Nothing Special   »   [go: up one dir, main page]

JPS5953368B2 - Method for manufacturing polyester staple with excellent spinnability - Google Patents

Method for manufacturing polyester staple with excellent spinnability

Info

Publication number
JPS5953368B2
JPS5953368B2 JP13664576A JP13664576A JPS5953368B2 JP S5953368 B2 JPS5953368 B2 JP S5953368B2 JP 13664576 A JP13664576 A JP 13664576A JP 13664576 A JP13664576 A JP 13664576A JP S5953368 B2 JPS5953368 B2 JP S5953368B2
Authority
JP
Japan
Prior art keywords
polyester
spinning
temperature
yarn
heat
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
JP13664576A
Other languages
Japanese (ja)
Other versions
JPS5361719A (en
Inventor
誠 斉藤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kanebo Ltd
Original Assignee
Kanebo Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kanebo Ltd filed Critical Kanebo Ltd
Priority to JP13664576A priority Critical patent/JPS5953368B2/en
Publication of JPS5361719A publication Critical patent/JPS5361719A/en
Publication of JPS5953368B2 publication Critical patent/JPS5953368B2/en
Expired legal-status Critical Current

Description

【発明の詳細な説明】 本発明は紡績性の優れたポリエステルステーブルの製造
方法に関する。
DETAILED DESCRIPTION OF THE INVENTION The present invention relates to a method for producing a polyester stable with excellent spinnability.

ポリエステル系繊維特にポリエチレンテレフタレート繊
維は天然繊維或は他の合成繊維と比較して優れた物理的
性質を有しており、衣料分野及び産業分野に於いて広範
囲に使用されている。
Polyester fibers, particularly polyethylene terephthalate fibers, have superior physical properties compared to natural fibers or other synthetic fibers, and are widely used in the clothing and industrial fields.

特にポリエチレンテレフタレートステープルは単独或は
綿・レーヨン・麻等他の繊維と混紡して主として衣料分
野に供されているが、紡績時、装置の摩耗が激しく、装
置寿命を大巾に短縮し、又精紡工程に於ては著しい量の
白粉を発生し、糸切れ或は品質の低下更には清掃頻度の
増加ならびに作業環境の悪化等操業上着しい支障をきた
している。
In particular, polyethylene terephthalate staples are mainly used in the clothing field either alone or blended with other fibers such as cotton, rayon, and linen, but during spinning, the equipment is subject to severe wear, which greatly shortens the life of the equipment. The spinning process generates a significant amount of white powder, which causes serious operational problems such as yarn breakage, deterioration of quality, increased cleaning frequency, and deterioration of the working environment.

例えば紡績工程に於いて、カードのテーカ−イン、ガー
ネットワイヤー、シリンダー、ドツファのメタリックワ
イヤー、トップ針布、或は線条はしめ各機のローラー、
各種ガイド等が短期間で摩耗し、特に空気精紡機の場合
にはコーミングワイヤーとしてビッカース硬度3000
のものを使用してもポリエステル65/綿35の混紡率
に於て6〜8ケ月程度で交換する必要を生じポリエステ
ルステープル旬0%による紡績は殆んど行なわれていな
い状況にある。
For example, in the spinning process, the taker-in of the card, the garnet wire, the cylinder, the metallic wire of the drawer, the top clothing, or the roller of each line tightening machine,
Various guides wear out in a short period of time, and especially in the case of air spinning machines, the combing wire has a Vickers hardness of 3000.
Even if a polyester staple is used, it has to be replaced every six to eight months due to the blend ratio of 65 polyester/35 cotton, and spinning with 0% polyester staple is hardly ever carried out.

又精紡工程に於ては空気精紡機の場合ローター内に粉砕
された繊維片が堆積して糸切れを生ぜしめ又リング精紡
機の場合、リングレール上に著しい量の白粉が付着して
作業環境を低下し、清掃頻度の増大に伴なうコストアッ
プ等の支障をきたしている。
In addition, in the spinning process, in the case of an air spinning machine, crushed fiber pieces accumulate in the rotor and cause yarn breakage, and in the case of a ring spinning machine, a significant amount of white powder adheres to the ring rail, making it difficult to operate. This is causing problems such as degrading the environment and increasing costs due to increased cleaning frequency.

