JPH0834881A - Polyamide/polypropylene resin composition - Google Patents

Polyamide/polypropylene resin composition

Info

Publication number
JPH0834881A
JPH0834881A JP17118794A JP17118794A JPH0834881A JP H0834881 A JPH0834881 A JP H0834881A JP 17118794 A JP17118794 A JP 17118794A JP 17118794 A JP17118794 A JP 17118794A JP H0834881 A JPH0834881 A JP H0834881A
Authority
JP
Japan
Prior art keywords
polyamide
resin composition
polyolefin
weight
component
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP17118794A
Other languages
Japanese (ja)
Other versions
JP3013971B2 (en
Inventor
Eiichi Kamei
衛一 亀井
Yukihiko Asano
之彦 浅野
Kiyoshi Tsurusawa
清 鶴澤
Yutaka Matsutomi
豊 松富
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Ube Corp
Original Assignee
Ube Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ube Industries Ltd filed Critical Ube Industries Ltd
Priority to JP6171187A priority Critical patent/JP3013971B2/en
Priority to EP19950303378 priority patent/EP0683210B1/en
Priority to DE69511615T priority patent/DE69511615T2/en
Publication of JPH0834881A publication Critical patent/JPH0834881A/en
Priority to US08/915,139 priority patent/US5874176A/en
Application granted granted Critical
Publication of JP3013971B2 publication Critical patent/JP3013971B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

PURPOSE:To improve the moldability by compounding a polyamide with a modified polyolefin and an unmodified polyolefin to disperse the polyolefins as core/shell particles into the polyamide as a matrix. CONSTITUTION:A polyamide (A), e.g. nylon 66, is mixed with a polyolefin (B) modified with an alpha,beta-unsaturated carboxylic acid, e.g. maleic acid, or a derivative thereof and having a modulus in flexure (at 23 deg.C) of 1GPa or higher, e.g. a modified crystalline polypropylene resin, and an unmodified polyolefin (C) having a modulus in tension (at 23 deg.C) of 200MPa or lower, e.g., an ethylene/alpha- olefin copolymer, the amounts of the ingredients (A), (B), and (C) being 30-80wt.%, 5-50wt.%, and 5-65wt.%, respectively, based on the total amount thereof. The mixture is melt-kneaded with, e.g. a kneader at about 220 deg.C or higher to obtain the objective composition with excellent moldability in which the ingredient (A) serves as a matrix phase and the ingredients (B) and (C) serve as a dispersed phase having a core/shell particle structure.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、ポリアミドとポリオレ
フィンからなる低吸水性、寸法安定性、剛性、靭性およ
び成形性に優れた熱可塑性樹脂組成物、特にポリアミド
−ポリプロピレン系樹脂組成物に関する。本発明の熱可
塑性樹脂組成物は、機械部品、自動車部品、電気・電子
部品など広い分野に使用できる。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a thermoplastic resin composition comprising a polyamide and a polyolefin, which is excellent in low water absorption, dimensional stability, rigidity, toughness and moldability, and more particularly to a polyamide-polypropylene resin composition. The thermoplastic resin composition of the present invention can be used in a wide range of fields such as machine parts, automobile parts, and electric / electronic parts.

【0002】[0002]

【従来の技術およびその問題点】ポリアミド樹脂は、機
械的特性、耐熱性、耐薬品性および成形性をバランスよ
く備えているため、電気・電子部品および自動車部品な
どに広く用いられている。しかしながら、ポリアミド樹
脂は、吸湿性のため、吸湿により寸法変化および曲げ強
さ、弾性率などの機械的性質の大きな低下を来たし、寸
法精度が必要とされる部品などには、その使用範囲を大
きく制約されることが多い状況にあり、その改善が望ま
れている。
2. Description of the Related Art Polyamide resins are widely used for electric / electronic parts, automobile parts, etc. because they have a good balance of mechanical properties, heat resistance, chemical resistance and moldability. However, since polyamide resin is hygroscopic, it causes a dimensional change due to moisture absorption and a significant decrease in mechanical properties such as bending strength and elastic modulus, and its range of use is wide for parts that require dimensional accuracy. There are many restrictions, and improvements are desired.

【0003】一方、ポリプロピレンは、軽量性、低吸水
性であり、成形時の流動性に優れ、かつ、低価格である
ことから自動車部品および電気部品に多く用いられてい
る。しかしながら、耐熱性、強度、剛性が不十分なこ
と、さらに結晶性に起因する成形時の収縮率が大きく成
形品の寸法精度に劣るため、その使用範囲が制約されて
いる。
On the other hand, polypropylene is widely used for automobile parts and electric parts because of its light weight, low water absorption, excellent fluidity during molding, and low price. However, its use range is restricted because heat resistance, strength, and rigidity are insufficient, and the shrinkage rate at the time of molding due to crystallinity is large and the dimensional accuracy of the molded product is poor.

【0004】従来、ポリアミドの吸水による寸法変化を
改善するために、ポリアミド主鎖に芳香族のジカルボン
酸あるいはジアミン、あるいはそれらの塩からなるモノ
マー単位を共重合により導入する方法、あるいは、低吸
水性のポリマーをブレンドする方法が開示されている。
この場合、ブレンドに用いられる低吸水性ポリマーとし
ては、不飽和カルボン酸およびその誘導体で変性された
ポリプロピレン、ポリエチレン、およびそれらの共重合
体からなる結晶性樹脂あるいはゴムが知られている。
Conventionally, in order to improve the dimensional change due to water absorption of polyamide, a method of introducing a monomer unit composed of an aromatic dicarboxylic acid or diamine or a salt thereof into the polyamide main chain by copolymerization, or low water absorption. Disclosed is a method of blending the above polymers.
In this case, as a low water-absorbing polymer used for blending, a crystalline resin or rubber made of polypropylene, polyethylene modified by unsaturated carboxylic acid and its derivative, and a copolymer thereof is known.

