JPS5874169A - Lens coating method - Google Patents
Lens coating methodInfo
- Publication number
- JPS5874169A JPS5874169A JP17112781A JP17112781A JPS5874169A JP S5874169 A JPS5874169 A JP S5874169A JP 17112781 A JP17112781 A JP 17112781A JP 17112781 A JP17112781 A JP 17112781A JP S5874169 A JPS5874169 A JP S5874169A
- Authority
- JP
- Japan
- Prior art keywords
- lens
- liquid
- boundary line
- lenses
- boundary
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【発明の詳細な説明】
本発明は、プラスチックレンズのコーティング方法に関
し、更に詳しくは、境目のあるプラスチ、クレンズのデ
ィッピングによるコーティング方法に関する。DETAILED DESCRIPTION OF THE INVENTION The present invention relates to a method for coating plastic lenses, and more particularly to a method for coating plastic lenses with borders by dipping.
1972年の米国の”PI)A規格の制走以来、眼鏡レ
ンズの安全性が見直されるようになってし亀る中で、レ
ンズ材料としてより安全性の高し1合成樹脂が、無機ガ
ラスレンズに代りて使用されるようになってきた。無機
ガラスレンズから合成樹脂レンズへの移行は、世界的な
傾向であり、我国においても年々合成樹脂レンズのシェ
アが拡大しつつある。特にジエチレングリコールビスア
リルカーボネート(以下0R−59と略す)樹脂による
レンズの比率は、アメリカ、フランスにおいて既に50
襲を越えたと予想される6合成樹脂レンズは安全性が高
く、万−割れた場合にも、無機ガラスのような微細な破
片をならず、眼に損傷を与える可能性が少ない、又、無
機ガラスに比べて軽い、加工性が良い、着色が容易であ
る等の多くの利点を有している。一方、合成樹脂材料に
よるプラスチックレンズは、傷がつきやすい、曇りやす
いといつた欠点を有している。Since the introduction of the PI)A standard in the United States in 1972, the safety of eyeglass lenses has been reconsidered, and inorganic glass lenses have been replaced by synthetic resins, which are safer as lens materials. The shift from inorganic glass lenses to synthetic resin lenses is a global trend, and in Japan, the share of synthetic resin lenses is increasing year by year.In particular, diethylene glycol bisallyl The ratio of lenses made of carbonate (hereinafter abbreviated as 0R-59) resin has already reached 50% in the United States and France.
6.Synthetic resin lenses are expected to be able to withstand many types of damage. Even if they break, they will not break into minute pieces like inorganic glass, and are less likely to cause eye damage. It has many advantages compared to glass, such as being lighter, easier to process, and easier to color. On the other hand, plastic lenses made of synthetic resin materials have drawbacks such as being easily scratched and easily fogged.
近代、合成樹脂材層によるプラスチックレンズ′の耐擦
傷性を向上させるために、シリコン系、アタリル系の^
−トコー)をコーティングをするようになりてきた。又
、プラスチックレンズの曇りやすさに、ついては、レン
ズ表面に防曇コートを施すことにより解決された。一方
、高齢化礼金の進む現在、二重、焦点レンズ、三重焦点
レンズの需要は急速にのびる傾向にあり、合成樹脂レン
ズについてもその′傾向は同じである。それにともない
、今後レンズ市場において、合成樹脂製レンズの二重焦
点、三重焦点等の多焦点レンズに、バートコ)、isコ
ーFを施したレンズの要望が高重うている。これら二重
焦点、三重焦点レンズは、そのレンズ目的から2種ある
いは3種の違ったレンズカーブな有するため、レンズ褒
面に境目(段差)ができる、しかし、この種の二重焦点
、三重焦点レンズをコーティングする際に境目の方向性
をもたせずにディッピングすると、たとえばデイツビン
ダ液面に対して水平にした場合、図1のように、レンズ
境目部分にコーテイング液がたまるという問題が発生す
る。この液だまりは、レンズの境目付近の像のぼけとな
り、視舒をさまたげるものである。
■・
本発明は、上記の点に鑑みこれら境目のあるレンズのコ
ーティング方法に関するものである。すなわち、本発明
による境目のあるプラスチックレ図2のごとく境目を液
面に対して垂直もしくは垂直に対して20度以内の傾き
で支持しディッピングする方法である。境目をディッピ
ング液面に対して垂直もしくは20度以内の傾きで支持
することにより、ディッピンダ液がなめらかに流れおち
、境目部分に液だ重りができないので境目部分において
像がぼけるという問題はなくなる。この方法によれば、
二重焦点レンズ、三重焦点レンズ等の多焦点レンズのい
かなるタイプについても適用できるものである。In modern times, in order to improve the scratch resistance of plastic lenses with synthetic resin material layers, silicone-based and ataryl-based materials are used.