従来、該問題点を改良してポリエステルステーブルの紡
績操業性を向上させるために原綿の捲縮形態、捲縮の堅
牢性或は紡績用油剤等積々の改良方法が提案されてきた
Conventionally, in order to improve the spinning operability of polyester stable by solving these problems, a number of methods have been proposed to improve the crimp form of raw cotton, the fastness of crimp, the spinning oil agent, etc.

しかし何れの方法によっても満足する効果が得られず紡
績操業性ならびに品質の優れたポリエステルステーブル
及びその製造方法が要望されている。
However, no satisfactory effect can be obtained by any of these methods, and there is a need for a polyester stable with excellent spinning operability and quality, and a method for producing the same.

本発明者等は上記問題点を解消すべく、全く別の観点か
ら鋭意研究を行ない本発明を完成したものである。
In order to solve the above-mentioned problems, the present inventors conducted intensive research from a completely different viewpoint and completed the present invention.

すなわち、本発明は相対粘度が1.20乃至1.45の
ポリエステル繊維中に分子量20.000以下のポリ有
機シロキサンを0.05乃至2.0重量%含有し且つ該
繊維表面に該ポリ有機シロキサンの被膜を有しで捲縮し
てなることを特徴とする紡績性の優れたポリエステルス
テープルを提供するものであって、本発明方法は相対粘
度が1.20乃至1.45のポリエステル中に分子量2
0.000以下のポリ有機シロキサンを0.05乃至2
.0重量%含有せしめて溶融紡糸しローラ一温度65℃
乃至85℃で延伸を行ない次にローラ一温度160℃乃
至195℃でヒートセットした後捲縮を付与して90℃
乃至130℃の温度雰囲気中で熱処理し、冷却した後切
断することを特徴とする。
That is, in the present invention, polyester fibers having a relative viscosity of 1.20 to 1.45 contain 0.05 to 2.0% by weight of polyorganosiloxane having a molecular weight of 20.000 or less, and the polyorganosiloxane is coated on the surface of the fiber. The method of the present invention provides a polyester staple with excellent spinnability characterized by having a coating film of 1.20 to 1.45 and having a molecular weight of 2
0.000 or less polyorganosiloxane from 0.05 to 2
.. Melt-spun with 0% by weight content, roller temperature 65℃
Stretching is performed at a temperature of 85°C to 85°C, then heat set at a roller temperature of 160°C to 195°C, and then crimped and stretched to 90°C.
It is characterized in that it is heat treated in an atmosphere at a temperature of 130°C to 130°C, cooled, and then cut.

本発明に於けるポリエステルとは酸成分としてテレフタ
ール酸、グリコール成分としてエチレングリコールを用
いた繊維形成用ポリエチレンテレフタレートを主体とし
て、ポリマー中の85モル%以上好ましくは90モル%
以上がポリエチレンテレフタレートであるポリエステル
である。
The polyester in the present invention is mainly composed of polyethylene terephthalate for fiber formation using terephthalic acid as the acid component and ethylene glycol as the glycol component, and is 85 mol% or more, preferably 90 mol% in the polymer.
The above is the polyester which is polyethylene terephthalate.

テレフタール酸或はエチレングリコールの一部をβ−ヒ
ドロキシエトキシ安息香酸、ヒドロキシ安息香酸、イソ
フタル酸、ジフェニルスルホンジカルボン酸、ジフェニ
ルメタンジカルボン酸、ジフェニルエーテルジカルボン 酸、ジフェノキシエタンジカルボン酸、ナトリウムスル
ホキシイソフタル ン酸、アジピン酸、セパチン酸等のオキシ酸又は二塩基
酸、更にトリメチレングリコール、テトラメチレングリ
コール、ヘキサメチレングリコール、フ冶ピレングリコ
ール、1,4−シクロヘキサンジオール、1,4−シク
ロヘキサンジメタツール、1,4−ビスヒドロキシエト
キシベンゼン、ビスフェノールA、ポリエチレングリコ
ール等の脂肪族、脂環族のジオキシ化合物の一種又は二
種以上と置換せるポリエチレンテレフタレートを主成分
とする繊維形成用変性ポリエステルを含むものである。
Part of terephthalic acid or ethylene glycol can be converted into β-hydroxyethoxybenzoic acid, hydroxybenzoic acid, isophthalic acid, diphenylsulfone dicarboxylic acid, diphenylmethane dicarboxylic acid, diphenyl ether dicarboxylic acid, diphenoxyethane dicarboxylic acid, sodium sulfoxyisophthalic acid, Oxyacids or dibasic acids such as adipic acid and sepatic acid, as well as trimethylene glycol, tetramethylene glycol, hexamethylene glycol, pyrene glycol, 1,4-cyclohexanediol, 1,4-cyclohexane dimetatool, 1, It contains a modified polyester for fiber formation whose main component is polyethylene terephthalate which can be substituted with one or more aliphatic or alicyclic dioxy compounds such as 4-bishydroxyethoxybenzene, bisphenol A, and polyethylene glycol.