【0005】例えば、特公昭42−12546号公報に
は、ポリアミド50〜99重量%と、不飽和カルボン酸
とオレフィンの共重合体50〜1重量%とよりなる相溶
性の改善された熱可塑性樹脂組成物が開示されている。
これらの樹脂組成物は、機械的性質において、特に破断
特性が優れているものの、開示されている樹脂組成物で
は、低吸水性と剛性および耐熱性との兼備が不十分であ
る。
For example, JP-B-42-12546 discloses a thermoplastic resin having an improved compatibility, which comprises 50 to 99% by weight of polyamide and 50 to 1% by weight of a copolymer of unsaturated carboxylic acid and olefin. Compositions are disclosed.
Although these resin compositions have excellent mechanical properties, in particular, rupture properties, the disclosed resin compositions are insufficient in combination of low water absorption, rigidity and heat resistance.

【0006】特公昭45−30945号公報には、オレ
フィン系ポリマーと、ポリアミドおよび/またはポリエ
ステルと、酸、エステル、アミド、酸無水物およびエポ
キシ基の少なくとも1個で変性したポリオレフィンとか
らなる分散性の良好な繊維に適した樹脂組成物の製造方
法が開示されている。しかし、得られる樹脂組成物は、
射出成形品および押出成形品に適用した場合は、成形時
の収縮率が大きく、成形品の寸法精度に劣るとともに、
耐衝撃性が不十分であるなどの問題がある。
JP-B-45-30945 discloses a dispersibility comprising an olefin polymer, a polyamide and / or a polyester, and a polyolefin modified with at least one of an acid, an ester, an amide, an acid anhydride and an epoxy group. A method for producing a resin composition suitable for good fibers is disclosed. However, the resin composition obtained is
When applied to injection molded products and extrusion molded products, the shrinkage rate at the time of molding is large, and the dimensional accuracy of the molded products is inferior.
There are problems such as insufficient impact resistance.

【0007】特開昭60−262853号公報には、ポ
リアミドと変性エチレン−プロピレンブロックコポリマ
ーからなる低吸水化ポリアミド樹脂組成物が開示されて
いる。この樹脂組成物は、剛性および耐熱性を著しく損
なうことなくポリアミドの低吸水化がある程度図られて
いるものの、低吸水化レベルは不十分な状況にある。
JP-A-60-262853 discloses a low water absorption polyamide resin composition comprising a polyamide and a modified ethylene-propylene block copolymer. Although this resin composition is intended to reduce the water absorption of the polyamide to some extent without significantly impairing the rigidity and heat resistance, the level of low water absorption is insufficient.

【0008】特開昭62−223250号公報には、結
晶性ポリオレフィンを、ポリアミドおよび不飽和カルボ
ン酸誘導体と混練することにより得られる変性ポリオレ
フィンを、さらにポリアミドおよびポリオレフィンとと
もに混練することにより、低吸水性、引張り強さおよび
表面光沢に優れた樹脂組成物が開示されている。しかし
ながら、この樹脂組成物は、剛性と耐衝撃性の両立が不
十分な状況にある。
In JP-A-62-223250, a modified polyolefin obtained by kneading a crystalline polyolefin with a polyamide and an unsaturated carboxylic acid derivative is further kneaded with the polyamide and the polyolefin to obtain a low water absorption property. , A resin composition excellent in tensile strength and surface gloss is disclosed. However, this resin composition is in a situation where compatibility of rigidity and impact resistance is insufficient.

【0009】特開昭62−223251号公報には、前
記樹脂組成物に、さらに、低結晶性エチレン−α−オレ
フィン共重合体を加えてなる耐衝撃性に優れた樹脂組成
物が開示されている。しかしながら、この樹脂組成物で
は、吸水性は改善されているものの剛性レベルが低く、
低吸水性と機械的性質の両立が不十分な状況にある。
Japanese Unexamined Patent Publication (Kokai) No. 62-223251 discloses a resin composition excellent in impact resistance, which is obtained by adding a low crystalline ethylene-α-olefin copolymer to the above resin composition. There is. However, in this resin composition, although the water absorption is improved, the rigidity level is low,
There is an insufficient balance between low water absorption and mechanical properties.

【0010】特開平1−51458号公報には、ポリア
ミド樹脂と不飽和カルボン酸変性結晶性ポリプロピレン
と不飽和カルボン酸変性エチレン−α−オレフィン共重
合体とからなる吸水寸法変化が小さく、剛性、耐衝撃性
の優れたポリアミド樹脂組成物が開示されている。しか
しながら、ポリアミド成分の多い組成物では、機械的性
質が優れているものの、吸水性の改善が不十分であり、
低吸水化と機械的性質の両立は依然として十分達成され
ているとは言えない。
Japanese Unexamined Patent Publication (Kokai) No. 1-51458 discloses a polyamide resin, an unsaturated carboxylic acid-modified crystalline polypropylene, and an unsaturated carboxylic acid-modified ethylene-α-olefin copolymer, which have a small water absorption dimensional change, rigidity and resistance. A polyamide resin composition having excellent impact properties is disclosed. However, in a composition having many polyamide components, although the mechanical properties are excellent, the improvement of water absorption is insufficient,
It cannot be said that compatibility between low water absorption and mechanical properties has been sufficiently achieved.

【0011】特開昭64−87652号公報には、一部
変性した結晶性プロピレン−エチレンブロック共重合体
とポリアミドおよび変性エチレン−α−オレフィン共重
合体ゴムとからなる耐衝撃性の優れたポリプロピレン樹
脂組成物が開示されている。しかしながら、これらは、
ポリプロピレンをマトリックスとし、ポリアミドを分散
相とするものであり、ポリプロピレンに比べて、耐熱性
および機械的特性の向上が図られているものの、ポリア
ミドの特性に対しては、大幅に剛性および耐熱性が低下
したものに留まっている。
Japanese Unexamined Patent Publication (Kokai) No. 64-86652 discloses a polypropylene having a high impact resistance which comprises a partially modified crystalline propylene-ethylene block copolymer, a polyamide and a modified ethylene-α-olefin copolymer rubber. Resin compositions are disclosed. However, these are
Polypropylene is used as a matrix and polyamide is used as the dispersed phase, and although it has improved heat resistance and mechanical properties compared to polypropylene, it has significantly higher rigidity and heat resistance than polyamide. It remains low.

