerythritol), 솔비톨(sorbitol), 메톡시폴리에틸렌글리콜, 네오펜틸글리콜(NPG), 트리메틸올 프로판(TMP), 에틸렌글리콜, 프로필렌글리콜, 디에틸렌글리콜, 부탄디올 1,4-헥산디올 및 3-메틸펜탄디올로 이루어진 군으로부터 선택된 1종 이상일 수 있다.The second polyol is 1,6-hexanediol (1,6-HD), pentaerythritol, sorbitol, methoxypolyethylene glycol, neopentyl glycol (NPG), trimethylol propane (TMP), and ethylene. It may be one or more selected from the group consisting of glycol, propylene glycol, diethylene glycol, butanediol, 1,4-hexanediol, and 3-methylpentanediol.
상기 제2 폴리에스터 수지는 산가(Av)가 20 내지 30 mgKOH/g, 또는 20 내지 25 mgKOH/g일 수 있다. 제2 폴리에스터 수지의 산가가 상기 범위 내인 경우, 열처리에 의한 급격한 경화가 방지되어 도막의 외관 불량을 방지하고 기포(popping)가 생기는 것을 줄이는 효과가 있다. 제2 폴리에스터 수지의 산가가 상기 범위 미만인 경우, 경화 반응 속도가 저하되어 제조된 도막의 경도와 외관 특성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 친수성이 향상됨에 따라 내수성이 저하되는 문제가 발생할 수 있다.The second polyester resin may have an acid value (Av) of 20 to 30 mgKOH/g, or 20 to 25 mgKOH/g. When the acid value of the second polyester resin is within the above range, rapid hardening due to heat treatment is prevented, which has the effect of preventing poor appearance of the coating film and reducing the occurrence of bubbles (popping). If the acid value of the second polyester resin is less than the above range, there is a problem that the hardness and appearance characteristics of the produced coating film decrease due to the curing reaction speed, and if it exceeds the above range, the water resistance decreases as the hydrophilicity improves. may occur.
또한, 상기 제2 폴리에스터 수지는 수산기가(OHv)가 80 내지 180 mgKOH/g, 또는 100 내지 150 mgKOH/g일 수 있다. 제2 폴리에스터 수지의 수산기가가 상기 범위 내인 경우, 도막의 퍼짐성을 향상시키고 우레탄 반응에 의한 내화학성을 향상시키 효과가 있다. 또한, 제2 폴리에스터 수지의 수산기가의 상기 범위 미만인 경우, 경화제인 멜라민 수지와의 가교 밀도가 부족하여 제조된 도막의 외관, 내구성 및 내화학성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 과경화되어 도막이 브리틀(Brittle)해져서 도장 작업성 및 내한치핑성이 저하되는 문제가 발생할 수 있다.Additionally, the second polyester resin may have a hydroxyl value (OHv) of 80 to 180 mgKOH/g, or 100 to 150 mgKOH/g. When the hydroxyl value of the second polyester resin is within the above range, it is effective in improving the spreadability of the coating film and improving chemical resistance due to urethane reaction. In addition, when the hydroxyl value of the second polyester resin is less than the above range, there is a problem that the appearance, durability, and chemical resistance of the manufactured coating film are deteriorated due to insufficient crosslinking density with the melamine resin, which is a curing agent, and when it is above the above range, Overcuring may cause the paint film to become brittle, which may result in reduced paint workability and cold chipping resistance.
상기 제2 폴리에스터 수지는 유리전이온도(Tg)가 1 내지 10 ℃, 또는 3 내지 7 ℃일 수 있다. 제2 폴리에스터 수지의 유리전이온도가 상기 범위 내인 경우, 작업성(스프레이감)이 우수하고, 도막에 유연성을 부여하는 효과가 있다. 제2 폴리에스터 수지의 유리전이온도가 상기 범위 미만인 경우, 도료의 건조속도가 저하되어 도막의 기계적 물성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 건조속도가 빨라져 외관이 저하되고 도막이 브리틀(Brittle)하게 되면서 내스크래치성이 저하되는 문제가 발생할 수 있다.The second polyester resin may have a glass transition temperature (Tg) of 1 to 10°C, or 3 to 7°C. When the glass transition temperature of the second polyester resin is within the above range, workability (spray feel) is excellent and there is an effect of imparting flexibility to the coating film. If the glass transition temperature of the second polyester resin is less than the above range, the drying speed of the paint decreases, causing a problem in that the mechanical properties of the coating film deteriorate. If it exceeds the above range, the drying speed becomes faster, the appearance deteriorates, and the coating film becomes brittle. (Brittle), a problem of deterioration in scratch resistance may occur.
또한, 상기 제2 폴리에스터 수지는 중량평균분자량(Mw)이 800 내지 1,600 g/mol, 또는 1,000 내지 1,500 g/mol일 수 있다. 제2 폴리에스터 수지의 중량평균분자량이 상기 범위 내일 경우, 도료의 평활성 및 부드러운(SOFT) 도막을 형성하는 효과가 있다. 제2 폴리에스터 수지의 중량평균분자량이 상기 범위 미만인 경우, 분자량이 작아 제조된 도막의 기계적 물성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 분자량 증가에 따른 흐름성이 저하되어 도막이 딱딱해져 평활성이 감소하고 내스크래치성이 저하되는 문제가 발생할 수 있다.Additionally, the second polyester resin may have a weight average molecular weight (Mw) of 800 to 1,600 g/mol, or 1,000 to 1,500 g/mol. When the weight average molecular weight of the second polyester resin is within the above range, the paint has the effect of forming a smooth and soft (SOFT) coating film. If the weight average molecular weight of the second polyester resin is less than the above range, there is a problem that the mechanical properties of the produced coating film are deteriorated due to the small molecular weight, and if it exceeds the above range, the flowability decreases as the molecular weight increases, and the coating film becomes hard and smooth. This may lead to problems such as decreased scratch resistance.
상기 제2 폴리에스터 수지는 고형분 함량(NV)이 수지 총 중량에 대하여 60 내지 80 중량%, 또는 65 내지 75 중량%일 수 있다. 제2 폴리에스터 수지의 고형분 함량이 상기 범위 내일 경우, 높은 고형분에 의한 총 휘발성 유기 화합물(TVOC)의 함량을 감소시키는 효과가 있다. 제2 폴리에스터 수지의 고형분 함량이 상기 범위 미만인 경우, 도료의 고형분 저하로 경화 반응성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 도료의 작업성 열세가 발생하여 제조된 도막의 외관 특성이 저하되는 문제가 발생할 수 있다.The second polyester resin may have a solid content (NV) of 60 to 80% by weight, or 65 to 75% by weight, based on the total weight of the resin. When the solid content of the second polyester resin is within the above range, there is an effect of reducing the total volatile organic compound (TVOC) content due to the high solid content. If the solid content of the second polyester resin is less than the above range, there is a problem that the curing reactivity is lowered due to a decrease in the solid content of the paint, and if it exceeds the above range, the workability of the paint is inferior, and the appearance characteristics of the manufactured coating film deteriorate. Problems may arise.