又該ポリエステルに艶消剤、耐光剤、静電防止剤、難燃
剤、顔料等の添加物を適宜含有せしめてもよい。
Further, the polyester may contain additives such as a matting agent, a light-fastening agent, an antistatic agent, a flame retardant, and a pigment as appropriate.

本発明に特に好適なるポリエステルは上記ポリエチレン
テレフタレートを主成分とするポリエステル中にペンタ
エリスリトール、トリメチロールプロパン、グリセリン
等の如き多価アルコール、或はトリメリット酸、ピロメ
リット酸等の如き少なくとも3個のカルボキシル基を有
するポリカルボン酸等の分岐剤を0.02〜1.0モル
%好ましくは0、05〜0.5モル%共重合せしめてな
るポリエステルである。
Particularly suitable polyesters for the present invention include polyhydric alcohols such as pentaerythritol, trimethylolpropane, glycerin, etc., or at least three alcohols such as trimellitic acid, pyromellitic acid, etc., in the polyester mainly composed of polyethylene terephthalate. It is a polyester obtained by copolymerizing 0.02 to 1.0 mol %, preferably 0.05 to 0.5 mol % of a branching agent such as a polycarboxylic acid having a carboxyl group.

該分岐剤のうち特にペンタエリスリトール、トリメリッ
ト酸が好適なる融点及び反応性等の点で好ましい。
Among these branching agents, pentaerythritol and trimellitic acid are particularly preferred in view of their favorable melting point and reactivity.

該分岐剤ならびにポリ有機シロキサンを含有するポリエ
ステルステープルは紡績時装置との摩擦による白粉の発
生ならびに装置の摩耗を著しく抑制すると共に優れた抗
ピリング性を付与するものである。
The polyester staple containing the branching agent and polyorganosiloxane significantly suppresses the generation of white powder due to friction with spinning equipment and wear of the equipment, and provides excellent anti-pilling properties.

ポリエステル中に共重合せしめる前記分岐剤が0、02
モル%未満の場合、抗ピリング効果が得られず、又1.
0モル%を超えた場合は溶融粘度の上昇により紡糸が困
難となるため、上記範囲に従うことが好ましい。
The branching agent copolymerized into the polyester is 0,02
If it is less than mol%, no anti-pilling effect will be obtained;
If it exceeds 0 mol%, spinning becomes difficult due to an increase in melt viscosity, so it is preferable to follow the above range.

本発明に用いるポリエステルは、フェノールと四塩化エ
タンの等重量混合溶媒によす0. 5/100mlの濃
度で20℃で測定した相対粘度(ηrel )が1、2
0乃至1.45特に好適には1.26乃至1.40の範
囲である。
The polyester used in the present invention is prepared using a mixed solvent of equal weights of phenol and tetrachloroethane. Relative viscosity (ηrel) measured at 20°C at a concentration of 5/100ml is 1,2
The range is from 0 to 1.45, particularly preferably from 1.26 to 1.40.

相対粘度の値が低すぎるときは、得られるポリエステル
ステープルの強度が低下し、紡績時に白粉が発生しやす
く、操業性が劣る。
When the value of relative viscosity is too low, the strength of the obtained polyester staple decreases, white powder is likely to be generated during spinning, and operability is poor.

又相対粘度が高すぎると紡績装置の摩耗が著るしく増大
する。
Furthermore, if the relative viscosity is too high, wear on the spinning device will increase significantly.

本発明において前記重合体に添加するポリ有機シロキサ
ンとしては該重合体と混合して溶融紡糸しても重合体の
分解を惹起しないものが望ましく、たとえばジメチルポ
リシロキサン、メチルフェニルポリシロキサン、ジフェ
ニルポリシロキサン等であり、中でも特にメチルフェニ
ルポリシロキサンがポリエステル中での耐熱性及び分散
性に優れ好適である。
In the present invention, the polyorganosiloxane added to the polymer is preferably one that does not cause decomposition of the polymer even when mixed with the polymer and melt-spun, such as dimethylpolysiloxane, methylphenylpolysiloxane, diphenylpolysiloxane. Among them, methylphenylpolysiloxane is particularly suitable because it has excellent heat resistance and dispersibility in polyester.