【0012】特開平1−146942号公報には、不飽
和カルボン酸またはその誘導体でグラフト変性された変
性ポリオレフィン共重合体40〜60重量%と、ポリア
ミド60〜40重量%とよりなる組成物において、MF
Rが2.0g/10分以下の比較的高分子量の変性ポリ
オレフィンを用いることにより、剛性、耐水性、ウェル
ド強度の優れた樹脂組成物が得られることが開示されて
いる。しかしながら、この樹脂組成物では、耐衝撃性の
改善効果が見られず、成形収縮率が高く、成形における
寸法安定性に乏しいとともに、溶融流動性が十分でない
という課題を残している。
JP-A-1-146942 discloses a composition comprising 40 to 60% by weight of a modified polyolefin copolymer graft-modified with an unsaturated carboxylic acid or a derivative thereof and 60 to 40% by weight of a polyamide. MF
It is disclosed that a resin composition having excellent rigidity, water resistance and weld strength can be obtained by using a modified polyolefin having a relatively high molecular weight of R of 2.0 g / 10 minutes or less. However, this resin composition does not show the effect of improving impact resistance, has a high molding shrinkage ratio, is poor in dimensional stability in molding, and has a problem that melt flowability is insufficient.

【0013】特開平3−91560号公報には、ポリア
ミド100重量部に対し、変性ポリオレフィン1〜10
0重量部およびポリプロピレン樹脂5〜250重量部か
らなるポリアミドと変性ポリオレフィンとポリプロピレ
ン樹脂との混合物に対して、有機耐熱安定剤0.01〜
3.0重量部および特定のカーボンブラック0.1〜
5.0重量部を配合してなる耐熱老化性に優れたポリア
ミド樹脂組成物が開示されている。しかしながら、この
樹脂組成物では、耐衝撃性および成形時寸法安定性が十
分でないという課題を残している。
JP-A-3-91560 discloses that modified polyolefins 1 to 10 are added to 100 parts by weight of polyamide.
Organic heat-resistant stabilizer 0.01 to 0.01 parts by weight based on a mixture of 0 parts by weight and polypropylene resin 5 to 250 parts by weight of polyamide, modified polyolefin and polypropylene resin.
3.0 parts by weight and specific carbon black 0.1 to
A polyamide resin composition containing 5.0 parts by weight and excellent in heat aging resistance is disclosed. However, this resin composition still has a problem that impact resistance and dimensional stability during molding are not sufficient.

【0014】特開平3−109452号公報には、ポリ
プロピレンとポリアミドからなる成形材料において、成
形材料100重量部に対して、ポリプロピレン樹脂10
〜89.9重量部、ポリアミド10〜89.9重量部、
不飽和カルボン酸変性ポリオレフィン0.1〜5重量
部、衝撃改良材0〜30重量部および強化材0〜60重
量部からなる樹脂組成物は、優れた靱性、剛性および熱
変形安定性を示すことが開示されている。しかしなが
ら、この樹脂組成物においても、成形時の溶融流動性、
軽量性が十分でなく、課題を残している。
Japanese Unexamined Patent Publication (Kokai) No. 3-109452 discloses a molding material composed of polypropylene and polyamide, wherein a polypropylene resin 10 is added to 100 parts by weight of the molding material.
~ 89.9 parts by weight, polyamide 10-89.9 parts by weight,
A resin composition comprising 0.1 to 5 parts by weight of an unsaturated carboxylic acid-modified polyolefin, 0 to 30 parts by weight of an impact modifier and 0 to 60 parts by weight of a reinforcing material exhibits excellent toughness, rigidity and thermal deformation stability. Is disclosed. However, even in this resin composition, melt fluidity at the time of molding,
Lightness is not enough, leaving a problem.

【0015】特開平3−115342号公報には、ポリ
プロピレン94〜50重量%、変性ポリオレフィン1〜
40重量%およびポリアミド5〜40重量%からなり、
用いるポリアミドに対するポリプロピレンの溶融粘度比
が1以上であるポリプロピレン樹脂組成物が開示されて
いる。しかしながら、この樹脂組成物は、ポリプロピレ
ンに比べて耐熱性が改善されているものの、成形時の寸
法安定性、および、靱性の改善レベルが十分でない。
Japanese Unexamined Patent Publication (Kokai) No. 3-115342 discloses that polypropylene 94 to 50% by weight, modified polyolefin 1 to
40% by weight and 5-40% by weight polyamide,
A polypropylene resin composition is disclosed in which the melt viscosity ratio of polypropylene to the polyamide used is 1 or more. However, although this resin composition has improved heat resistance as compared with polypropylene, the level of improvement in dimensional stability during molding and toughness is not sufficient.

【0016】特開平3−146552号公報には、ポリ
アミド40〜80重量%、変性ポリオレフィン1〜40
重量%およびポリプロピレン20〜60重量%からなる
樹脂組成物において、成形温度における剪断速度350
0sec-1の溶融粘度比ηPP/ηPAを0.75以上とす
ることにより、優れた塗装性を示すことが開示されてい
る。しかしながら、この樹脂組成物においても、耐衝撃
性や成形時の寸法安定性が十分でない。
JP-A-3-146552 discloses that polyamide 40 to 80% by weight, modified polyolefin 1 to 40
A resin composition consisting of 20% by weight of polypropylene and 20 to 60% by weight of polypropylene, and a shear rate of 350 at the molding temperature.
It is disclosed that when the melt viscosity ratio η PP / η PA of 0 sec −1 is 0.75 or more, excellent coatability is exhibited. However, even with this resin composition, impact resistance and dimensional stability during molding are not sufficient.

【0017】特開平3−207735号公報には、ポリ
アミド、ポリオレフィンおよび変性ポリオレフィンから
なる樹脂組成物において、引張降伏強度が300kg/
cm 2 以上の変性ポリオレフィンを用いることにより、
機械的特性、特にウェルド強度に優れた樹脂成形品が得
られることが開示されている。しかしながら、この樹脂
組成物においては、成形時の固化に伴う収縮率が大き
く、成形品の寸法安定性および靱性が不十分である。
Japanese Unexamined Patent Publication (Kokai) No. 3-207735 discloses that poly
From amides, polyolefins and modified polyolefins
In the resin composition, the tensile yield strength is 300 kg /
cm 2By using the above modified polyolefin,
A resin molded product with excellent mechanical properties, especially weld strength, is obtained.
Is disclosed. However, this resin
The composition has a large shrinkage rate due to solidification during molding.
In addition, the dimensional stability and toughness of the molded product are insufficient.

