JPS641281B2 - - Google Patents
Info
- Publication number
- JPS641281B2 JPS641281B2 JP11536279A JP11536279A JPS641281B2 JP S641281 B2 JPS641281 B2 JP S641281B2 JP 11536279 A JP11536279 A JP 11536279A JP 11536279 A JP11536279 A JP 11536279A JP S641281 B2 JPS641281 B2 JP S641281B2
- Authority
- JP
- Japan
- Prior art keywords
- decorative
- core material
- irregularities
- unevenness
- board
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired
Description
【発明の詳細な説明】
この発明は、凹凸付きの化粧板の製法に関する
ものである。DETAILED DESCRIPTION OF THE INVENTION The present invention relates to a method for manufacturing a decorative board with irregularities.
表面に多数の凹凸をもつ凹凸付きの化粧板は、
これまでつぎのようにして製造されていた。すな
わち、厚物合板、パーテイクルボード、むく材
(板)等の剛性を有する芯材の表面をNCルータ
ー等で加工して凹凸状にしたのち、その凹凸に沿
つて化粧単板を貼着することにより製造されてい
た。しかしながら、このようにして凹凸付きの化
粧板を製造する場合は、ルーター加工に手間がか
かるため、得られる製品のコストが高くなるとい
う欠点があつた。 The textured decorative board has many unevenness on its surface.
Until now, it has been manufactured as follows. In other words, the surface of a rigid core material such as thick plywood, particle board, or wood (board) is processed using an NC router to create an uneven shape, and then a decorative veneer is pasted along the unevenness. It was manufactured by. However, when producing a decorative board with irregularities in this manner, the router process is time-consuming, so the cost of the resulting product is high.
この発明は、このような事情に鑑みなされたも
ので、剛性を有する芯材の表面に、木部破壊を生
じさせうる圧力を部分的に加えることにより凹凸
を形成し、この凹凸が形成された芯材の表面に凹
凸に沿つて薄い化粧材を貼着することにより凹凸
付きの化粧板を得ることをその要旨とするもので
ある。 This invention was made in view of these circumstances, and involves forming unevenness on the surface of a rigid core material by partially applying pressure that can cause xylem breakage. The gist of this method is to obtain a decorative board with irregularities by attaching a thin decorative material to the surface of a core material along the irregularities.
すなわち、この発明者の見出したところによれ
ば、芯材の表面に部分的に、木部破壊を生じさせ
うる圧力を加えると、その部分では繊維配列が破
壊されて復元性が失われるため、圧力を取り去つ
たあとに所望の凹凸が生じる。厚物合板、パーテ
イクルボード、むく材等の剛性を有する芯材は、
インシユレーシヨンボードやセミハードボードの
ごとき軟性材と異なりプレス成形できないと言う
のが従来の常識であつたが、この発明者の見出し
たところによれば、「木部破壊を生じさせうる圧
力を部分的に加える」と言う特殊の加圧加工によ
り、剛性材に対して所望の凹凸加工を加圧成形に
より施すことが可能となつたのである。そのた
め、この凹凸に沿つて化粧材を貼着することによ
り容易に凹凸付きの化粧板が得られるようになる
のである。なお、ここで、芯材とは、化粧板のベ
ース材としての意味を持つものであり、心材
(heartwood)とは異なる。心材は、丸太材の中
心部分であり、小径木時の材を示す語である。ま
た、剛性とは、加圧に対する強度、すなわち、圧
縮強度を意味する。上記剛性材は、ある加圧以上
では、木材繊維や種々の組織により構成された空
間がつぶされ、木部破壊が生じる。剛性材の圧縮
強度は、たとえば80〜400Kg/cm2程度である。こ
れに対し、上記軟性材は、繊維を解繊したものを
抄造したもので、加圧に従つて次第に変形してい
き、木部破壊を生じないと言つて良く、強いて言
えば、繊維の絡みとわずかのバインダーによる応
力が生じる程度である。軟性材を帯に圧縮変形さ
せうる加圧力は、5〜50Kg/cm2程度である。 That is, according to the findings of the inventor, when pressure that can cause xylem destruction is applied to a portion of the surface of the core material, the fiber arrangement is destroyed in that portion and the restorability is lost. After the pressure is removed, the desired irregularities occur. Rigid core materials such as thick plywood, particle board, and peeled wood are
It was conventional wisdom that unlike soft materials such as insulation boards and semi-hard boards, press forming was not possible, but the inventor discovered that By using a special pressure process called "partial addition", it became possible to apply the desired unevenness to a rigid material by pressure forming. Therefore, by pasting the decorative material along the unevenness, a decorative board with unevenness can be easily obtained. Note that the core material here has the meaning of a base material for the decorative board, and is different from heartwood. Heartwood is the central part of a log, and is a term used to describe small-diameter wood. Moreover, rigidity means strength against pressurization, that is, compressive strength. When the above-mentioned rigid material is pressurized to a certain level or higher, the space formed by the wood fibers and various tissues is crushed, resulting in xylem destruction. The compressive strength of the rigid material is, for example, about 80 to 400 kg/cm 2 . On the other hand, the above-mentioned soft materials are made from fibers that have been defibrated, so they gradually deform as pressure is applied, and it can be said that the wood does not break. This is only a slight stress caused by the binder. The pressing force capable of compressively deforming the soft material into a band is about 5 to 50 kg/cm 2 .