또한, 상기 제2 폴리에스터 수지는 클리어 코트 조성물의 총 중량을 기준으로 15 내지 25 중량%, 또는 17 내지 23 중량%의 함량으로 조성물에 포함될 수 있다. 상기 제2 폴리에스터 수지가 상기 함량 범위 내로 포함되는 경우, 외관, 내스크래치성 및 도막 평활성 향상의 효과가 있다. 조성물 내 제2 폴리에스터 수지의 함량이 상기 범위 미만인 경우, 도막의 가교 밀도가 저하되어 재도장 부착성 및 내스크래치성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 조성물의 점도가 과도하게 높아져 작업성 및 건조성이 저하되어 제조된 도막의 외관 특성이 저하되는 문제가 발생할 수 있다.Additionally, the second polyester resin may be included in the composition in an amount of 15 to 25% by weight, or 17 to 23% by weight, based on the total weight of the clear coat composition. When the second polyester resin is included within the above content range, there is an effect of improving appearance, scratch resistance, and coating film smoothness. If the content of the second polyester resin in the composition is less than the above range, the crosslink density of the coating film decreases, causing a problem of reduced recoating adhesion and scratch resistance, and if it exceeds the above range, the viscosity of the composition becomes excessively high. Problems may arise in which the appearance characteristics of the manufactured coating film are deteriorated due to reduced workability and drying properties.
실리콘 변성 폴리에스터 수지Silicone modified polyester resin
실리콘 변성 폴리에스터 수지는 반응성이 빨라 제조된 도막에 핀홀 발생을 방지하여 외관 특성을 향상시키는 역할을 한다.Silicone-modified polyester resin is highly reactive and prevents pinholes from forming in the manufactured coating film, thereby improving the appearance characteristics.
상기 실리콘 변성 폴리에스터 수지의 폴리에스터 수지는 공지된 방법에 따라 직접 합성된 것을 사용하거나, 시판되는 제품을 사용할 수 있으며, 제3 카르복실산과 제3 폴리올을 반응시켜 제조한 폴리에스터 수지를 유기 폴리실록산 으로 변성한 것일 수 있다.The polyester resin of the silicone-modified polyester resin can be directly synthesized according to a known method, or a commercially available product can be used, and the polyester resin prepared by reacting the third carboxylic acid and the third polyol can be used as an organic polysiloxane. It may have been transformed into .
이때, 상기 제3 카르복실산은 예를 들어, 아디프산(AA), 이소프탈산(IPA), 트리말레트산 무수물(TMA), 지환족산, 프탈산 무수물, 이소프탈산, 테레프탈산, 숙신산, 아디프산, 푸마르산, 말레산 무수물, 테트라하이드로프탈산 무수물, 헥사히드로프탈산 무수물(HHPA), 이소노난산(INA) 및 이들의 유도체로 이루어진 군으로부터 선택된 1종 이상일 수 있다. At this time, the third carboxylic acid is, for example, adipic acid (AA), isophthalic acid (IPA), trimaltic anhydride (TMA), cycloaliphatic acid, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, It may be one or more selected from the group consisting of fumaric acid, maleic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride (HHPA), isononanoic acid (INA), and derivatives thereof.
상기 제3 폴리올은 1,6-헥산디올(1,6-HD), 펜타에리스리톨(pentaerythritol), 솔비톨(sorbitol), 메톡시폴리에틸렌글리콜, 네오펜틸글리콜(NPG), 트리메틸올 프로판(TMP), 에틸렌글리콜, 프로필렌글리콜, 디에틸렌글리콜, 부탄디올 1,4-헥산디올 및 3-메틸펜탄디올로 이루어진 군으로부터 선택된 1종 이상일 수 있다.The third polyol is 1,6-hexanediol (1,6-HD), pentaerythritol, sorbitol, methoxypolyethylene glycol, neopentyl glycol (NPG), trimethylol propane (TMP), and ethylene. It may be one or more selected from the group consisting of glycol, propylene glycol, diethylene glycol, butanediol, 1,4-hexanediol, and 3-methylpentanediol.
상기 유기 폴리실록산은 관능기 및 비관능 유기기를 포함할 수 있다. 예를 들어, 상기 유기 폴리실록산은 실란올 및 알콕시기로 이루어진 군으로부터 선택된 1종 이상의 관능기를 포함하고, 메틸, 프로필 및 페닐기로 이루어진 군으로부터 선택된 1종 이상의 비관능 유기기를 포함할 수 있다. 상기 알콕시기는 예를 들어, 메톡시, 에톡시 및 부톡시기를 들 수 있다.The organic polysiloxane may include functional groups and non-functional organic groups. For example, the organic polysiloxane may include one or more functional groups selected from the group consisting of silanol and alkoxy groups, and may include one or more non-functional organic groups selected from the group consisting of methyl, propyl, and phenyl groups. The alkoxy group includes, for example, methoxy, ethoxy, and butoxy groups.
상기 실리콘 변성 폴리에스터 수지는 산가(Av)가 10mgKOH/g 이하, 8mgKOH/g 이하, 또는 1 내지 8 mgKOH/g일 수 있다. 실리콘 변성 폴리에스터 수지의 산가가 상기 범위 미만인 경우, 도료의 표면 장력이 높아 제조된 도막의 외관 특성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 도료의 표면 장력이 너무 낮아 제조된 도막의 기계적 물성이 저하되는 문제가 발생할 수 있다.The silicone-modified polyester resin may have an acid value (Av) of 10 mgKOH/g or less, 8 mgKOH/g or less, or 1 to 8 mgKOH/g. If the acid value of the silicone-modified polyester resin is less than the above range, the surface tension of the paint is high, which causes a problem in that the appearance characteristics of the manufactured paint film are deteriorated. If it exceeds the above range, the surface tension of the paint is too low, causing mechanical problems of the manufactured paint film. Problems with deterioration of physical properties may occur.
또한, 상기 실리콘 변성 폴리에스터 수지는 수산기가(OHv)가 150 내지 250 mgKOH/g, 또는 190 내지 210 mgKOH/g일 수 있다. 실리콘 변성 폴리에스터 수지의 수산기가의 상기 범위 미만인 경우, 멜라민 수지와의 반응성이 부족하여 가교 밀도가 저하되어 제조된 도막의 내구성 및 내화학성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 과경화되어 도막이 브리틀(Brittle)하게 되면서 외관 특성 및 내스크래치성이 저하되는 문제가 발생할 수 있다.Additionally, the silicone-modified polyester resin may have a hydroxyl value (OHv) of 150 to 250 mgKOH/g, or 190 to 210 mgKOH/g. If the hydroxyl value of the silicone-modified polyester resin is less than the above range, there is a problem that the durability and chemical resistance of the produced coating film is reduced due to insufficient reactivity with the melamine resin and the crosslinking density is lowered, and if it exceeds the above range, overcuring occurs. As a result, the coating film becomes brittle, which may cause problems with deterioration in appearance characteristics and scratch resistance.