【0018】特公昭55−44108号公報には、エチ
レン、カルボニル化合物、α、β−不飽和カルボン酸お
よびその誘導体、不飽和エポキシド、カルボン酸および
その誘導体、アクリル酸エステル、芳香族側鎖を有する
単量体、不飽和炭素−炭素単量体のうち、少なくとも1
個以上の残基を有するポリマーが、ポリアミドマトリッ
クス樹脂中で分離した粒子中に共存する多相熱可塑性樹
脂組成物が開示されている。しかしながら、この組成物
は、耐衝撃性および曲げ弾性率に優れる一方、低吸水化
が不十分であり、機械的特性と吸水寸法安定性の兼備が
実現されていない。
Japanese Patent Publication No. 55-44108 has ethylene, carbonyl compounds, α, β-unsaturated carboxylic acids and their derivatives, unsaturated epoxides, carboxylic acids and their derivatives, acrylic acid esters, and aromatic side chains. At least one of a monomer and an unsaturated carbon-carbon monomer
A multiphase thermoplastic resin composition is disclosed in which a polymer having one or more residues coexists in separate particles in a polyamide matrix resin. However, while this composition is excellent in impact resistance and flexural modulus, it is insufficient in low water absorption, and has not achieved both mechanical properties and water absorption dimensional stability.

【0019】特開昭55−9661号公報には、α、β
−不飽和カルボン酸またはその誘導体を0.05〜1.
5重量%グラフトさせた変性エチレン系共重合体とポリ
アミドとを、2/3:1〜6:1の比で含んでなる柔軟
性を有する熱可塑性樹脂組成物が開示されている。しか
しながら、この熱可塑性樹脂組成物においては、柔軟性
および耐衝撃性は改善されているものの、剛性および破
断時の伸びの低下を来たしている。
JP-A-55-9661 discloses that α, β
-Unsaturated carboxylic acid or its derivative 0.05-1.
A flexible thermoplastic resin composition comprising a modified ethylene copolymer grafted with 5% by weight and a polyamide in a ratio of 2/3: 1 to 6: 1 is disclosed. However, in this thermoplastic resin composition, although the flexibility and impact resistance are improved, the rigidity and the elongation at break are reduced.

【0020】特開昭54−123158号公報には、不
飽和カルボン酸付加ポリオレフィン樹脂を含むポリオレ
フィン樹脂と窒素含有樹脂および充填剤とからなる機械
的強度、耐熱性および塗装性に優れたポリオレフィン樹
脂組成物が開示されている。しかしながら、この樹脂組
成物は、曲げ強さ、熱変形温度および塗装性は改善され
るものの、剛性、靱性、軽量性および寸法安定性の兼備
に課題を残している。
Japanese Unexamined Patent Publication (Kokai) No. 54-123158 discloses a polyolefin resin composition which comprises a polyolefin resin containing an unsaturated carboxylic acid-added polyolefin resin, a nitrogen-containing resin and a filler and which is excellent in mechanical strength, heat resistance and paintability. The thing is disclosed. However, although this resin composition is improved in bending strength, heat distortion temperature and coatability, it still has problems in combining rigidity, toughness, lightness and dimensional stability.

【0021】特開昭59−232135号公報には、変
性ポリオレフィン、ポリアミドおよび結晶性ポリオレフ
ィンからなり、オレフィン単位量が全体の70重量%以
上である染色性の優れたポリオレフィン樹脂組成物が開
示されている。しかしながら、このポリオレフィン樹脂
組成物は、ポリオレフィンを主成分とするものであるか
ら、射出成形品に適用された場合、強度、剛性、耐熱性
などの特性はポリオレフィンより改善されるものの、そ
の改善レベルはなお十分ではないといった課題を残して
いる。
Japanese Unexamined Patent Publication (Kokai) No. 59-232135 discloses a polyolefin resin composition comprising a modified polyolefin, a polyamide and a crystalline polyolefin and having an olefin unit content of 70% by weight or more and having excellent dyeability. There is. However, since this polyolefin resin composition is mainly composed of polyolefin, when it is applied to an injection-molded article, the properties such as strength, rigidity and heat resistance are improved as compared with the polyolefin, but the improvement level is However, there is still a problem that it is not enough.

【0022】特開昭60−118735号公報には、ポ
リアミドと変性ポリオレフィンからなる機械的特性およ
び低吸水性を併せ有する樹脂組成物が開示されている。
しかしながら、開示された樹脂組成物では、剛性および
低吸水性のバランスが必ずしも十分でない。
Japanese Unexamined Patent Publication (Kokai) No. 60-118735 discloses a resin composition composed of a polyamide and a modified polyolefin and having both mechanical properties and low water absorption.
However, the disclosed resin composition does not always have sufficient balance between rigidity and low water absorption.

【0023】特開昭57−8246号公報には、ポリア
ミドと、結晶化度40%以上のポリオレフィンと、結晶
化度35%以下のエチレン−α−オレフィン共重合体を
α、β−不飽和カルボン酸およびその誘導体で変性した
ポリオレフィンからなる樹脂組成物が開示されている。
この樹脂組成物では、耐衝撃性および外観が改善されて
いるものの、剛性と低吸水性のバランスが十分でない。
JP-A-57-8246 discloses a polyamide, a polyolefin having a crystallinity of 40% or more, and an ethylene-α-olefin copolymer having a crystallinity of 35% or less as an α, β-unsaturated carvone. A resin composition comprising a polyolefin modified with an acid and its derivative is disclosed.
Although this resin composition has improved impact resistance and appearance, the balance between rigidity and low water absorption is not sufficient.

【0024】特開昭59−149940号公報および特
開昭60−110740号公報には、ポリプロピレンと
ポリアミドおよび変性プロピレン−α−オレフィン共重
合体を加えてなる剛性、耐衝撃性、光沢、耐熱性に優れ
たプロピレン重合体組成物が開示されている。しかしな
がら、開示された樹脂組成物は、ポリプロピレンをマト
リックスとするものであるから、曲げ弾性率で示される
剛性は、ポリアミドのそれに比べかなり低いものに留ま
るものになっている。
JP-A-59-149940 and JP-A-60-110740 disclose rigidity, impact resistance, gloss and heat resistance obtained by adding polypropylene, polyamide and modified propylene-α-olefin copolymer. A superior propylene polymer composition is disclosed. However, since the disclosed resin composition uses polypropylene as a matrix, the rigidity indicated by the flexural modulus is much lower than that of polyamide.

