Nothing Special   »   [go: up one dir, main page]

JPS61228946A - Composite blank for ornament - Google Patents

Composite blank for ornament

Info

Publication number
JPS61228946A
JPS61228946A JP7044685A JP7044685A JPS61228946A JP S61228946 A JPS61228946 A JP S61228946A JP 7044685 A JP7044685 A JP 7044685A JP 7044685 A JP7044685 A JP 7044685A JP S61228946 A JPS61228946 A JP S61228946A
Authority
JP
Japan
Prior art keywords
alloy
brazing
weight
composite material
clad
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP7044685A
Other languages
Japanese (ja)
Inventor
斉 辻
清一 川口
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tanaka Kikinzoku Kogyo KK
Original Assignee
Tanaka Kikinzoku Kogyo KK
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tanaka Kikinzoku Kogyo KK filed Critical Tanaka Kikinzoku Kogyo KK
Priority to JP7044685A priority Critical patent/JPS61228946A/en
Publication of JPS61228946A publication Critical patent/JPS61228946A/en
Pending legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
(57) [Summary] This bulletin contains application data before electronic filing, so abstract data is not recorded.

Description

【発明の詳細な説明】 (産業上の利用分野) 本発明は、眼鏡フレーム、時計側、時計バンド、ネック
レスなど用の複合素材の改良に係り、詳しくは複合素材
のクラッド複合強度が強く、且つろう付特性に優れた装
飾品用複合素材に関する。
DETAILED DESCRIPTION OF THE INVENTION (Field of Industrial Application) The present invention relates to improvements in composite materials for eyeglass frames, watch sides, watch bands, necklaces, etc. Specifically, the present invention relates to improvements in composite materials for eyeglass frames, watch sides, watch bands, necklaces, etc. Concerning composite materials for decorative items with excellent brazing properties.

(従来技術とその問題点) 近時、各種装飾品に於いて、活動性を高める意味から軽
量の装飾品が要望されている。
(Prior Art and its Problems) Recently, there has been a demand for lightweight ornaments among various ornaments in order to enhance activity.

このような要望に応えようとする装飾品用素材として、
最近Ti又はTi合金が使用されている。
As a material for decorative items that meets these demands,
Recently Ti or Ti alloys have been used.

しかしTi又はTi合金は、ろう付性が悪く、強い強度
を持たせる為には、高真空中或いは特殊な雰囲気の下で
ろう付を行う必要があり、この点での改善が望まれてい
た。
However, Ti or Ti alloys have poor brazing properties and must be brazed in a high vacuum or in a special atmosphere in order to have strong strength, and improvements in this respect have been desired. .

その1つの手段として、第3図に示す如< T i又は
Ti合金を芯材1とし、これの外側に耐食性が良く且つ
ろう付性に優れた材料2、例えばNi合金、Au合金、
白金族合金、ステンレス鋼などのいずれかをクラッドす
る方法が採られている。
As one means for this purpose, as shown in FIG. 3, a core material 1 is made of Ti or a Ti alloy, and a material 2 having good corrosion resistance and brazing properties, such as a Ni alloy, an Au alloy, etc.
A method of cladding with platinum group alloy, stainless steel, etc. has been adopted.

しかしこの方法に依ると、Ti又はTi合金の芯材1の
酸化或いは窒化が防げ、大気中で簡単にろう付が行える
という長所があるものの、この装飾品用複合素材3を圧
延して、板材4を作り、この板材4を第4図に示す如<
Agろう、Auろう等のろう材5を用いて600〜90
.0℃大気中で、ろう付すると、芯材lと外側の材料2
との界面に非常に脆いTi−Ni5 Tl −Au等の
金属間化合物6が生成されるので、ろう付後にこの金属
間化合物6の層から剥離するという致命的な欠点があっ
た。
However, although this method has the advantage of preventing the oxidation or nitridation of the Ti or Ti alloy core material 1 and allowing easy brazing in the atmosphere, the decorative composite material 3 is rolled and made into a sheet material. 4 and this plate material 4 as shown in Fig. 4.
600 to 90 using a brazing material 5 such as Ag wax or Au wax
.. When brazing in the atmosphere at 0℃, the core material 1 and the outer material 2
Since a very brittle intermetallic compound 6 such as Ti--Ni5 Tl--Au is formed at the interface with the metal, there is a fatal drawback that the intermetallic compound 6 peels off from the layer after brazing.