-Toko) has started to be coated. Furthermore, the tendency of plastic lenses to fog has been solved by applying an anti-fog coating to the lens surface. On the other hand, as the population ages, the demand for double-focal lenses, focal lenses, and trifocal lenses is rapidly increasing, and the same trend holds true for synthetic resin lenses. Accordingly, in the future lens market, there will be a growing demand for multifocal lenses such as bifocal and trifocal synthetic resin lenses that are coated with BARTCO) and ISCO F. These bifocal and trifocal lenses have two or three different lens curves depending on their purpose, so there is a boundary (step) on the lens surface. If a lens is coated by dipping without proper boundary direction, for example, when the dipping is done horizontally to the Deitzbinder liquid level, a problem arises in that the coating liquid accumulates at the lens boundary, as shown in FIG. 1. This liquid pool blurs the image near the boundary between the lenses and obstructs visibility.
(2) In view of the above points, the present invention relates to a method of coating lenses with these boundaries. That is, as shown in FIG. 2, the plastic plate with a boundary according to the present invention is supported with the boundary perpendicular to the liquid level or at an angle of less than 20 degrees to the vertical, and dipping is carried out. By supporting the boundary perpendicularly to the dipping liquid level or at an angle of 20 degrees or less, the dipping liquid flows down smoothly and no liquid pool is formed at the boundary, eliminating the problem of blurred images at the boundary. According to this method,
It is applicable to any type of multifocal lens such as a bifocal lens or a trifocal lens.
以下に記載する実施例は、本発明をより良く説明するも
のであり、本発明の範囲を限定するものではない。The examples described below serve to better explain the invention and are not intended to limit the scope of the invention.
実施例中のh−ドコート液、防曇コート液組成は次のと
うりヤ′ある。The compositions of the hard coating solution and the antifogging coating solution in the examples are as follows.
t ハづコミト液
(1) テトラエトキシシラン部分加水分解物溶液の
調整、イソプ田ビルアルコール50重量部にテ)フェト
キシシラ2150重量部を溶堺し、さらに、O,OSS
規定塩酸水溶液3型
温で10時間以上攪拌した。t Hazucomito solution (1) Preparation of tetraethoxysilane partial hydrolyzate solution, dissolve 2150 parts by weight of fethoxysilane in 50 parts by weight of isoptabil alcohol, and further add O, OSS.
The mixture was stirred at a normal aqueous hydrochloric acid solution temperature for 10 hours or more.
(2) r−グリシドキシプ四ピルトリメトキシシラン
部分加水分解瞼溶液の調瓢イソプソビルアルコール13
3重量部、r−グリシドキシプロビルトリメトキシシラ
ン55重量部、およびa05規定塩酸水溶液12重量部
な用いて、(1)と同様にして加水分解した。(2) Preparation of r-glycidoxyp4pyltrimethoxysilane partially hydrolyzed eyelid solution Isopsovir alcohol 13
Hydrolysis was carried out in the same manner as in (1) using 3 parts by weight, 55 parts by weight of r-glycidoxypropyltrimethoxysilane, and 12 parts by weight of a05 normal hydrochloric acid aqueous solution.
(1) 、 (2)の溶液を1:1の一合で混合したも
のに開環重合触媒を、溶液全重量に対してα01襲加え
、混合攪拌してきた溶液。A solution obtained by mixing the solutions (1) and (2) at a ratio of 1:1, adding a ring-opening polymerization catalyst at α01 times relative to the total weight of the solution, and mixing and stirring.
2、 防曇コート液
2−とドロキシエチルメタクリレートの予備重合体の1
8重量部エチレングリコールメチルエーテル溶液(商品
名:ハイド胃ン)を@温性樹脂母体とし、この固彫成分
に対して、)リメリット蒙を化学当量外で15襲加え、
さらに界面活性剤とシテポリオキシエチレンノニルフェ
ノールエーテル(商品名:エマルゲン950、花王アシ
ラス株式金社製)を樹脂固彫成分に対して重量比で15
弧配合した。これに触媒としてカートルエンスルホン讃
少量を添加してなる溶液。2. Anti-fog coating liquid 2- and droxyethyl methacrylate prepolymer 1
8 parts by weight of ethylene glycol methyl ether solution (trade name: Hyde Gastric) was used as a thermoplastic resin matrix, and 15 times of Limeritol was added outside the chemical equivalent to this hard carving component.
Furthermore, a surfactant and Cite polyoxyethylene nonylphenol ether (trade name: Emulgen 950, manufactured by Kao Acillus Co., Ltd.) were added at a weight ratio of 15 to the resin hard carving component.
The arc was combined. A solution made by adding a small amount of cartoluenesulfone as a catalyst to this.