상기 실리콘 변성 폴리에스터 수지는 유리전이온도(Tg)가 -20 내지 0 ℃, 또는 -15 내지 -5 ℃일 수 있다. 실리콘 변성 폴리에스터 수지의 유리전이온도가 상기 범위 미만인 경우, 탄성이 증가하여 도료의 경도가 저하되고 건조성 열세에 따른 도막의 외관 특성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 도료의 흐름성이 저하로 도막의 외관 특성이 저하되고 도막의 탄성이 떨어져 부착성 및 내치핑성이 저하되는 문제가 발생할 수 있다.The silicone-modified polyester resin may have a glass transition temperature (Tg) of -20 to 0 °C, or -15 to -5 °C. If the glass transition temperature of the silicone-modified polyester resin is less than the above range, there is a problem that the hardness of the paint decreases due to increased elasticity and the appearance characteristics of the paint film deteriorate due to poor drying, and if it exceeds the above range, the flow of the paint Due to a decrease in properties, the appearance characteristics of the coating film may deteriorate and the elasticity of the coating film may decrease, which may cause problems such as deterioration in adhesion and chipping resistance.
상기 실리콘 변성 폴리에스터 수지는 25℃에서의 점도가 5,000 내지 10,000 cps, 또는 6,000 내지 9,000 cps일 수 있다. 실리콘 변성 폴리에스터 수지의 25℃에서의 점도가 상기 범위 미만인 경우, 조성물의 점도가 너무 낮아 제조된 도막의 미형성으로 도막의 부착성 및 내스크래치성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 조성물의 작업성이 부족하여 제조된 도막의 외관 특성이 저하되는 문제가 발생할 수 있다.The silicone-modified polyester resin may have a viscosity of 5,000 to 10,000 cps, or 6,000 to 9,000 cps at 25°C. If the viscosity of the silicone-modified polyester resin at 25°C is less than the above range, the viscosity of the composition is too low and there is a problem of deterioration of the adhesion and scratch resistance of the coating film due to non-formation of the manufactured coating film, and if it exceeds the above range. , a problem may occur in which the appearance characteristics of the manufactured coating film are deteriorated due to insufficient workability of the composition.
또한, 상기 실리콘 변성 폴리에스터 수지는 고형분 함량(NV)이 수지 총 중량에 대하여 80중량% 이상, 또는 85 내지 95 중량%일 수 있다. 실리콘 변성 폴리에스터 수지의 고형분 함량이 상기 범위 미만인 경우, 조성물의 고형분 저하로 경화 반응성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 제조된 도료의 작업성이 열세하여 도막의 외관 특성이 저하되는 문제가 발생할 수 있다.Additionally, the silicone-modified polyester resin may have a solid content (NV) of 80% by weight or more, or 85 to 95% by weight, based on the total weight of the resin. If the solid content of the silicone-modified polyester resin is less than the above range, there is a problem that the curing reactivity is lowered due to a decrease in the solid content of the composition, and if it exceeds the above range, the workability of the manufactured paint is inferior and the appearance characteristics of the coating film are deteriorated. Problems may arise.
상기 실리콘 변성 폴리에스터 수지는 클리어 코트 조성물의 총 중량을 기준으로 2 내지 10 중량%, 또는 4 내지 8 중량%의 함량으로 포함될 수 있다. 상기 실리콘 변성 폴리에스터 수지가 상기 함량 범위 내로 포함되는 경우, 외관, 내스크래치성 및 도막 평활성 향상의 효과가 있다. 조성물 내 폴리에스터 수지의 함량이 상기 범위 미만인 경우, 가교 밀도가 저하되어 외관 및 내스크래치성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 조성물의 점도가 과도하게 높아져 작업성 및 건조성이 저하되어 외관 및 기계적 물성이 저하되는 문제가 발생할 수 있다.The silicone-modified polyester resin may be included in an amount of 2 to 10% by weight, or 4 to 8% by weight, based on the total weight of the clear coat composition. When the silicone-modified polyester resin is included within the above content range, there is an effect of improving appearance, scratch resistance, and coating film smoothness. If the content of polyester resin in the composition is less than the above range, the crosslink density is lowered, which causes a problem of poor appearance and scratch resistance, and if it is more than the above range, the viscosity of the composition is excessively high, resulting in reduced workability and drying properties. This may cause problems with deterioration of appearance and mechanical properties.
멜라민 수지melamine resin
멜라민 수지는 경화제로서, 클리어 코트 조성물의 각 성분들과 가교 반응하여 조성물을 경화시키는 역할을 한다. Melamine resin is a curing agent and serves to harden the composition by crosslinking with each component of the clear coat composition.
상기 멜라민 수지는 공지된 방법에 따라 직접 합성된 것을 사용하거나, 시판되는 제품을 사용할 수 있다. 예를 들어, 멜라민 수지로는 메톡시 메틸 멜라민, 메틸 멜라민, 부틸 멜라민, 이소부톡시 멜라민, 부톡시 멜라민, 헥사메틸올 멜라민, 헥사메톡시 메틸 멜라민, 헥사부톡시 메틸 멜라민, 헥사메톡시부톡시 메틸 멜라민 및 이미노메톡시 메틸 멜라민으로 이루어진 군으로부터 선택되는 하나 이상을 사용할 수 있다.The melamine resin can be directly synthesized according to a known method, or a commercially available product can be used. For example, melamine resins include methoxy methyl melamine, methyl melamine, butyl melamine, isobutoxy melamine, butoxy melamine, hexamethylol melamine, hexamethoxy methyl melamine, hexabutoxy methyl melamine, and hexamethoxybutoxy methyl. One or more selected from the group consisting of melamine and iminomethoxy methyl melamine may be used.
또한, 상기 멜라민 수지는 중량평균분자량(Mw)이 100 내지 5,000g/mol, 500 내지 4,500 g/mol, 또는 1,000 내지 4,000 g/mol일 수 있다. 멜라민 수지의 중량평균분자량이 상기 범위 내일 경우, 가교 밀도를 향상시켜 제조된 도막의 부착성 및 경도를 향상시키는 효과가 있다. 또한, 멜라민 수지의 중량평균분자량이 상기 범위 미만인 경우, 도막의 가교 밀도가 저하되어 내화학성 및 내스크래치성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 분자량 상향에 따라 도막의 외관 특성이 저하되는 문제가 발생할 수 있다.Additionally, the melamine resin may have a weight average molecular weight (Mw) of 100 to 5,000 g/mol, 500 to 4,500 g/mol, or 1,000 to 4,000 g/mol. When the weight average molecular weight of the melamine resin is within the above range, there is an effect of improving the adhesion and hardness of the manufactured coating film by improving the crosslinking density. In addition, if the weight average molecular weight of the melamine resin is less than the above range, the crosslink density of the coating film decreases, which causes a problem of reduced chemical resistance and scratch resistance, and if it exceeds the above range, the appearance characteristics of the coating film deteriorate as the molecular weight increases. Problems may arise.