剛性を有する芯材(以下、「芯材」とのみ記す)
の表面に木部破壊を生じさせうる圧力を部分的に
加えることにより凹凸を形成することは、通常、
押圧面に多数の凹凸をもつ金型を芯材の表面に置
き、この金型を加圧することにより行われる。す
なわち、第1図に示すように、芯材1を平坦な下
金型2上に置き、芯材1の表面に、押圧面に凹凸
をもつ上金型3を対面させ、その状態から上金型
3を下降させて木部破壊を生じさせうる圧力で加
圧する。ついで、上金型3を上昇させる。その結
果、第2図に示すように、芯材1の表面に多数の
凹凸が形成される。この場合、芯材1としては、
前記のような厚物合板、バーテイクルボード、む
く材等の通常使用されているものが用いられる。 Core material with rigidity (hereinafter referred to only as "core material")
The formation of irregularities by locally applying pressure that can cause xylem failure to the surface of
This is done by placing a mold with a large number of depressions and depressions on the pressing surface on the surface of the core material, and applying pressure to this mold. That is, as shown in FIG. 1, a core material 1 is placed on a flat lower mold 2, an upper mold 3 having an uneven pressing surface is made to face the surface of the core material 1, and from this state the upper mold is placed. The mold 3 is lowered and pressurized with a pressure that can cause xylem destruction. Then, the upper mold 3 is raised. As a result, as shown in FIG. 2, many irregularities are formed on the surface of the core material 1. In this case, as the core material 1,
Commonly used materials such as thick plywood, verteckle board, and timber as described above are used.
つぎに、多数の凹凸が形成された芯材1の表面
に、その凹凸に沿つて薄い化粧材(図示せず)を
貼着する。この貼着は、通常、真空プレスを用
い、薄い化粧材を、芯材1表面の多数の凹凸に沿
つて接着することにより行われる。薄い化粧材と
しては、通常、化粧単板が用いられるが、これに
限定するものではない。 Next, a thin decorative material (not shown) is adhered to the surface of the core material 1 on which many irregularities are formed along the irregularities. This adhesion is usually performed by adhering a thin decorative material along the many irregularities on the surface of the core material 1 using a vacuum press. As a thin decorative material, a decorative veneer is usually used, but it is not limited to this.
このようにして凹凸付きの化粧板(図示せず)
が得られる。この化粧板は、芯材1に形成された
凹凸が、木部破壊を生じさせうる圧力を加えるこ
とにより形成されており、その繊維配列が破壊さ
れていて復元性がないため、吸湿、吸水等によつ
ても凹凸の形状が変化しない。したがつて寸法変
化が起こらない優れたものである。さらに、芯材
1に形成された上記凹凸は、化粧材貼着後も、化
粧板の表面において、コーナー部が鋭角的で、深
く、くつきりとした立体模様を現出するようにな
つている。 In this way, a decorative board with unevenness (not shown)
is obtained. This decorative board is formed by applying pressure that can cause the unevenness formed on the core material 1 to break the wood, and the fiber arrangement is destroyed and there is no restorability, so it absorbs moisture and water. The shape of the unevenness does not change even if Therefore, it is excellent in that dimensional changes do not occur. Further, the unevenness formed on the core material 1 is such that even after the decorative material is attached, a deep, tight three-dimensional pattern with sharp corners appears on the surface of the decorative board. .
以上のように、この発明は、芯材の表面に、木
部破壊を生じさせうる圧力を部分的に加えること
により凹凸を形成し、この凹凸が形成された芯材
の表面に凹凸に沿つて薄い化粧材を貼着すること
により凹凸付きの化粧板を得るため、凹凸の形成
が簡単であり、コストダウンを実現することがで
きる。また、芯材の表面に、木部破壊を生じさせ
うる圧力を部分的に加えることにより凹凸を形成
することを、芯材の表面に、押圧面に凹凸をもつ
金型を置き、この金型を加圧することにより行う
ときは、同形の多数の凹凸を1動作で形成するこ
とができるという効果がある。 As described above, the present invention forms irregularities on the surface of the core material by partially applying pressure that can cause xylem breakage, and then applies pressure along the irregularities to the surface of the core material on which the irregularities are formed. Since a decorative board with irregularities is obtained by pasting a thin decorative material, it is easy to form irregularities, and costs can be reduced. In addition, a mold with an uneven pressing surface is placed on the surface of the core material to form unevenness by partially applying pressure that can cause xylem breakage. When this is done by applying pressure, there is an effect that a large number of concave and convex portions of the same shape can be formed in one operation.