実施例t
ビスタパイフォーカル8 2 B−6s (版部BHt
店商品名、第4図aタイプ)レンズを、レンズ境目部が
ディッピング液面に対して垂直になるように支持して、
1の八−ドコート液をディッピングによってコーティン
グし、150℃の恒温槽中で1時間加熱し硬化させた。Example t Vista Pi Focal 8 2 B-6s (Banbu BHt
Store product name, Figure 4 a type) Support the lens so that the lens border is perpendicular to the dipping liquid level,
The coating was coated with the 8-decoat solution No. 1 by dipping, and heated in a constant temperature bath at 150° C. for 1 hour to cure.
又、同じくビスタ828ー65レンズに、2の防曇コー
ト液を、同じくレンズ境目部分がディッピング液面に対
して垂直になるように支持して、ディッピングによって
コーティングした。その後、30分間空気中に放置して
溶媒を飛散させた後、150℃恒温榴中で40分間加熱
し、硬化させた。Further, the anti-fog coating liquid of No. 2 was applied to the same Vista 828-65 lens by dipping while supporting the lens so that the boundary portion of the lens was perpendicular to the dipping liquid level. Thereafter, it was left in the air for 30 minutes to scatter the solvent, and then heated for 40 minutes in a thermostat at 150° C. to be cured.
硬化シ終ったハードコーシレンズ,防曇レンズの境目部
分を検査した結果、液だまりはみられず、像のぼけもな
く鯉明なレンズでありた。When we inspected the boundary between the hard-cured lens and the anti-fog lens, we found that there were no liquid pools, and the lens was clear with no blurred images.
実施例2
ビスメトライフオーカルTRニー1X(服部時計店商品
名(第4図のbタイプレンズ))レンズをレンズ境目部
がディッピンダ液面に対して垂直に対して20度の傾き
で支持して、1のハードコート液をコーティングし、実
施例1の方法で硬化した。Example 2 A Bismet Life Ocal TR Knee 1X (product name of Hattori Watch Store (type b lens in Fig. 4)) lens was supported with the lens border at an angle of 20 degrees to the perpendicular to the Dipinder liquid surface. Then, the hard coat solution No. 1 was coated and cured by the method of Example 1.
又、同じくビスタトライ7オーカルTR1−mlXレン
ズを上記の方法で支持し、2の防曇コート液をコーティ
ングして実施例1の方法で乾燥硬化させた。硬化し終っ
たハードコートレンズ、防曇レンズともに境目部分を検
査した結果、液だまりは見られず、像のぼけもない鮮明
なレンズであった。In addition, a Vista Tri 7 Ocal TR1-mlX lens was similarly supported using the method described above, coated with the antifogging coating solution of No. 2, and dried and cured using the method of Example 1. When we inspected the boundary between the hard-coated lens and the anti-fog lens after it had hardened, we found that there were no liquid pools and the lens was clear with no blurred images.
第1図は、レンズの境目を液面に対して水平に支持した
ときの図であり、第2図は、第1W1の姿勢でディッピ
ングしてできたし1:ンズの図である。
第sv!Jは、レンズの境目を液面に対して垂直になる
ように支持した時の図であり、第4図は、実施例中のレ
ンズの形式をあられす。
1・・・レンズ支持部
2・・・ディッピンダ液
3・・・レンズ
4・・・液だまり
(α)・・・ビスタ82B−65
(6)・・・ビスメトライフオーカルTRX−11以
上
出願人 松島工業株式金社
株式会社諏訪精工舎
代理人 弁理士 最上 務
1
1
篤1団 1
第2図
第3図
第4圀FIG. 1 is a diagram when the boundary of the lens is supported horizontally with respect to the liquid surface, and FIG. 2 is a diagram of the first lens formed by dipping in the first W1 attitude. Chapter sv! J is a diagram when the lens is supported so that the borderline is perpendicular to the liquid level, and FIG. 4 shows the type of the lens in the example. 1... Lens support part 2... Dipinder liquid 3... Lens 4... Liquid pool (α)... Vista 82B-65 (6)... Vismet Life Ocal TRX-11 or later
Applicant Matsushima Kogyo Kinsha Co., Ltd. Suwa Seikosha Co., Ltd. Agent Patent Attorney Tsutomu Mogami 1 1 Atsushi 1 Group 1 Figure 2 Figure 3 Figure 4
Claims (1)
コーティングする際、境目を液面に対して垂直もしくは
垂直に対して2O2以内の傾きで支持することを特徴と
するレンズコーティング方法。A lens coating method characterized in that when coating a plastic lens with a border by dipping, the border is supported perpendicular to the liquid surface or at an angle of less than 2O2 with respect to the vertical.