상기 멜라민 수지는 25℃에서의 점도가 400 내지 1,200 cps, 500 내지 1,100 cps, 또는 600 내지 1,000 cps일 수 있다. 멜라민 수지의 25℃에서의 점도가 상기 범위 내일 경우, 제조된 도막의 광택 및 외관이 우수한 효과가 있다. 또한, 멜라민 수지의 25℃에서의 점도가 상기 범위 미만인 경우, 점도가 낮아 도막 미형성으로 도막의 부착성 및 내스크래치성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 조성물의 작업성이 열세하여 제조된 도막의 외관 특성이 부족한 문제가 발생할 수 있다.The melamine resin may have a viscosity of 400 to 1,200 cps, 500 to 1,100 cps, or 600 to 1,000 cps at 25°C. When the viscosity of the melamine resin at 25°C is within the above range, the produced coating film has excellent gloss and appearance. In addition, if the viscosity of the melamine resin at 25°C is less than the above range, the viscosity is low and the adhesion and scratch resistance of the coating film are reduced due to non-formation of the coating film, and if it exceeds the above range, the workability of the composition is inferior. As a result, a problem may arise in which the appearance characteristics of the manufactured coating film are insufficient.
또한, 상기 멜라민 수지는 산가(Av)가 5mgKOH/g 이하, 또는 0.1 내지 3 mgKOH/g일 수 있다. 멜라민 수지의 산가가 상기 범위 미만인 경우, 경화 반응 속도가 저하되어 제조된 도막의 경도와 외관특성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 친수성이 향상됨에 따라 내수성이 저하되는 문제가 발생할 수 있다.Additionally, the melamine resin may have an acid value (Av) of 5 mgKOH/g or less, or 0.1 to 3 mgKOH/g. If the acid value of the melamine resin is less than the above range, the hardness and appearance characteristics of the produced coating film may decrease due to a decrease in the curing reaction rate. If the acid value of the melamine resin exceeds the above range, the water resistance may decrease as the hydrophilicity improves. there is.
상기 멜라민 수지는 고형분 함량(NV)이 수지 총 중량에 대하여 50 내지 70 중량%, 또는 55 내지 60 중량%일 수 있다. 멜라민 수지의 고형분 함량이 상기 범위 미만인 경우, 도료의 작업성이 저하되는 문제가 발생하며, 상기 범위 초과인 경우, 도료 제조상 고고형분으로 인해 작업성 저하되는 문제가 발생할 수 있다.The melamine resin may have a solid content (NV) of 50 to 70% by weight, or 55 to 60% by weight, based on the total weight of the resin. If the solid content of the melamine resin is less than the above range, the workability of the paint may be reduced, and if it exceeds the above range, the workability may be reduced due to the high solid content during the manufacture of the paint.
또한, 상기 멜라민 수지는 클리어 코트 조성물의 총 중량을 기준으로 5 내지 15 중량%, 또는 7 내지 13 중량%의 함량으로 포함될 수 있다. 상기 멜라민 수지가 상기 함량 범위 내로 포함되는 경우, 가교 밀도를 향상시켜 제조된 도막의 부착성 및 경도를 향상시키는 효과가 있다. 조성물 내 멜라민 수지의 함량이 상기 범위 미만인 경우, 경화성 저하에 따른 기계적 물성 및 내화학성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 경화성 과다에 따른 도막이 브리틀(Brittle)해짐에 따라 부착성 저하 및 내치핑성이 저하되는 문제가 발생할 수 있다.Additionally, the melamine resin may be included in an amount of 5 to 15% by weight, or 7 to 13% by weight, based on the total weight of the clear coat composition. When the melamine resin is included within the above content range, there is an effect of improving the adhesion and hardness of the manufactured coating film by improving the crosslinking density. If the content of melamine resin in the composition is less than the above range, there is a problem of deterioration of mechanical properties and chemical resistance due to a decrease in curability, and if it exceeds the above range, the adhesion decreases as the coating film becomes brittle due to excessive curability. And problems such as deterioration in chipping resistance may occur.
상기 클리어 코트 조성물은 용제를 추가로 포함할 수 있다.The clear coat composition may further include a solvent.
용제solvent
용제는 조성물의 점도를 조절하고, 건조성을 개선하며, 제조된 도막의 외관 특성 및 퍼짐성을 개선시키는 역할을 한다. The solvent controls the viscosity of the composition, improves drying properties, and improves the appearance characteristics and spreadability of the produced coating film.
상기 용제는 통상적으로 클리어 코트 조성물에 사용되는 것이라면 특별히 제한되지 않으며, 예를 들어, 방향족, 아세테이트계, 알콜계 및 프로피오네이트계로 이루어진 군으로부터 선택된 1종 이상을 포함할 수 있다. 구체적으로, 상기 용제는 톨루엔 및 크실렌 등의 방향족 용제; 1-메톡시-2-프로필아세테이트, 메틸아세테이트, 에틸아세테이트, n-프로필아세테이트, n-부틸아세테이트, 메틸 글루타레이트, 메틸 석신에이트, 메틸 아디페이트, 디메틸 글루타레이트, 디메틸 석신에이트, 디메틸 아디페이트, 부틸 카르비톨 아세테이트, 부틸 셀로솔브 아세테이트, 프로필렌글리콜 메틸 에테르 아세테이트(PMA), 트리메틸-o-아세테이트 등의 아세테이트계 용제; n-부탄올, 프로판올, 1-메톡시-2-프로판올, 2-부톡시에탄올 등의 알콜계 용제; 아세톤, 메틸에틸케톤, 메틸부틸케톤 및 메틸이소부틸케톤 등의 케톤계; 및 에틸에톡시프로피오네이트 등의 프로피오네이트계 용제; 등을 포함할 수 있다. 또한, 상기 방향족 용제의 시판품으로는 코코졸 #100, 코코졸 #150 등을 들 수 있다.The solvent is not particularly limited as long as it is commonly used in clear coat compositions, and may include, for example, one or more selected from the group consisting of aromatic, acetate-based, alcohol-based, and propionate-based solvents. Specifically, the solvent includes aromatic solvents such as toluene and xylene; 1-methoxy-2-propyl acetate, methyl acetate, ethyl acetate, n-propyl acetate, n-butyl acetate, methyl glutarate, methyl succinate, methyl adipate, dimethyl glutarate, dimethyl succinate, dimethyl adipate Acetate-based solvents such as pate, butyl carbitol acetate, butyl cellosolve acetate, propylene glycol methyl ether acetate (PMA), and trimethyl-o-acetate; Alcohol-based solvents such as n-butanol, propanol, 1-methoxy-2-propanol, and 2-butoxyethanol; Ketones such as acetone, methyl ethyl ketone, methyl butyl ketone, and methyl isobutyl ketone; and propionate-based solvents such as ethyl ethoxypropionate; It may include etc. Additionally, commercially available products of the aromatic solvent include Cocosol #100 and Cocosol #150.