(発明の目的) 本発明は斯かる欠点を解消すべくなされたもので、大気
中でろう付が可能で、しかもろう付強度が著しく高くそ
の上外側の材料とが剥離する事のない装飾品用複合素材
を提供せんとするものである。
(Object of the Invention) The present invention was made in order to eliminate such drawbacks, and provides a decorative product that can be brazed in the atmosphere, has extremely high brazing strength, and does not peel off from the upper and outer materials. The aim is to provide composite materials for use in

(発明の構成) 本発明の装飾品用複合素材は、第1図に示す如<Agま
たはSnめっきの施されたTi又はTi合金lに、これ
の外側にCu2,5〜50重量%とSn0.01〜10
重量%を含むAg合金が中間層7としてクラッドされ、
この中間層7の外側に耐食性が良く且つろう付性に優れ
た材料2、例えばNi合金、Au合金、白金族合金、ス
テンレス鋼などのいずれかがクラッドされてなるもので
ある。
(Structure of the Invention) As shown in FIG. 1, the composite material for decorative articles of the present invention consists of Ti or Ti alloy l plated with Ag or Sn, and on the outside thereof 5 to 50% by weight of Cu and Sn0. .01~10
% by weight of Ag alloy is clad as the intermediate layer 7,
The outer side of the intermediate layer 7 is clad with a material 2 having good corrosion resistance and excellent brazing properties, such as a Ni alloy, an Au alloy, a platinum group alloy, or stainless steel.

ここで中間層としてAg合金を用いたのはろう付の際の
熱ひずみをAgが緩和するからである。
The reason why an Ag alloy was used as the intermediate layer here is that Ag relieves thermal strain during brazing.

更にCuを添加するのはTiあるいは耐食性材料とCu
が優先的に拡散結合し、特にCu−Tiは脆くなくろう
付後の剥離が防げるからである。
Furthermore, Cu is added to Ti or corrosion-resistant material and Cu.
This is because Cu-Ti is not brittle and peeling after brazing can be prevented.

Cuを2.5〜50重量%と限定したのは2.5重量%
未満ではCuが優先結合してCu−Ti層を形成するに
十分でなく、50重量%を超えると、熱緩和材としての
Ag層が少なくなり熱ひずみにより剥離が生ずるからで
ある。
The Cu content is limited to 2.5 to 50% by weight, which is 2.5% by weight.
If it is less than 50% by weight, it is not sufficient for Cu to bond preferentially to form a Cu-Ti layer, and if it exceeds 50% by weight, the Ag layer as a thermal relaxation material will decrease and peeling will occur due to thermal strain.

更にSnを添加する理由は、ろう付温度を上げすぎた場
合のCu−’[”i層の異常成長を妨げ剥離が生ずるの
を防止するためである。これはTiとSnがCuとTi
よりも優先的に結合し、5n−Tiの固溶体を形成し、
この合金が成長しても脆くないからである。Snの量を
0.01〜10重量%とじたのは、o、oi重量%未満
ではその効果がなく、10重量%をこえると加工困難と
なるからである。
The reason why Sn is further added is to prevent abnormal growth of the Cu-'["i layer and prevent peeling if the brazing temperature is raised too high. This is because Ti and Sn
binds preferentially to form a solid solution of 5n-Ti,
This is because this alloy is not brittle even when it grows. The reason why the amount of Sn is limited to 0.01 to 10% by weight is that if it is less than o or oi% by weight, there is no effect, and if it exceeds 10% by weight, it becomes difficult to process.

またAgまたはSnめっきの施されたTiまたはTi合
金を用いるのは、複合素材の製造工程中におけるTiの
酸化を防止し、接合強度の高い複合素材を得るためであ
る。
Furthermore, the reason for using Ti or Ti alloy plated with Ag or Sn is to prevent oxidation of Ti during the manufacturing process of the composite material and to obtain a composite material with high bonding strength.