本発明に適するポリ有機シロキサンの分子量は20、
000以下が好ましく特に好適には15, 000以下
である。
The molecular weight of the polyorganosiloxane suitable for the present invention is 20,
000 or less, particularly preferably 15,000 or less.

該分子量が20, 000超えた場合ポリエステル中で
の均一分散性が低下し、又ステープルの熱処理によるポ
リ有機シロキサンの繊維表面への滲出ならびに被膜の展
延性が劣り、紡績時の白粉の発生を抑制する効果を得る
ことができない。
If the molecular weight exceeds 20,000, the uniform dispersibility in the polyester will decrease, the polyorganosiloxane will ooze out onto the fiber surface due to staple heat treatment, the spreadability of the coating will be poor, and the generation of white powder during spinning will be suppressed. I can't get the desired effect.

該ポリ有機シロキサンの25℃で測定した粘度は10、
000センチポイズ以下が好ましく特に6,000セ
ンチポイズ以下が好適である。
The viscosity of the polyorganosiloxane measured at 25°C is 10,
000 centipoise or less is preferable, and 6,000 centipoise or less is particularly preferable.

又該ポリ有機シロキサンは180℃における24時間後
の揮発分が1.5%以下が好ましく、特に好適には1.
0%以下である。
The polyorganosiloxane preferably has a volatile content of 1.5% or less after 24 hours at 180°C, particularly preferably 1.5% or less.
It is 0% or less.

該揮発分が多すぎると紡糸時の操業安定性ならびに繊維
の品質を低下せしめる。
If the volatile content is too large, operational stability during spinning and fiber quality will be reduced.

前記ポリエステル中に含有せしめるポリ有機シロキサン
の量は0.05乃至2.0重量%特に0.1乃至1.5
重量%が好適である。
The amount of polyorganosiloxane contained in the polyester is 0.05 to 2.0% by weight, particularly 0.1 to 1.5%.
% by weight is preferred.

該範囲より少ない場合本発明の目的とする効果が得られ
ず又該範囲を挑えた場合ポリエステル中での均一分散性
が低下して紡糸時或は延伸時に糸切れを発生する原因と
なるため上記範囲内で使用することが望ましい。
If it is less than this range, the desired effect of the present invention cannot be obtained, and if it exceeds this range, the uniform dispersibility in the polyester decreases, causing yarn breakage during spinning or drawing. It is desirable to use within this range.

本発明に於いてポリエステル中にポリ有機シロキサンを
含有せしめる方法はポリエステルを製造する原料中或は
重縮合中更には紡糸する際のポリエステルチップに添加
混合する等何れの方法によってもポリ有機シロキサンを
含有せしめることができるが特に紡糸の際のポリエステ
ルチップの乾燥時或は紡糸直前にポリ有機シロキサンを
添加混合する方法が作業上張も容易である。
In the present invention, the polyorganosiloxane can be incorporated into the polyester by any method such as adding it to the raw materials for producing polyester, during polycondensation, or adding and mixing it to polyester chips during spinning. However, a method in which polyorganosiloxane is added and mixed during drying of the polyester chips during spinning or immediately before spinning is particularly easy to work with.

ポリ有機シロキサン含有ポリエステルは常法に従って溶
融紡糸を行ない得られた未延伸糸トウを65℃乃至85
℃に加熱せるローラーにより延伸処理して次に160℃
乃至195℃に加熱せるローラーによりヒートセットし
た後常法により捲縮処理を行ない更に90℃乃至130
℃の温度特に好適には100℃乃至120℃の温度雰囲
気中で熱処理を行なう。
The polyorganosiloxane-containing polyester is prepared by melt-spinning the undrawn yarn tow according to a conventional method at 65°C to 85°C.
Stretched using rollers that can be heated to 160°C
After heat setting with a roller that can be heated to 195°C, crimping is performed by a conventional method, and further 90°C to 130°C.
The heat treatment is carried out in an atmosphere at a temperature of 100°C to 120°C, particularly preferably 100°C to 120°C.

該工程中延伸及びヒートセットに於いて前記処理温度範
囲を外れた場合白粉の発生が著るしく大となり又、均質
な物性値を有するトウが得られない。
If the temperature during stretching and heat setting during this process is outside the above-mentioned processing temperature range, the generation of white powder will be significantly increased, and a tow with uniform physical properties will not be obtained.