또한, 상기 용제는 클리어 코트 조성물의 총 중량을 기준으로 5 내지 40 중량%, 또는 10 내지 35 중량%의 함량으로 포함될 수 있다. 상기 용제가 상기 범위 내로 포함되는 경우, 조성물의 점도를 적절히 조절하여 작업성 및 건조성이 향상되는 효과가 있다. 또한, 용제의 함량이 상기 범위 미만인 경우, 조성물 내 고형분의 함량이 높아 조성물의 작업성이 부족한 문제가 있고, 상기 범위 초과인 경우, 제조된 도료의 고형분 함량이 낮아 제조된 도막의 외관 및 부착성이 부족한 문제가 발생할 수 있다.Additionally, the solvent may be included in an amount of 5 to 40% by weight, or 10 to 35% by weight, based on the total weight of the clear coat composition. When the solvent is contained within the above range, the viscosity of the composition is appropriately adjusted, thereby improving workability and drying properties. In addition, if the solvent content is less than the above range, there is a problem of insufficient workability of the composition due to the high solid content in the composition, and if it exceeds the above range, the solid content of the manufactured paint is low, affecting the appearance and adhesion of the manufactured coating film. This shortage problem may occur.
첨가제additive
본 발명에 따른 클리어 코트 조성물은 흐름성 조절제, 자외선 흡수제, 분산제, 표면 조정제, 소포제 및 경화 촉매 등의 첨가제를 추가로 포함할 수 있다. 이때, 상기 첨가제는 통상적으로 도료 조성물에 첨가할 수 있는 것이라면 특별히 제한하지 않는다. The clear coat composition according to the present invention may further include additives such as flow control agents, ultraviolet absorbers, dispersants, surface conditioners, anti-foaming agents, and curing catalysts. At this time, the additive is not particularly limited as long as it can be added to the paint composition normally.
또한, 상기 첨가제의 함량은 통상적으로 클리어 코트 조성물에 포함될 수 있는 범위라면 특별히 한정하지 않으며, 예를 들어, 클리어 코트 조성물의 총 중량을 기준으로 10 내지 30 중량%, 또는 15 내지 25 중량%의 함량으로 포함될 수 있다.In addition, the content of the additive is not particularly limited as long as it is within the range that can normally be included in the clear coat composition, for example, the content is 10 to 30% by weight, or 15 to 25% by weight based on the total weight of the clear coat composition. may be included.
상기 클리어 코트 조성물은 고형분 함량이 40 내지 60 중량%, 또는 45 내지 55 중량%일 수 있다. 상기 클리어 코트 조성물의 고형분 함량이 상기 범위 내일 경우, 조성물의 도장 작업성이 적절해지는 장점이 있다.The clear coat composition may have a solid content of 40 to 60% by weight, or 45 to 55% by weight. When the solid content of the clear coat composition is within the above range, there is an advantage that the painting workability of the composition becomes appropriate.
또한, 상기 클리어 코트 조성물은 25℃에서의 포드컵 4번을 기준으로 15 내지 50 초, 또는 20 내지 35 초의 점도를 가질 수 있다. 상기 클리어 코트 조성물의 25℃에서의 점도가 상기 범위 미만인 경우, 수직면 흘러내림 등의 문제가 발생하여 작업성이 부족할 수 있고, 상기 범위 초과인 경우, 조성물의 점도가 높아 이로부터 제조된 도막의 외관 특성이 저하거나 도장기에 부하가 걸려 도장기 고장의 원인이 될 수 있다.Additionally, the clear coat composition may have a viscosity of 15 to 50 seconds, or 20 to 35 seconds, based on Ford Cup No. 4 at 25°C. If the viscosity of the clear coat composition at 25°C is less than the above range, problems such as flowing down vertical surfaces may occur and workability may be insufficient, and if it exceeds the above range, the viscosity of the composition is high and the appearance of the coating film manufactured therefrom may be impaired. This may cause the sprayer to malfunction due to poor characteristics or load on the sprayer.
상술한 바와 같은 본 발명에 따른 클리어 도료 조성물은 반응성이 우수하여 도장 후 건조 시간이 짧거나 클리어 코트 건조 후 경화를 위한 오븐까지의 이동 거리가 짧거나, 차체 간 거리가 짧은 경우도 제조된 도막의 핀홀이 발생하지 않고 광택 저하가 발생하지 않아 외관 특성이 우수하다. 또한, 상기 클리어 코트 조성물로부터 제조된 도막은 경도, 부착성, 내스크래치성 등의 기계적 물성도 우수하여 차체 도장용으로 유용하게 사용할 수 있다.As described above, the clear paint composition according to the present invention has excellent reactivity, so even when the drying time after painting is short, the travel distance to the oven for curing after drying the clear coat is short, or the distance between car bodies is short, the manufactured paint film It has excellent appearance characteristics as no pinholes occur and no loss of gloss occurs. In addition, the coating film prepared from the clear coat composition has excellent mechanical properties such as hardness, adhesion, and scratch resistance, and can be usefully used for car body painting.
클리어 도료 키트clear paint kit
또한, 본 발명의 클리어 도료 키트는 상술한 바와 같은 클리어 코트 조성물; 및 경화제;를 포함한다. 즉, 본 발명의 클리어 도료 키트는 2액형 도료이다.Additionally, the clear paint kit of the present invention includes the clear coat composition as described above; and a curing agent. That is, the clear paint kit of the present invention is a two-component paint.
상기 클리어 도료 키트는 사용전 상기 클리어 코트 조성물과 경화제를 혼합한 후 사용할 수 있다. The clear paint kit can be used after mixing the clear coat composition and hardener before use.
경화제hardener
경화제는 상술한 바와 같은 수지의 수산기와 반응하여 우레탄 결합을 형성하여 조성물을 경화시킴으로써 도막을 형성하는 역할을 한다.The curing agent serves to form a coating film by reacting with the hydroxyl group of the resin as described above to form a urethane bond and curing the composition.