【0025】以上述べたように、従来公知のポリアミド
樹脂組成物においては、ポリアミドの有する機械的強
度、耐熱性および成形性と、ポリオレフィンの有する軽
量性および低吸水性とをバランスよく備えているとはい
えず、これらポリアミドの有する特性とポリオレフィン
の有する特性を兼ね備えているとともに、さらに、両樹
脂に不足している、成形時の低反り性、寸法安定性およ
び耐衝撃性を備えている、高度に特性バランスに優れた
熱可塑性樹脂組成物が、さらに、求められている。
As described above, the conventionally known polyamide resin composition has a good balance of the mechanical strength, heat resistance and moldability of polyamide, and the light weight and low water absorption of polyolefin. Not only that, it possesses the properties of these polyamides and the properties of polyolefins, and also has the low warpage during molding, dimensional stability and impact resistance that are lacking in both resins. Further, there is a further demand for a thermoplastic resin composition having an excellent property balance.

【0026】[0026]

【発明が解決しようとする課題】本発明は、ポリアミド
の有する機械的強度、耐熱性および成形性と、ポリオレ
フィンの有する軽量性および低吸水性とをバランスよく
備え、さらに、両樹脂に不足している、成形時の低反り
性、寸法安定性および耐衝撃性を備えた熱可塑性樹脂組
成物、特にポリアミド−ポリプロピレン系樹脂組成物を
提供することを目的とする。
DISCLOSURE OF THE INVENTION The present invention has a good balance of the mechanical strength, heat resistance and moldability of polyamide and the light weight and low water absorption of polyolefin. It is an object of the present invention to provide a thermoplastic resin composition having low warpage during molding, dimensional stability, and impact resistance, particularly a polyamide-polypropylene resin composition.

【0027】[0027]

【課題を解決するための手段】本発明者らは、上記課題
を達成するために鋭意検討した結果、ポリアミド樹脂
と、特定の曲げ弾性率を有する、変性されたポリオレフ
ィン樹脂と、さらに、特定範囲の共重合組成および、特
定の引張弾性率を有する未変性のポリα−オレフィン共
重合体とを特定割合で配合することにより、上述の目的
を満足する樹脂組成物が得られることを見出し、本発明
に到達した。
Means for Solving the Problems The inventors of the present invention have conducted extensive studies to achieve the above object, and as a result, have found that a polyamide resin, a modified polyolefin resin having a specific flexural modulus, and a specific range It has been found that a resin composition satisfying the above-mentioned object can be obtained by blending the copolymer composition of (1) and an unmodified poly α-olefin copolymer having a specific tensile modulus at a specific ratio, and The invention was reached.

【0028】すなわち、本発明は、ポリアミド(A)、
変性ポリオレフィン(B)および未変性ポリオレフィン
(C)からなる樹脂組成物において、該樹脂組成物全体
に対して、ポリアミド(A)が30〜80重量%、変性
ポリオレフィン(B)が5〜50重量%、および未変性
ポリオレフィン(C)が5〜65重量%(ただし、
(A)と(B)と(C)の合計は100重量%)からな
り、かつ、変性ポリオレフィン(B)がα、β−不飽和
カルボン酸無水物およびその誘導体で変性された、23
℃における曲げ弾性率が1GPa以上の結晶性ポリプロ
ピレン系樹脂であり、そして、未変性ポリオレフィン
(C)が、23℃における引張弾性率が200MPa以
下のエチレン−α−オレフィン共重合体であることを特
徴とする熱可塑性樹脂組成物である。
That is, the present invention relates to polyamide (A),
In a resin composition comprising a modified polyolefin (B) and an unmodified polyolefin (C), the polyamide (A) is 30 to 80% by weight and the modified polyolefin (B) is 5 to 50% by weight based on the entire resin composition. , And 5 to 65% by weight of the unmodified polyolefin (C) (however,
The total amount of (A), (B) and (C) is 100% by weight), and the modified polyolefin (B) is modified with α, β-unsaturated carboxylic acid anhydride and its derivative.
A crystalline polypropylene resin having a flexural modulus of 1 GPa or more at 0 ° C., and the unmodified polyolefin (C) is an ethylene-α-olefin copolymer having a tensile modulus of 20 MPa or less at 23 ° C. It is a thermoplastic resin composition.

【0029】本発明の熱可塑性樹脂組成物は、前述した
ように、ポリアミドの有する機械的強度、耐熱性および
成形性と、ポリオレフィンの有する軽量性および低吸水
性とをバランスよく備え、さらに、両樹脂に不足してい
る、成形時の低反り性、寸法安定性および耐衝撃性を兼
ね備えたポリアミド−ポリプロピレン系樹脂組成物であ
る。
As described above, the thermoplastic resin composition of the present invention has a good balance of the mechanical strength, heat resistance and moldability of polyamide, and the light weight and low water absorption of polyolefin. It is a polyamide-polypropylene resin composition having low warpage during molding, dimensional stability, and impact resistance, which are lacking in resin.

【0030】そこで、本発明において、上記課題を達成
する手段としては、熱可塑性ポリアミドと、前記特定の
曲げ弾性率を有する、α、β−不飽和カルボン酸無水物
およびその誘導体で変性された結晶性ポリプロピレン系
樹脂と、さらに、未変性のエチレン−α−オレフィン共
重合体ゴムとを前記特定の割合で配合してなる樹脂組成
物において、前記ポリアミドを連続相(マトリックス
相)と成し、前記変性された結晶性ポリプロピレン系樹
脂と、さらに、前記未変性の結晶性のエチレン−α−オ
レフィン共重合体ゴムとからなるポリオレフィン成分
は、コアーシェル型の複合粒子分散相を形成させること
によるのである。
Therefore, in the present invention, as means for achieving the above object, crystals modified with a thermoplastic polyamide and an α, β-unsaturated carboxylic acid anhydride and a derivative thereof having the above-mentioned specific flexural modulus. In a resin composition obtained by blending a water-soluble polypropylene-based resin and an unmodified ethylene-α-olefin copolymer rubber in the above-mentioned specific ratio, the polyamide being a continuous phase (matrix phase), This is because the polyolefin component composed of the modified crystalline polypropylene resin and the unmodified crystalline ethylene-α-olefin copolymer rubber forms a core-shell type composite particle dispersed phase.