つぎに、実施例について説明する。 Next, examples will be described.
〔実施例 1〕
厚みが15mmの合板を平坦な下金型に載せ、合板
の表面に、押圧面に凹凸をもつ上金型を置き、こ
の上金型を水圧プレスにより150Kg/cm2に加圧し、
合板の表面側の部分に木部破壊を生じさせて多数
の凹凸を形成した。つぎに、合板の表面に酢酸ビ
ニル系接着剤を塗布し、その上に厚みが0.15mmの
天然銘木単板調の化粧単板を置き、真空プレスに
より減圧して化粧単板を合板表面の凹凸に沿わせ
て貼着した。このようにして簡単に凹凸付きの化
粧板を得た。[Example 1] Plywood with a thickness of 15 mm was placed on a flat lower mold, an upper mold with an uneven pressing surface was placed on the surface of the plywood, and this upper mold was pressurized to 150 kg/cm 2 using a hydraulic press. Press,
The wood was destroyed on the surface side of the plywood, creating many uneven surfaces. Next, apply vinyl acetate adhesive to the surface of the plywood, place a 0.15 mm thick decorative veneer that looks like a natural wood veneer on top of it, and reduce the pressure with a vacuum press to apply the decorative veneer to the uneven surface of the plywood. I pasted it along the In this way, a decorative board with unevenness was easily obtained.
〔実施例 2〕
厚みが20mmのパーテイクルボードを平坦な下金
型上に置き、ボードの表面に押圧面に凹凸をもつ
上金型を置き、この上金型を、木部破壊を生じさ
せうる200Kg/cm2の圧力で加熱しながら加圧し、
ボードの表面に多数の凹凸を形成した、つぎに、
ボードの表面にゴム系接着剤を塗布し、その上に
厚みが0.20mmの天然銘木単板調の化粧単板を置
き、ゴムローラにより加圧して化粧単板をボード
表面の凹凸に沿わせて貼着した。このようにして
簡単に凹凸付きの化粧板を得た。[Example 2] Particle board with a thickness of 20 mm was placed on a flat lower mold, and an upper mold with an uneven pressing surface was placed on the surface of the board, and this upper mold was used to cause wood breakage. Heat and pressurize at a pressure of 200Kg/ cm2 ,
After forming many irregularities on the surface of the board,
Apply rubber adhesive to the surface of the board, place a 0.20 mm thick decorative veneer made of natural wood veneer on top of it, and apply pressure with a rubber roller to stick the decorative veneer along the unevenness of the board surface. I arrived. In this way, a decorative board with unevenness was easily obtained.
第1図および第2図は、この発明に用いる芯材
に、凹凸を形成する説明図である。
1……芯材、2……下金型、3……上金型。
FIGS. 1 and 2 are explanatory views of forming irregularities on the core material used in the present invention. 1...Core material, 2...Lower mold, 3...Upper mold.
Claims (1)
させうる圧力を部分的に加えることにより凹凸を
形成し、この凹凸が形成された芯材の表面に凹凸
に沿つて薄い化粧材を貼着することにより凹凸付
きの化粧板を得ることを特徴とする化粧板の製
法。 2 芯材の表面に、木部破壊を生じさせうる圧力
を部分的に加えることにより凹凸を形成すること
を、芯材の表面に、押圧面に凹凸をもつ金型を置
き、この金型を加圧することにより行う特許請求
の範囲第1項記載の化粧板の製法。 3 化粧材が、化粧単板である特許請求の範囲第
1項または第2項記載の化粧板の製法。[Scope of Claims] 1. Unevenness is formed on the surface of a core material having rigidity by partially applying pressure capable of causing xylem breakage, and the surface of the core material on which the irregularities are formed is provided along the irregularities. A method for manufacturing a decorative board characterized by obtaining a decorative board with unevenness by pasting a thin decorative material. 2. A mold with an uneven pressing surface is placed on the surface of the core material, and this mold is A method for manufacturing a decorative laminate according to claim 1, which is carried out by applying pressure. 3. The method for manufacturing a decorative board according to claim 1 or 2, wherein the decorative material is a decorative veneer.