상기 경화제는 이소시아네이트계 경화제일 수 있다. 이때, 상기 이소시아네이트계 경화제는 그 종류를 특별히 한정하지 않으며, 예를 들어, 황변 현상이 없는 지방족 폴리이소시아네이트 화합물을 포함할 수 있다. 구체적으로, 상기 이소시아네이트계 경화제는 헥사메틸렌 디이소시아네이트, 이소포론 디이소시아네이트, 4,4'-디사이클로헥실 메탄 디이소시아네이트, 테트라메틸 크실렌 디이소시아네이트 또는 이들의 혼합물을 포함할 수 있다.The curing agent may be an isocyanate-based curing agent. At this time, the type of the isocyanate-based curing agent is not particularly limited, and may include, for example, an aliphatic polyisocyanate compound without yellowing phenomenon. Specifically, the isocyanate-based curing agent may include hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexyl methane diisocyanate, tetramethyl xylene diisocyanate, or mixtures thereof.
또한, 상기 이소시아네이트계 경화제는 경화제 총 중량에 대하여 미반응 이소시아네이트기의 함량(NCO%)이 15 내지 30 중량%, 또는 19 내지 24 중량%일 수 있다. 이소시아네이트계 경화제의 NCO%가 상기 범위 미만인 경우, 도막의 가교 밀도가 저하되어 도막의 내충격성, 내수성 및 내한치핑성이 저하되는 문제가 있고, 상기 범위 초과인 경우, 경화 속도가 증대되고 수지가 응집되어 도막의 외관 특성, 광택 및 기계적 물성이 저하되는 문제가 발생할 수 있다.In addition, the isocyanate-based curing agent may have an unreacted isocyanate group content (NCO%) of 15 to 30 wt%, or 19 to 24 wt%, based on the total weight of the curing agent. If the NCO% of the isocyanate-based curing agent is less than the above range, the crosslink density of the coating film decreases, which causes a problem in that the impact resistance, water resistance, and cold chipping resistance of the coating film deteriorate. If it exceeds the above range, the curing speed increases and the resin aggregates. This may cause problems such as deterioration in the appearance, gloss, and mechanical properties of the coating film.
상기 클리어 도료 키트는 클리어 코트 조성물과 경화제를 2 내지 4 : 1의 중량비, 또는 2.5 내지 3.4 : 1의 중량비로 포함할 수 있다. 클리어 코트 조성물과 경화제의 중량비가 상기 범위 미만인 경우, 즉 경화제 중량에 대하여 소량의 클리어 코트 조성물을 포함하는 경우, 경화 후 도막 내에 미반응 이소시아네이트기가 발생하여 도막의 물성이 저하되는 문제가 발생하고, 상기 범위 초과인 경우, 즉 경화제 중량에 대하여 과량의 클리어 코트 조성물을 포함하는 경우, 조성물의 반응성이 부족하여 경화 밀도가 떨어지는 문제가 발생할 수 있다.The clear paint kit may include a clear coat composition and a curing agent at a weight ratio of 2 to 4:1, or 2.5 to 3.4:1. If the weight ratio of the clear coat composition and the curing agent is less than the above range, that is, if a small amount of the clear coat composition is included relative to the weight of the curing agent, unreacted isocyanate groups are generated in the coating film after curing, causing a problem in which the physical properties of the coating film are deteriorated. If the range is exceeded, that is, if an excessive amount of clear coat composition is included relative to the weight of the curing agent, a problem of low curing density may occur due to insufficient reactivity of the composition.
상기 클리어 도료 키트는 고형분 함량이 50 내지 70 중량%, 또는 55 내지 65 중량%일 수 있다. 상기 클리어 도료 키트의 고형분 함량이 상기 범위 내일 경우, 조성물의 도장 작업성이 적절해지는 장점이 있다.The clear paint kit may have a solid content of 50 to 70% by weight, or 55 to 65% by weight. When the solid content of the clear paint kit is within the above range, there is an advantage that the painting workability of the composition becomes appropriate.
또한, 상기 클리어 도료 키트는 25℃에서의 포드컵 4번을 기준으로 20 내지 50 초, 또는 25 내지 45 초의 점도를 가질 수 있다. 상기 클리어 도료 키트의 25℃에서의 점도가 상기 범위 미만인 경우, 수직면 흘러내림 등의 문제가 발생할 수 있고, 상기 범위 초과인 경우, 도료의 점도가 높아 이로부터 제조된 도막의 외관 특성이 저하거나 도장기에 부하가 걸려 도장기 고장의 원인이 될 수 있다.Additionally, the clear paint kit may have a viscosity of 20 to 50 seconds, or 25 to 45 seconds based on Ford Cup No. 4 at 25°C. If the viscosity of the clear paint kit at 25°C is less than the above range, problems such as dripping on vertical surfaces may occur, and if it exceeds the above range, the viscosity of the paint is high, so the appearance characteristics of the paint film manufactured therefrom deteriorate or the paint may be damaged. The load on the machine may cause the sprayer to malfunction.
상술한 바와 같은 본 발명에 따른 클리어 도료 키트는 반응성이 우수하여 도장 후 건조 시간이 짧거나 클리어 코트 건조 후 경화를 위한 오븐까지의 이동 거리가 짧거나, 차체 간 거리가 짧은 경우도 제조된 도막의 핀홀이 발생하지 않고 광택 저하가 발생하지 않아 외관 특성이 우수하다.As described above, the clear paint kit according to the present invention has excellent reactivity, so even when the drying time after painting is short, the travel distance to the oven for curing after drying the clear coat is short, or the distance between car bodies is short, the manufactured paint film can be used. It has excellent appearance characteristics as no pinholes occur and no loss of gloss occurs.
이하, 실시예를 통해 본 발명을 보다 구체적으로 설명한다. 그러나 이들 실시예는 본 발명의 이해를 돕기 위한 것일 뿐 어떠한 의미로든 본 발명의 범위가 이들 실시예로 한정되는 것은 아니다.Hereinafter, the present invention will be described in more detail through examples. However, these examples are only intended to aid understanding of the present invention, and the scope of the present invention is not limited to these examples in any way.
[실시예][Example]
실시예 1 내지 21 및 비교예 1 내지 11. 클리어 코트 조성물의 제조Examples 1 to 21 and Comparative Examples 1 to 11. Preparation of clear coat composition
표 1 내지 3과 같은 함량의 성분을 혼합하여 25℃에서의 점도가 포드컵 4호를 기준으로 28초의 클리어 코트 조성물을 제조하였다. The ingredients in the same amounts as shown in Tables 1 to 3 were mixed to prepare a clear coat composition with a viscosity of 28 seconds at 25°C based on Ford Cup No. 4.
이하, 비교예 및 실시예에서 사용한 각 성분들의 제조사 및 제품명, 또는 성분명 등은 표 4에 나타냈다.Hereinafter, the manufacturer, product name, or ingredient name of each ingredient used in comparative examples and examples is shown in Table 4.
참조예. 경화제의 제조Reference example. Preparation of hardeners
이소시아네이트계 수지로 헥사메틸렌디이소시아네이트(HMDI) 49중량%, 유기 용제로 코코졸-100 15중량%, 자일렌 17중량% 및 부틸 아세테이트 19중량%를 혼합하여 경화제를 제조하였다.A curing agent was prepared by mixing 49% by weight of hexamethylene diisocyanate (HMDI) as an isocyanate resin, 15% by weight of Cocosol-100, 17% by weight of xylene, and 19% by weight of butyl acetate as an organic solvent.