【0031】以下に本発明について詳細に説明する。本
発明の樹脂組成物に用いられるポリアミド(A)として
は、ヘキサメチレンジアミン、デカメチレンジアミン、
ドデカメチレンジアミン、2,2,4−または2,4,
4−トリメチルヘキサメチレンジアミン、1,3−また
は1,4−ビス(アミノメチル)シクロヘキサン、ビス
(p−アミノシクロヘキシルメタン)、m−またはp−
キシリレンジアミンなどの脂肪族、脂環族および芳香族
などのジアミンとアジピン酸、スベリン酸、セバシン
酸、シクロヘキサンジカルボン酸、テレフタル酸、イソ
フタル酸などの脂肪族、脂環族および芳香族などのジカ
ルボン酸との重縮合によって得られるポリアミド、ε−
カプロラクタム、ω−ラウロラクタムなどのラクタムか
ら得られるポリアミド、あるいは、これらの成分からな
る共重合ポリアミド、これらポリアミドおよび/または
共重合ポリアミドの混合物などが例示される。
The present invention will be described in detail below. Examples of the polyamide (A) used in the resin composition of the present invention include hexamethylenediamine, decamethylenediamine,
Dodecamethylenediamine, 2,2,4- or 2,4
4-trimethylhexamethylenediamine, 1,3- or 1,4-bis (aminomethyl) cyclohexane, bis (p-aminocyclohexylmethane), m- or p-
Diamines such as aliphatic, alicyclic and aromatic such as xylylenediamine and dicarboxylic acids such as adipic acid, suberic acid, sebacic acid, cyclohexanedicarboxylic acid, terephthalic acid, isophthalic acid, etc. Polyamide obtained by polycondensation with acid, ε-
Examples thereof include polyamides obtained from lactams such as caprolactam and ω-laurolactam, copolymerized polyamides containing these components, and mixtures of these polyamides and / or copolymerized polyamides.

【0032】具体的には、ナイロン6、ナイロン66、
ナイロン46、ナイロン610、ナイロン612、ナイ
ロン9、ナイロン11、ナイロン12、ナイロン6/6
6、ナイロン66/610、ナイロン6/9、ナイロン
6/11、ナイロン6/12、ナイロン6/610、ナ
イロン6/612、ナイロン6/66/610、ナイロ
ン6/66/612、ナイロン6T(T:テレフタル酸
成分)、ナイロン6I(I:イソフタル酸成分)、ナイ
ロン6/6T、ナイロン6/6I、ナイロン66/6
T、ナイロン66/6Iなどが挙げられる。これらのう
ち成形性、機械的物性バランスおよびコストの点から
は、ナイロン6、ナイロン66、ナイロン11、ナイロ
ン12、ナイロン6/66、ナイロン6T、ナイロン6
6/6Tなどの使用が好ましい。特に好ましくは、ナイ
ロン6、ナイロン66、および、これらの共重合体、な
らびにそれらの混合物である。また、前記成分(A)と
して用いるポリアミドの分子量としては、特に限定され
るものではないが、98%硫酸溶液中におけるポリマー
濃度1g/dlで測定された相対粘度が1.0以上、好
ましくは2.0〜4.0のものが好ましい。ポリアミド
の相対粘度が2.0未満では、最終的に得られるポリア
ミド樹脂組成物の機械的強度が低下することがあり、
1.0未満になると、このポリアミド樹脂組成物の機械
的強度の低下が顕著である。また、ポリアミドの相対粘
度が4.0を越えると、このポリアミド−ポリプロピレ
ン系樹脂組成物の溶融粘度が高くなり、成形性の低下な
どが生じる。
Specifically, nylon 6, nylon 66,
Nylon 46, Nylon 610, Nylon 612, Nylon 9, Nylon 11, Nylon 12, Nylon 6/6
6, nylon 66/610, nylon 6/9, nylon 6/11, nylon 6/12, nylon 6/610, nylon 6/612, nylon 6/66/610, nylon 6/66/612, nylon 6T (T : Terephthalic acid component), nylon 6I (I: isophthalic acid component), nylon 6 / 6T, nylon 6 / 6I, nylon 66/6
T, nylon 66 / 6I and the like. Of these, nylon 6, nylon 66, nylon 11, nylon 12, nylon 6/66, nylon 6T, nylon 6 are considered in terms of moldability, balance of mechanical properties, and cost.
The use of 6 / 6T or the like is preferable. Particularly preferred are nylon 6, nylon 66, copolymers thereof, and mixtures thereof. The molecular weight of the polyamide used as the component (A) is not particularly limited, but the relative viscosity measured at a polymer concentration of 1 g / dl in a 98% sulfuric acid solution is 1.0 or more, preferably 2 It is preferably from 0.0 to 4.0. If the relative viscosity of the polyamide is less than 2.0, the mechanical strength of the finally obtained polyamide resin composition may decrease.
If it is less than 1.0, the mechanical strength of this polyamide resin composition is significantly reduced. Further, when the relative viscosity of the polyamide exceeds 4.0, the melt viscosity of the polyamide-polypropylene resin composition becomes high, resulting in deterioration of moldability.

【0033】本発明の樹脂組成物の成分(B)として用
いられる変性ポリオレフィンは、α、β−不飽和カルボ
ン酸あるいはその誘導体で変性された結晶性ポリオレフ
ィンであり、後述する曲げ弾性率が1GPa以上の結晶
性ポリプロピレン系樹脂を、α、β−不飽和カルボン酸
あるいはその誘導体で変性させたものである。ここで用
いられるα、β−不飽和カルボン酸あるいはその誘導体
としては、アクリル酸、メタクリル酸、クロトン酸、イ
ソクロトン酸などの一塩基性カルボン酸、マレイン酸、
フマール酸、イタコン酸、シトラコン酸などの二塩基性
カルボン酸、および、これらの酸無水物あるいは塩であ
る。好ましくは、アクリル酸、メタクリル酸、無水マレ
イン酸、無水イタコン酸およびこれらの亜鉛塩やナトリ
ウム塩であり、特に好ましくは無水マレイン酸および無
水イタコン酸である。
The modified polyolefin used as the component (B) of the resin composition of the present invention is a crystalline polyolefin modified with α, β-unsaturated carboxylic acid or its derivative, and has a flexural modulus of 1 GPa or more as described later. Is a crystalline polypropylene resin modified with α, β-unsaturated carboxylic acid or its derivative. Examples of the α, β-unsaturated carboxylic acid or its derivative used herein include monobasic carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid and isocrotonic acid, maleic acid,
Dibasic carboxylic acids such as fumaric acid, itaconic acid and citraconic acid, and acid anhydrides or salts thereof. Acrylic acid, methacrylic acid, maleic anhydride, itaconic anhydride and their zinc salts and sodium salts are preferable, and maleic anhydride and itaconic anhydride are particularly preferable.