次に本発明の装飾品用複合素材の効果を明瞭にする為に
具体的な実施例と従来例について説明する。
Next, in order to clarify the effects of the composite material for decorative articles of the present invention, specific examples and conventional examples will be described.

(実施例1) 直径471IllのTiの棒材にSnめっきを5μ施し
、これにλg−CulO重量%−5n2重量%合金を被
せ、その上に、内周面にNiめっきを5μ施したNi−
CrlO%合金パイプを被せ、押出し、引抜加工等によ
り、第1図に示す如く、Tiを直径3IIImの芯材1
とし、これの外側に厚さ0.017mmのAg−Cu−
3n合金を中間層7としてクラッドし、この中間層7の
外側に厚さ0.25mmのNi−Cr合金2をクラッド
して装飾品用複合素材3′と成し、これを圧延して0.
75mm厚の板材4′を作り、この板材4′を第2図に
示す如<Ag−Cu28重量%のろう材5を用いて83
0℃大気中でろう付してテストピースを得た。
(Example 1) A Ti bar with a diameter of 471 Ill was coated with 5 μm of Sn plating, covered with a λg-CulO wt%-5n2 wt.
Covering with a CrlO% alloy pipe and extruding or drawing, as shown in Fig. 1, Ti is made into a core material 1 with a diameter of 3IIIm.
Ag-Cu- with a thickness of 0.017 mm is placed on the outside of this.
A 3n alloy is clad as the intermediate layer 7, and a 0.25 mm thick Ni-Cr alloy 2 is clad on the outside of the intermediate layer 7 to form a composite material 3' for ornaments, which is rolled to form a 0.25 mm thick Ni-Cr alloy 2.
A plate material 4' with a thickness of 75 mm is made, and this plate material 4' is 83 mm thick using a brazing material 5 containing 28% by weight of Ag-Cu as shown in FIG.
A test piece was obtained by brazing in the atmosphere at 0°C.

(実施例2) 直径41mmのTi−A13重景重景72重量%合金棒
材にAgめっきを5μ施し、これにAg−Cu5重量%
−S n 1.5重量%合金を被せ、その上にAu−A
g25重量%−Cu25重量%合金を被せ、押出し、引
抜加工等により、第1図に示す如く、Ti合金を直径3
mmの芯材1とし、これの外側にAg−Cu−3n合金
を中間層7としてクラドし、この中間層7の外側に厚さ
0.25mmのAu−Ag−Cu合金2をクラッドして
装飾品用複合素材3′と成し、これを圧延して0.75
mn+厚の板材4゛を作り、この板材4′を第2図に示
す如くAg−Cu2O重量%のろう材5を用いて830
℃大気中でろう付してテストピースを得た。
(Example 2) A Ti-A13 72% by weight alloy rod with a diameter of 41 mm was plated with 5μ of Ag, and this was coated with 5% by weight of Ag-Cu.
-S n 1.5% by weight alloy is covered, and Au-A is placed on top of it.
As shown in Figure 1, the Ti alloy is coated with a 25% g25%-Cu25% alloy and extruded or drawn to form a Ti alloy with a diameter of 3%.
A core material 1 with a thickness of 1 mm is used, an Ag-Cu-3n alloy is clad on the outside as an intermediate layer 7, and an Au-Ag-Cu alloy 2 with a thickness of 0.25 mm is clad on the outside of this intermediate layer 7 for decoration. Composite material for products 3' is made and rolled to 0.75
A plate material 4' with a thickness of mn+ is made, and this plate material 4' is 830 mm thick using a brazing material 5 of Ag-Cu2O weight% as shown in Fig. 2.
A test piece was obtained by brazing in the atmosphere at ℃.