捲縮処理により付与する捲縮数は10乃至25回/25
mmが好ましく、特に13乃至20回/25mmが好適
である。
The number of crimps imparted by the crimping process is 10 to 25 times/25
mm is preferred, and 13 to 20 times/25 mm is particularly preferred.

捲縮数が上記範囲より少ない場合精紡工程での素抜けが
起り易くなり、紡績操業性が低下する。
If the number of crimps is less than the above range, droplets are likely to occur during the spinning process, resulting in reduced spinning operability.

又上記範囲を超えた場合はラップのリッキングが多くな
り紡績操業性が悪くなる。
If it exceeds the above range, the licking of the wrap will increase and the spinning operability will deteriorate.

熱処理は乾熱、温熱のうち特に捲縮トウの形態安定性の
点からら乾熱処理が好ましく少なくとも30秒間処理す
ることが望ましく、該処理によりポリエステル中に含有
するポリ有機シロキサンが捲縮繊維の表面に滲出して被
膜を形成し表面滑性を付与する。
The heat treatment is either dry heat or warm heat, and from the viewpoint of the morphological stability of the crimped tow, dry heat treatment is preferred, and the treatment is preferably carried out for at least 30 seconds. It oozes out to form a film that gives the surface smoothness.

この際前記温度範囲より未満の場合、該効果が得られな
い。
At this time, if the temperature is below the above range, the effect cannot be obtained.

又該温度範囲を超えた場合前工程で付与せる捲縮が弛緩
もしくは消失するため前記温度範囲内で処理することが
好ましい。
Furthermore, if the temperature exceeds the above range, the crimps imparted in the previous step will loosen or disappear, so it is preferable to carry out the treatment within the above temperature range.

該熱処理せる捲縮延伸糸トウは空冷或は冷風吹付は等任
意の方法により常温もしくはその近傍まで冷却した後常
法により切断して紡績性の優れたポリエステルステーブ
ルが得られる。
The heat-treated crimped and drawn yarn tow is cooled to room temperature or its vicinity by any method such as air cooling or blowing with cold air, and then cut by a conventional method to obtain a polyester stable with excellent spinnability.

本発明のポリエステルステープルは通常の方法で紡績さ
れ紡績機械の部品の摩耗を著しく減少し、例えば空気精
紡機のコーミングワイヤーは混紡率50%に於いても従
来の装置寿命の少なくとも2倍の使用が可能となり、ポ
リエステル100%の場合でも少なくとも8ケ月の使用
が可能である。
The polyester staple of the present invention is spun in a conventional manner and significantly reduces wear on parts of spinning machines; for example, the combing wire of an air spinning machine can be used for at least twice the life of conventional equipment even at a 50% blend. Even in the case of 100% polyester, it can be used for at least 8 months.

更に紡績工程及びその他捲糸、撚糸等の工程に於て空気
精紡機或はリング精紡機等何れの方法によっても白粉の
発生が極めて少なく糸切れ及び品質の低下を生ゼしぬる
ことなく又作業環境をも良好にして操業性ならびに品質
の安定した優れた紡績糸を得ることが出来る。
Furthermore, in the spinning process and other processes such as winding, twisting, etc., whether using an air spinning machine or a ring spinning machine, the generation of white powder is extremely small, and the work can be carried out without causing yarn breakage or quality deterioration. It is possible to obtain excellent spun yarn with stable operability and quality while maintaining a favorable environment.

以下実施例により本発明を説明する。The present invention will be explained below with reference to Examples.

実施例 1 ペンタエリスリトール0.2モル%を共重合した相対粘
度(ηrel) 1.38を有するポリエチレンテレフ
タレートの乾燥チップに分子量6000、粘度5000
センチポイズ(25℃)、揮発分が0.5%(180℃
、24時間)であるポリメチルフェニルシロキサンを所
定量添加し、タンブラ−型のブレンダーで混合後押出機
に供給して常法によす285℃で溶融して1200m
/minで引取り未延伸糸トウを得た。
Example 1 Dry chips of polyethylene terephthalate having a relative viscosity (ηrel) of 1.38 copolymerized with 0.2 mol% of pentaerythritol were coated with a molecular weight of 6000 and a viscosity of 5000.
centipoise (25℃), volatile content 0.5% (180℃
, 24 hours) was added in a predetermined amount, mixed in a tumbler-type blender, fed to an extruder, and melted at 285°C in a conventional manner to obtain 1200 m
/min to obtain an undrawn yarn tow.