【0034】変性ポリオレフィン(B)中における、上
記α、β−不飽和カルボン酸およびその誘導体の含有量
は、0.05〜5重量%が好ましく、0.1〜3重量%
が特に好ましい。α、β−不飽和カルボン酸およびその
誘導体の含有量が上記範囲よりも低すぎると、ポリアミ
ドとポリオレフィン相の密着性が不十分であり、得られ
る樹脂組成物の組織構造が不安定になるとともに、機械
的強度が低くなる。また、上記範囲よりも高すぎると、
得られる樹脂組成物において溶融流動性の低下を来た
す。ポリオレフィンの変性方法としては、ポリオレフィ
ンの溶融状態あるいは溶液状態において、ポリオレフィ
ンと上記α、β−不飽和カルボン酸およびその誘導体
を、ラジカル開始剤(ヒドロペルオキシド、ジアルキル
ペルオキシド、ペルオキシエステルなどの有機過酸化物
など、例えば、ベンゾイルペルオキシド、ジクロルベン
ゾイルペルオキシド、ジクミルペルオキシド、シクロヘ
キサノンペルオキシド、t−ブチルペルオキシベンゾエ
ートなど)とともに、加熱攪拌する方法が挙げられる。
The content of the α, β-unsaturated carboxylic acid and its derivative in the modified polyolefin (B) is preferably 0.05 to 5% by weight, and 0.1 to 3% by weight.
Is particularly preferable. When the content of the α, β-unsaturated carboxylic acid and its derivative is lower than the above range, the adhesion between the polyamide and the polyolefin phase is insufficient and the resulting resin composition has an unstable structure structure. , The mechanical strength becomes low. If it is higher than the above range,
In the obtained resin composition, the melt fluidity is deteriorated. As a method for modifying a polyolefin, the polyolefin and the above α, β-unsaturated carboxylic acid and its derivative are mixed with a radical initiator (hydroperoxide, dialkyl peroxide, peroxy ester or other organic peroxide) in a molten state or a solution state of the polyolefin. Etc., for example, benzoyl peroxide, dichlorobenzoyl peroxide, dicumyl peroxide, cyclohexanone peroxide, t-butylperoxybenzoate, etc.) and the method of stirring under heating.

【0035】本発明の変性ポリオレフィン(B)構成す
る変性前のポリオレフィンは、結晶性ポリオレフィンで
あり、特には結晶性ポリプロピレン系樹脂である。この
結晶性ポリプロピレン系樹脂としては、プロピレン単独
重合体および、プロピレンと20モル%以下のエチレ
ン、1−ブテンなどのα−オレフィンとのブロックある
いはランダム共重合体を用いることができる。この中で
も、プロピレン単独重合体が高弾性率を有することか
ら、好ましい。さらに、上記成分(B)の分子量の目安
としては、ASTM D1238に従って測定される、
荷重2.16kg、230℃におけるメルトフローレー
ト(以下「MFR」と略記)が1g/10min以上、
好ましくは10〜200g/10minである。さらに
好ましくは10〜100g/10minであることが望
ましい。MFRが1g/10minより小さい場合は、
得られる熱可塑性樹脂組成物中におけるポリオレフィン
分散相のサイズが大きくなり、耐衝撃性などの破壊特性
が低くなるので好ましくない。なお、MFRが1〜10
g/10minの範囲では、この好ましくない現象が発
現する傾向がある。また、MFRが200g/10mi
nを越えると、成分(A)の溶融粘度に比較して成分
(B)の溶融粘度が低くなりすぎ、成分(A)が連続相
を形成するのが困難となり、得られる樹脂組成物の機械
的強度を低下させることになるし、100〜200g/
10minの範囲では、その傾向が見られるようにな
る。
The unmodified polyolefin constituting the modified polyolefin (B) of the present invention is a crystalline polyolefin, and particularly a crystalline polypropylene resin. As the crystalline polypropylene resin, a propylene homopolymer and a block or random copolymer of propylene and 20 mol% or less of α-olefin such as ethylene or 1-butene can be used. Among these, propylene homopolymer is preferable because it has a high elastic modulus. Further, as a measure of the molecular weight of the above component (B), it is measured according to ASTM D1238,
A load of 2.16 kg, a melt flow rate at 230 ° C. (hereinafter abbreviated as “MFR”) of 1 g / 10 min or more,
It is preferably 10 to 200 g / 10 min. More preferably, the amount is 10 to 100 g / 10 min. If the MFR is less than 1g / 10min,
This is not preferable because the size of the polyolefin dispersed phase in the obtained thermoplastic resin composition becomes large and the fracture properties such as impact resistance become low. In addition, MFR is 1-10
In the range of g / 10 min, this unfavorable phenomenon tends to occur. In addition, MFR is 200g / 10mi
When it exceeds n, the melt viscosity of the component (B) becomes too low as compared with the melt viscosity of the component (A), and it becomes difficult for the component (A) to form a continuous phase. Will decrease the mechanical strength, 100-200 g /
In the range of 10 min, the tendency becomes visible.

【0036】さらには、用いられる成分(B)の、AS
TM D790に従って測定される、23℃における曲
げ弾性率が1GPa以上、特には1.5GPa以上であ
ることが好ましい。曲げ弾性率が1GPa未満の場合、
得られる樹脂組成物の剛性が低くなり、本発明の目的を
達成することができない。
In addition, the component (B) used, AS
The flexural modulus at 23 ° C. measured according to TM D790 is preferably 1 GPa or more, particularly preferably 1.5 GPa or more. If the flexural modulus is less than 1 GPa,
The resulting resin composition has low rigidity, and the object of the present invention cannot be achieved.