(従来例) 直径49mmのTi棒材にNi−CrlO重量%合金を
被せ、押出し、引抜加工等により、第3図に示す如く、
Tiを直径3mmの芯材1とし、これの外側に厚さ0.
25mのNi−Cr合金2をクラッドして装飾品用複合
素材3と成し、これを圧延して0.75mm厚の板材4
を作り、この板材4を第4図に示す如<Ag−Cu28
重量%のろう材5を用いて830℃大気中でろう付しテ
ストピースを得た。
(Conventional Example) A Ni-CrlO wt% alloy was covered with a Ti bar having a diameter of 49 mm, and by extrusion, drawing, etc., as shown in Fig. 3,
A Ti core material 1 with a diameter of 3 mm is used, and a thickness of 0.0 mm is placed on the outside of this core material 1.
A 25 m long Ni-Cr alloy 2 is clad to form a composite material 3 for decorative items, and this is rolled to form a plate material 4 with a thickness of 0.75 mm.
This plate material 4 is made of <Ag-Cu28> as shown in Fig. 4.
A test piece was obtained by brazing at 830° C. in the atmosphere using a brazing filler metal of 5% by weight.

然して実施例1.2及び従来例のテストピースを引っ張
り試験した処、下表に示すような結果を得た。柱相呵弁
弁 *試験個数 : 5個 上表で明らかなように実施例1.2のテストピースは従
来例のテストピースに比し、破断強度が著しく高く、接
合強度が高いことが判る。また従来例のテストピースは
芯材1と外側の材料2との接合面が破断面であったのに
対し実施例のテストピースは母材が破断面で、芯材lと
外側の材料2との接合強度が高いことが判る。
However, when the test pieces of Example 1.2 and the conventional example were subjected to a tensile test, the results shown in the table below were obtained. Pillar phase valve *Number of test pieces: 5 As is clear from the table above, the test piece of Example 1.2 has significantly higher breaking strength and bonding strength than the conventional test piece. In addition, in the test piece of the conventional example, the joint surface between the core material 1 and the outer material 2 was a fracture surface, whereas in the test piece of the example, the base material was a fracture surface, and the joint surface between the core material 1 and the outer material 2 was a fracture surface. It can be seen that the bonding strength is high.

(発明の効果) 以上詳記した通り本発明の装飾品用複合素材は、大気中
でろう付が可能でろう付作業性に優れ、しかもろう付は
強度が著しく高く、その上TiまたはTi合金と外側の
耐食性材料とが剥離することが無いので、耐久性、機能
性に優れ、軽量装飾品用複合素材としては画期的なもの
と云える。
(Effects of the Invention) As detailed above, the composite material for ornaments of the present invention can be brazed in the atmosphere, has excellent brazing workability, has extremely high brazing strength, and is made of Ti or Ti alloy. Since the material and the outer corrosion-resistant material do not peel off, it has excellent durability and functionality, and can be said to be an epoch-making composite material for lightweight decorative items.

【図面の簡単な説明】[Brief explanation of the drawing]

第1図は本発明の装飾品用複合素材の断面図、第2図は
その複合素材を圧延して得た板材をろう付して得たテス
トピースの断面図、第3図は従来の装飾品用複合素材の
断面図、第4図はその複合素材を圧延して得た板材をろ
う付して得たテストピースの断面図である。 出願人  田中貴金属工業株式会社 第1図 第3図 第2図 第4図
Fig. 1 is a cross-sectional view of the composite material for decorative articles of the present invention, Fig. 2 is a cross-sectional view of a test piece obtained by brazing plates obtained by rolling the composite material, and Fig. 3 is a cross-sectional view of a conventional decorative material. FIG. 4 is a sectional view of a test piece obtained by brazing a plate obtained by rolling the composite material. Applicant Tanaka Kikinzoku Kogyo Co., Ltd. Figure 1 Figure 3 Figure 2 Figure 4

Claims (1)

【特許請求の範囲】[Claims] AgまたはSnめっきの施されたTiまたはTi合金に
、Cu2.5〜50重量%とSn0.01〜10重量%
を含むAg合金が中間層としてクラッドされ、外側に耐
食性材料がクラッドされていることを特徴とする装飾品
用複合素材。
2.5-50% by weight of Cu and 0.01-10% by weight of Sn on Ti or Ti alloy plated with Ag or Sn
A composite material for decorative items, characterized in that the intermediate layer is clad with an Ag alloy containing , and the outer layer is clad with a corrosion-resistant material.
JP7044685A 1985-04-03 1985-04-03 Composite blank for ornament Pending JPS61228946A (en)