제조된 경화제는 미반응 이소시아네이트기의 함량(NCO%)가 21중량%였다.The prepared curing agent had an unreacted isocyanate group content (NCO%) of 21% by weight.
실험예. 도막의 특성 평가Experiment example. Evaluation of paint film properties
시편에 프라이머 도료(제조사: KCC, 제품명: FU2290)를 도포하고 140℃에서 20분간 경화시켜 두께 40㎛의 프라이머 도막을 형성하였다. 이후 프라이머 도막 상에 베이스 코트(제조사: KCC, 제품명: WT3062)를 벨도장하고 80℃에서 3분간 핫 에어를 불어주어 도료 내에 잔존하는 물을 증발시켜 두께 15㎛의 베이스 도막을 형성하였다. Primer paint (manufacturer: KCC, product name: FU2290) was applied to the specimen and cured at 140°C for 20 minutes to form a primer film with a thickness of 40㎛. Afterwards, a base coat (manufacturer: KCC, product name: WT3062) was applied on the primer film, and hot air was blown at 80°C for 3 minutes to evaporate the water remaining in the paint, forming a base film with a thickness of 15㎛.
이후 베이스 도막 상에 실시예 및 비교예에서 제조한 클리어 코트 조성물과 참조예의 경화제를 3:1의 중량비로 혼합하여 클리어 도료를 제조하고, 상기 클리어 도료를 도장하고 140℃에서 25분 동안 경화하여 두께 40㎛의 클리어 도막을 형성하여 최종 도막을 제조하였다. 상기 시편을 대상으로 하기와 같은 방법으로 물성을 측정하였으며, 그 결과를 표 5에 나타냈다.Afterwards, a clear paint was prepared by mixing the clear coat composition prepared in Examples and Comparative Examples and the curing agent of the Reference Example at a weight ratio of 3:1 on the base coating film, and the clear paint was applied and cured at 140°C for 25 minutes to obtain a thickness. The final coating film was prepared by forming a 40㎛ clear coating film. The physical properties of the specimen were measured in the following manner, and the results are shown in Table 5.
(1) 핀홀 특성(1) Pinhole characteristics
클리어 도료를 두께 10 내지 80 ㎛까지 5㎛ 간격의 두께로 상술한 바와 동일한 방법으로 도장하면서 최초 핀홀 발생 지점을 측정하였다.The clear paint was applied in the same manner as described above at a thickness of 10 to 80 ㎛ at 5 ㎛ intervals, and the point where the first pinhole occurred was measured.
구체적으로, 두께 60㎛ 이상에서 핀홀이 발생한 경우 우수(◎), 두께 50㎛ 이상 60㎛ 미만에서 핀홀이 발생한 경우 양호(○), 두께 40㎛ 이상 50㎛ 미만에서 핀홀이 발생한 경우 보통(△), 두께 40㎛ 미만에서 핀홀이 발생한 경우 불량(×)으로 평가하였다.Specifically, if a pinhole occurs at a thickness of 60㎛ or more, excellent (◎), if a pinhole occurs at a thickness of 50㎛ or more but less than 60㎛, good (○), and if a pinhole occurs at a thickness of 40㎛ or more but less than 50㎛, then average (△). , if a pinhole occurred at a thickness of less than 40㎛, it was evaluated as defective (×).
(2) 외관(2) Appearance
제조된 최종 도막을 대상으로 자동차 외관 측정기인 Wave Scan DOI(BYK Gardner)를 이용하여 광택(LU), 선명도(SH) 및 오렌지필(OP)을 측정하였으며, 측정된 물성을 이용하여 종합 외관 평가 수치(CF)을 하기 수학식 1로 계산하였다.Gloss (LU), clarity (SH), and orange peel (OP) were measured for the manufactured final coating using an automotive exterior measuring instrument, Wave Scan DOI (BYK Gardner), and comprehensive appearance evaluation values were obtained using the measured physical properties. (CF) was calculated using Equation 1 below.
[수학식 1][Equation 1]
CF = LU X 0.15 + SH X 0.35 + OP X 0.5CF = LU
이때, CF는 수평 및 수직으로 측정 및 계산하였다.At this time, CF was measured and calculated horizontally and vertically.
계산된 CF가 65 이상일 경우 우수(◎), 60 이상 65 미만일 경우 양호(○), 55 이상 60 미만일 경우 보통(△), 55 미만일 경우 불량(×)으로 평가하였다.If the calculated CF was 65 or more, it was evaluated as excellent (◎), if it was 60 or more but less than 65, it was evaluated as good (○), if it was 55 or more but less than 60, it was evaluated as average (△), and if it was less than 55, it was evaluated as poor (×).
(3) 광택(3) Glossy
최종 도막을 대상으로 광택기(Gloss Meter)를 이용하여 20° 광택을 측정하였으며, 20° 광택이 91 이상인 경우 우수(◎), 89 이상 91 미만일 경우 양호(○), 87 이상 89 미만일 경우 보통(△), 87 미만일 경우 불량(×)으로 평가하였다.The 20° gloss of the final film was measured using a gloss meter. If the 20° gloss was 91 or more, it was excellent (◎), if it was 89 or more but less than 91, it was good (○), and if it was 87 or more but less than 89, it was average (△). ), if it was less than 87, it was evaluated as defective (×).
(4) 재도장 부착성(4) Recoating adhesion
최종 도막을 대상으로 상술한 바와 동일한 방법으로 베이스 코트 및 클리어 코트를 도장한 후 바둑목법으로 재도장 부착성을 평가하였다.The base coat and clear coat were applied to the final film in the same manner as described above, and then the adhesion of recoating was evaluated using the checkerboard method.
구체적으로, 상기 바둑목법은 최종 도막의 표면을 칼로 가로 2mm 및 세로 2mm의 정사각형 100개를 만든 후 테이프를 사용하여 정사각형을 떼어내어 부착성을 측정하였다. 이때, 측정된 부착성은 100개의 정사각형이 100% 온전히 붙어있는 경우 우수(◎), 남은 정사각형이 70% 이상 100% 미만인 경우 양호(○), 50% 이상 70% 미만인 경우 보통(△), 50% 미만인 경우 불량(×)으로 평가하였다. Specifically, in the checkerboard method, 100 squares of 2 mm in width and 2 mm in length were made on the surface of the final coating film with a knife, and then the squares were removed using tape to measure adhesion. At this time, the measured adhesion is excellent (◎) when 100 squares are 100% completely attached, good (○) when the remaining squares are between 70% and less than 100%, average (△) when the remaining squares are between 50% and 70%, and 50%. If it is less than that, it was evaluated as defective (×).