該未延伸糸トウを延伸糸換算50万テ゛ニールになるよ
うに集束して75℃に加熱せるローラーにより3.97
倍に延伸し次に190℃に加熱せるローラーでヒートセ
ットした後ラウリルホスフェートカリウム塩を主体とす
る紡績油を付着せしめて、捲縮処理し、所定の熱処理温
度で処理した後切断して繊維長38mm、繊度1.39
デニールのステープルを得た。
The undrawn yarn tow was bundled to 500,000 niels in terms of drawn yarn, and heated to 75°C using a roller that heated the yarn to 3.97 mm.
It is stretched twice and then heat-set with a roller that can be heated to 190°C, then a spinning oil mainly containing potassium lauryl phosphate salt is applied, crimped, treated at a predetermined heat treatment temperature, and then cut to lengthen the fibers. 38mm, fineness 1.39
Got denier staples.

得られたステーブルを綿と50150にスライバー混紡
し空気精紡機で20番手の糸の紡績を行ない糸切れ回数
、白粉の発生状態を第1表に示した。
The resulting stable was blended with cotton and 50150 sliver, and spun into yarn of 20 count using an air spinning machine. Table 1 shows the number of yarn breaks and the state of white powder generation.

上表より明らかな如くポリメチルフェニルシロキサンの
添加量が0.05乃至2.0重量%である延伸ポリエス
テル捲縮糸トウを90℃乃至130℃で熱処理すること
により得られた捲縮形態安定なステープルを紡績して糸
切れならびに白粉発生量の極めて少ない均質なる紡績糸
が得られた。
As is clear from the above table, the crimped shape of the drawn polyester crimped yarn tow containing 0.05 to 2.0% by weight of polymethylphenylsiloxane was heat-treated at 90°C to 130°C. By spinning the staples, a homogeneous spun yarn with very little yarn breakage and white powder generation was obtained.

特にポリメチルフェニルシロキサンの添加量が0.01
乃至1.5重量%の場合、更に熱処理温度が100℃乃
至120℃の場合その効果は顕著である。
In particular, the amount of polymethylphenylsiloxane added is 0.01
The effect is remarkable when the content is 1.5% by weight and the heat treatment temperature is 100°C to 120°C.

又、本発明によるポリエステルステープルの原綿は従来
のポリメチルフェニルシロキサンを含有しないものに比
較してラップかや・嵩高となリケンスの収容量が減少す
る傾向が認められたが前紡後紡共紡績性は良好であった
In addition, it was observed that the raw cotton of the polyester staple according to the present invention tends to have less wrap and bulk, and has a reduced retentivity capacity compared to the conventional polyester staple that does not contain polymethylphenylsiloxane. The properties were good.

実施例 2 相対粘度(ηrel) 1,367であるポリエチレン
テレフタレートの乾燥チップに分子量の異なるポリジメ
チルシロキサンを0.3重量%添加して実施例1と同様
の方法で紡糸、延伸、ヒートセット、捲縮処理及び10
0℃で熱処理を行なって繊度1.4デニール、繊維長3
8mmのステープルを製造した。
Example 2 0.3% by weight of polydimethylsiloxane having a different molecular weight was added to dry chips of polyethylene terephthalate having a relative viscosity (ηrel) of 1,367, and the mixture was spun, stretched, heat set, and wound in the same manner as in Example 1. Shrinking process and 10
After heat treatment at 0℃, the fineness is 1.4 denier and the fiber length is 3.
8mm staples were manufactured.

この場合捲縮処理に於いて条件を種々変化せしめて捲縮
率の異なるステープルを得た。
In this case, staples with different crimp rates were obtained by varying the conditions in the crimp process.

これ等のポリエステル原綿を線条工程でポリエステル6
5/綿35の比率で混紡し45番手の糸をリング精紡機
により紡績した結果を第2表に示す。
These polyester raw cottons are made into polyester 6 through a filament process.
Table 2 shows the results of spinning a 45-count yarn using a ring spinning machine with a blend of 5/35 cotton.