(5) 내스크래치성(5) Scratch resistance
광택기를 이용하여 최종 도막의 초기 20° 광택을 측정하고, 자동차 세차기인 Amtec Kistler를 이용하여 석영 파우더와 물을 분사하면서 10회 왕복 표면처리한 후 20° 광택을 측정했다. 표면처리 전의 광택을 기준으로 표면처리 후의 광택의 광택유지율을 계산했다. The initial 20° gloss of the final film was measured using a polisher, and the 20° gloss was measured after 10 reciprocating surface treatments while spraying quartz powder and water using an Amtec Kistler car wash machine. The gloss retention rate of the gloss after surface treatment was calculated based on the gloss before surface treatment.
이때, 광택 유지율이 70% 이상이면 우수(◎), 60% 이상 70% 미만이면 양호(○), 55% 이상 60% 미만이면 보통(△), 55% 미만이면 불량(×)으로 평가하였다.At this time, if the gloss retention was 70% or more, it was evaluated as excellent (◎), if it was 60% or more but less than 70%, it was evaluated as good (○), if it was 55% or more but less than 60%, it was evaluated as average (△), and if it was less than 55%, it was evaluated as poor (×).
표 5에서 보는 바와 같이, 실시예의 조성물로부터 제조된 도막은 핀홀 특성, 외관 특성, 광택, 재도장 부착성 및 내스크래치성이 모두 우수함을 알 수 있었다.As shown in Table 5, it was found that the coating film prepared from the composition of the example was excellent in all pinhole characteristics, appearance characteristics, gloss, recoating adhesion, and scratch resistance.
반면, 제1 폴리에스터 수지를 미포함하는 비교예 1은 핀홀 특성 및 내스크래치성이 부족했다.On the other hand, Comparative Example 1, which did not contain the first polyester resin, lacked pinhole characteristics and scratch resistance.
제2 폴리에스터 수지를 미포함하는 비교예 2는 외관 특성 및 광택이 부족했다.Comparative Example 2, which did not contain the second polyester resin, lacked appearance properties and gloss.
또한, 실리콘 변성 폴리에스터 수지를 미포함하는 비교예 3은 핀홀 특성 및 외관 특성이 부족했다.Additionally, Comparative Example 3, which did not contain silicone-modified polyester resin, lacked pinhole characteristics and appearance characteristics.
수산기가가 낮은 제1 폴리에스터 수지-4를 포함하는 비교예 4 및 유리전이온도가 낮은 제2 폴리에스터 수지-8을 포함하는 비교예 10은 재도장 부착성 및 내스크래치성이 부족했다.Comparative Example 4, including the first polyester resin-4 with a low hydroxyl value, and Comparative Example 10, including the second polyester resin-8 with a low glass transition temperature, lacked recoating adhesion and scratch resistance.
또한, 수산기가가 높은 제1 폴리에스터 수지-5를 포함하는 비교예 5 및 수산기가가 높은 제2 폴리에스터 수지-5를 포함하는 비교예 9는 외관 특성 및 내스크래치성이 부족했다. 특히, 비교예 9는 광택 및 재도장 부착성도 부족했다.In addition, Comparative Example 5 including the first polyester resin-5 with a high hydroxyl value and Comparative Example 9 including the second polyester resin-5 with a high hydroxyl value lacked appearance characteristics and scratch resistance. In particular, Comparative Example 9 lacked gloss and recoating adhesion.
유리전이온도가 낮은 제1 폴리에스터 수지-8을 포함하는 비교예 6 및 수산기가가 낮은 제2 폴리에스터 수지-4를 포함하는 비교예 8은 핀홀 특성, 재도장 부착성 및 내스크래치성이 부족했다.Comparative Example 6 including the first polyester resin-8 with a low glass transition temperature and Comparative Example 8 including the second polyester resin-4 with a low hydroxyl value lacked pinhole properties, recoating adhesion, and scratch resistance. did.
또한, 유리전이온도가 높은 제1 폴리에스터 수지-9를 포함하는 비교예 7 및 유리전이온도가 높은 제2 폴리에스터 수지-9를 포함하는 비교예 11은 핀홀 특성, 외관 특성 및 내스크래치성이 부족했다.In addition, Comparative Example 7 including the first polyester resin-9 having a high glass transition temperature and Comparative Example 11 including the second polyester resin-9 having a high glass transition temperature had pinhole characteristics, appearance characteristics, and scratch resistance. It wasn't enough.
Claims (6)
상기 제1 폴리에스터 수지는 수산기가가 220 내지 280 mgKOH/g이고, 유리전이온도가 18 내지 25 ℃이며, 중량평균분자량이 800 내지 1,500g/mol이고,
상기 제2 폴리에스터 수지는 수산기가가 100 내지 150 mgKOH/g이고, 유리전이온도가 3 내지 7 ℃이며, 중량평균분자량이 800 내지 1,600g/mol인, 클리어 코트 조성물.Based on the total weight of the composition, it contains 22 to 28% by weight of the first polyester resin, 17 to 23% by weight of the second polyester resin, 4 to 8% by weight of the silicone modified polyester resin, and 7 to 13% by weight of the melamine resin; ,
The first polyester resin has a hydroxyl value of 220 to 280 mgKOH/g, a glass transition temperature of 18 to 25 ℃, and a weight average molecular weight of 800 to 1,500 g/mol,
The second polyester resin has a hydroxyl value of 100 to 150 mgKOH/g, a glass transition temperature of 3 to 7° C., and a weight average molecular weight of 800 to 1,600 g/mol.
상기 제1 폴리에스터 수지는 산가가 15 내지 25 mgKOH/g이고,
상기 제2 폴리에스터 수지는 산가가 20 내지 30 mgKOH/g인, 클리어 코트 조성물.In claim 1,
The first polyester resin has an acid value of 15 to 25 mgKOH/g,
The clear coat composition wherein the second polyester resin has an acid value of 20 to 30 mgKOH/g.
상기 실리콘 변성 폴리에스터 수지는 산가가 10mgKOH/g 이하이고, 수산기가가 150 내지 250 mgKOH/g이며, 유리전이온도가 -20 내지 0 ℃이고, 25℃에서의 점도가 5,000 내지 10,000 cps 인, 클리어 코트 조성물.In claim 1,
The silicone-modified polyester resin has an acid value of 10 mgKOH/g or less, a hydroxyl value of 150 to 250 mgKOH/g, a glass transition temperature of -20 to 0 ℃, and a viscosity at 25 ℃ of 5,000 to 10,000 cps, clear Coat composition.
상기 조성물과 경화제를 2 내지 4 : 1의 중량비로 포함하고,
상기 경화제는 이소시아네이트계 화합물을 포함하는, 클리어 도료 키트.In claim 5,
The composition and the curing agent are included in a weight ratio of 2 to 4:1,
A clear paint kit wherein the curing agent includes an isocyanate-based compound.