上表より明らかな如く、ジメチルポリシロキサンの分子
量が20.000以下の場合、精紡工程での糸切及び泊
粉の発生が著しく少なく操業性が優れていた。
As is clear from the above table, when the molecular weight of dimethylpolysiloxane was 20.000 or less, the occurrence of thread breakage and loose powder during the spinning process was extremely small, and the operability was excellent.

尚第2表に示す白粉の発生(級)は次の3等級に区分し
て判定した。
Incidentally, the occurrence (grade) of white powder shown in Table 2 was classified into the following three grades.

又捲縮数は10乃至25回/25mm特に13乃至20
回/25mmの場合紡績操業性が優れており、前記範囲
より少ない場合、素抜けを生じて糸切れを多発し又前記
範囲を超えた場合ラップのリッキングが多くなり紡績操
業性を低下させるものであった。
Also, the number of crimp is 10 to 25 times/25mm, especially 13 to 20
When the number of turns/25 mm is less than the above range, yarn breakage occurs frequently due to slippage, and when it exceeds the above range, the licking of the wrap increases and reduces the spinning operability. there were.

実施例 3 実施例1に従って相対粘度(ηrel) 1.27(A
)、1、38(B)、1.42(C)を有するポリエチ
レンテレフタレート乾燥チップに各々゛ポリメチルフェ
ニルシロキサンを0.3重量%添加して製造した未延伸
糸トウを延伸ローラー及びヒートセットローラーの温度
を種々変化せしめて処理を行ない同様にして捲縮処理後
90℃で熱処理し、繊維長38mm繊度1.39デニー
ルのステープルを得た。
Example 3 Relative viscosity (ηrel) 1.27 (A
), 1, 38 (B), and 1.42 (C) by adding 0.3% by weight of polymethylphenylsiloxane to polyethylene terephthalate dry chips, respectively. Treatment was carried out at various temperatures, followed by crimping and heat treatment at 90° C. to obtain staples with a fiber length of 38 mm and a fineness of 1.39 denier.

該ステーブルを単独で用いリング精紡機により40番手
の糸を紡績して白粉の発生状態を実施例2に示す判定方
法に従って区分した。
Using the stable alone, a 40-count yarn was spun using a ring spinning machine, and the generation of white powder was classified according to the determination method shown in Example 2.

その結果を第3表に示す。The results are shown in Table 3.

上表より明らかな如く、延伸ローラ一温度が65℃〜8
5℃及びヒートセットローラ一温度が160℃〜195
℃の条件下でポリメチルフェニルシロキサンを含有する
ポリエチレンテレフタレートの未延伸糸トウを処理する
ことにより紡績時の白粉発生を抑制することができた。
As is clear from the table above, the temperature of the stretching roller is 65°C to 8°C.
5℃ and heat set roller temperature 160℃~195℃
By treating the undrawn yarn tow of polyethylene terephthalate containing polymethylphenylsiloxane under conditions of .degree. C., it was possible to suppress the generation of white powder during spinning.

実施例 4 実施例1に於てペンタエリスリトールの共重合比率を変
化させ更にペンタエリスリトールの代りにトリメリット
酸を同様に共重合せしめた相対粘度(ηrel) 1.
35〜1.38を有するポリエチレンテレフタレートの
乾燥チップに分子量9,000、粘度6,000センチ
ポイズ(25℃)、揮発分0.45%(180℃24時
間)であるポリメチルフェニルシロキサンを0.2重量
%添加し同様にして溶融紡糸を行ない得られた未延伸糸
トウを同一条件下で延伸、ヒートセット、捲縮処理を行
なって100℃で熱処理することにより、繊維内部に含
有せるポリメチルフェニルシロキサンを繊維表面に滲出
せしめて被膜を付与し、切断して繊維長38mm、繊度
1.37デニールのステープルを得た。
Example 4 Relative viscosity (ηrel) obtained by changing the copolymerization ratio of pentaerythritol in Example 1 and further copolymerizing trimellitic acid instead of pentaerythritol.1.
0.2 of polymethylphenylsiloxane having a molecular weight of 9,000, a viscosity of 6,000 centipoise (at 25°C), and a volatile content of 0.45% (at 180°C for 24 hours) was added to dry chips of polyethylene terephthalate having a molecular weight of 35 to 1.38. % by weight and melt-spun in the same manner, and the resulting undrawn yarn tow is stretched, heat-set, and crimped under the same conditions and heat-treated at 100°C to obtain polymethylphenyl contained inside the fiber. A coating was applied by exuding siloxane onto the fiber surface, and the fiber was cut to obtain a staple having a fiber length of 38 mm and a fineness of 1.37 denier.

得られたステープルを各々ポリエステル65%、綿35
%でスライバー混紡し、空気精紡機で20番手の紡績糸
を作製し、その際の糸切及び泊粉発生量を測定し更に紡
績糸を目付100g/m’の平織織布を作成しI、 C
,I型ピリングテスターにて5Qr、 p、 mで5時
間試験を行なって耐ピリング性(級)を判定した。
The resulting staples were each made of 65% polyester and 35% cotton.
% of the sliver, produced a 20 count spun yarn using an air spinning machine, measured the amount of yarn breakage and powder generated at that time, and further produced a plain weave woven fabric with a basis weight of 100 g/m' from the spun yarn. C
A test was conducted for 5 hours at 5 Qr, p, and m using a type I pilling tester to determine the pilling resistance (grade).

その結果を第4表に示す。上表より明らかな如く本発明
の方法によるステープルは紡績時の糸切ならびに白粉の
発生が少なくその効果は顕著である。
The results are shown in Table 4. As is clear from the above table, the staple produced by the method of the present invention has a remarkable effect in that thread breakage and generation of white powder during spinning are small.

更に分岐剤を0.02〜1.0モル%特に0.05〜0
.5モル%共重合せしめたポリエチレンテレフタレート
はメチルフェニルポリシロキサンとの相剰効果により極
めて優れた耐ピリン性を付与することができた。
Furthermore, 0.02 to 1.0 mol% of branching agent, especially 0.05 to 0
.. Polyethylene terephthalate copolymerized with 5 mol % was able to impart extremely excellent pilin resistance due to its mutual effect with methylphenylpolysiloxane.

更に前記試料A5及びA16の原綿をポリエステル65
/綿35の混紡比率で使用して三錘で長期紡出試験を行
なった結果従来のポリ有機シロキサンを含有しない原綿
を使用するものはコーミングワイヤーがビッカース硬度
3000を有する超硬型であったが耐用限度が6〜8ケ
月であり本発明による原綿を使用した場合10ケ月経過
時に於ても何等支障は認められず精紡機の摩耗が極めて
少ないことが解った。
Furthermore, the raw cotton of samples A5 and A16 was made of polyester 65.
A long-term spinning test was conducted using three spindles using a blend ratio of 35/cotton, and the result was that the combing wire of the conventional product using raw cotton that does not contain polyorganosiloxane was a carbide type with a Vickers hardness of 3000. The durability limit is 6 to 8 months, and when the raw cotton according to the present invention was used, no problems were observed even after 10 months, and it was found that the wear of the spinning machine was extremely small.

Claims (1)

【特許請求の範囲】 1 相対粘度が1.20乃至1.45のポリエステル中
に分子量20.000以下のポリ有機シロキサンを0.
05乃至2.0重量%含有せしめて溶融紡糸し、ローラ
一温度65℃乃至85℃で延伸を行ない、次にローラ一
温度160℃乃至195℃でヒートセットした後捲縮を
付与して90℃乃至130℃の温度雰囲気中で熱処理し
冷却した後切断することを特徴とする紡績性の優れたポ
リエステルステープルの製造方法。 2 熱処理温度が100℃乃至120℃の温度範囲であ
る特許請求の範囲第1項記載の紡績性の優れたポリエス
テルステーブルの製造方法。 3 熱処理が乾熱処理である特許請求の範囲第1項又は
第2項記載の紡績性の優れたポリエステルステーブルの
製造方法。
[Scope of Claims] 1. Polyorganosiloxane having a molecular weight of 20.000 or less is mixed into a polyester having a relative viscosity of 1.20 to 1.45.
05 to 2.0% by weight, melt-spun, stretched at a roller temperature of 65°C to 85°C, then heat set at a roller temperature of 160°C to 195°C, and then crimped at 90°C. A method for producing a polyester staple with excellent spinnability, which comprises heat-treating in an atmosphere at a temperature of 130°C to 130°C, cooling, and then cutting. 2. The method for producing a polyester stable with excellent spinnability according to claim 1, wherein the heat treatment temperature is in the temperature range of 100°C to 120°C. 3. The method for producing a polyester stable with excellent spinnability according to claim 1 or 2, wherein the heat treatment is a dry heat treatment.
JP13664576A 1976-11-13 1976-11-13 Method for manufacturing polyester staple with excellent spinnability Expired JPS5953368B2 (en)