【0037】次に、本発明のポリアミド−ポリプロピレ
ン系樹脂組成物の成分(C)として用いられる未変性ポ
リオレフィン共重合体は、ポリα−オレフィン共重合体
であり、後述するα−オレフィンから選ばれる少なくと
も2種以上の単量体を共重合して得られ、ASTM D
638に従って測定される、23℃における引張弾性率
が200MPa以下であるα−オレフィン共重合体であ
る。上記成分(C)として用いられる未変性ポリオレフ
ィン共重合体を構成するα−オレフィン成分単位として
は、炭素原子数2以上、特に2〜18のα−オレフィン
であり、エチレン、プロピレン、1−ブテン、1−ペン
テン、1−ヘキセン、1−ヘプテン、1−オクテン、1
−デセンなどを例示することができ、これらの1種また
は2種以上の混合物である。これらのオレフィンモノマ
ー単位のうち、エチレンが必須単位であり、その共重合
モノマー単位としてプロピレン、1−ブテンが好ましく
用いられる。そして、成分(C)として用いられる未変
性ポリオレフィン共重合体の共重合組成としては、エチ
レン単位が30〜85モル%、好ましくは45〜85モ
ル%である。エチレン含量がこの範囲より低い場合は、
前記成分(B)と上述の成分(C)との親和性が不十分
で、組織構造が不安定となるとともに、得られる樹脂組
成物の機械的強度が低くなる。エチレン含量がこの範囲
より高い場合には、耐衝撃性の改良効果が小さくなると
ともに、成形固化時の収縮が大きくなり、ポリアミド樹
脂組成物成形品の寸法安定性が低くなる。なお、これら
の好ましくない現象の発生を確実に抑えるためには、エ
チレン含量は前述の好ましい範囲にするのがよい。
Next, the unmodified polyolefin copolymer used as the component (C) of the polyamide-polypropylene resin composition of the present invention is a poly α-olefin copolymer and is selected from α-olefins described later. Obtained by copolymerizing at least two kinds of monomers,
The α-olefin copolymer has a tensile elastic modulus at 23 ° C. of 200 MPa or less measured according to 638. The α-olefin component unit constituting the unmodified polyolefin copolymer used as the component (C) is an α-olefin having 2 or more carbon atoms, particularly 2 to 18 carbon atoms, ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1
-Decene and the like can be exemplified, and these are one kind or a mixture of two or more kinds. Of these olefin monomer units, ethylene is an essential unit, and propylene and 1-butene are preferably used as its copolymerization monomer unit. The copolymer composition of the unmodified polyolefin copolymer used as the component (C) has an ethylene unit content of 30 to 85 mol%, preferably 45 to 85 mol%. If the ethylene content is below this range,
The affinity between the component (B) and the above-mentioned component (C) is insufficient, the tissue structure becomes unstable, and the mechanical strength of the obtained resin composition becomes low. When the ethylene content is higher than this range, the effect of improving the impact resistance becomes small, the shrinkage at the time of molding and solidification becomes large, and the dimensional stability of the molded product of the polyamide resin composition becomes low. In addition, in order to surely suppress the occurrence of these unfavorable phenomena, it is preferable that the ethylene content be within the above-mentioned preferable range.

【0038】さらに、成分(C)は、分子鎖に沿ったモ
ノマー単位の配列においてエチレン以外のα−オレフィ
ン単位が3個連続して存在する確率が0.5以下である
ことが好ましい。この範囲を逸脱する場合は、得られる
樹脂組成物の引張強度および耐衝撃性が改良されない場
合があるので好ましくない。また、成分(C)は、室温
で柔軟性のものが適しており、ASTM D638に従
って測定される、23℃における引張弾性率が200M
Pa以下のものが好ましい。引張弾性率がこれより高い
と、得られる樹脂組成物の耐衝撃性が低くなるととも
に、成形収縮率や成形時の反りの改善効果が十分でない
場合がある。
Further, the component (C) preferably has a probability of 0.5 or less of the presence of three consecutive α-olefin units other than ethylene in the arrangement of the monomer units along the molecular chain. If it deviates from this range, the tensile strength and impact resistance of the obtained resin composition may not be improved, which is not preferable. Further, as the component (C), one that is flexible at room temperature is suitable, and has a tensile elastic modulus of 200 M at 23 ° C. measured according to ASTM D638.
It is preferably Pa or less. If the tensile modulus is higher than this range, the resulting resin composition may have low impact resistance and the effect of improving molding shrinkage and warpage during molding may not be sufficient.

【0039】さらにはまた、上記成分(C)の分子量の
目安としては、ASTM D1238に従って測定され
る、荷重2.16kg、230℃におけるMFRが0.
5g/10min以上、好ましくは2〜60g/10m
inである。MFRが0.5g/10minより小さい
場合は、得られる熱可塑性樹脂組成物中におけるポリオ
レフィン分散相のサイズが大きくなり、耐衝撃性などの
破壊特性が低くなるので好ましくない。なお、MFRが
0.5〜2g/10minの範囲では、この好ましくな
い現象が発現する傾向がある。また、MFRが60g/
10minを越えると、成分(A)の溶融粘度に比較し
て成分(C)の溶融粘度が低くなりすぎ、成分(A)が
連続相を形成するのが困難になり、得られる樹脂組成物
の機械的強度を低下させることになる。
Furthermore, as a measure of the molecular weight of the above-mentioned component (C), the MFR at 230 ° C. under a load of 2.16 kg measured according to ASTM D1238 is 0.
5g / 10min or more, preferably 2-60g / 10m
in. If the MFR is less than 0.5 g / 10 min, the size of the polyolefin dispersed phase in the obtained thermoplastic resin composition will be large, and the fracture characteristics such as impact resistance will be unfavorable. In addition, when the MFR is in the range of 0.5 to 2 g / 10 min, this undesirable phenomenon tends to occur. Also, MFR is 60g /
If it exceeds 10 min, the melt viscosity of the component (C) becomes too low as compared with the melt viscosity of the component (A), and it becomes difficult for the component (A) to form a continuous phase. It will reduce the mechanical strength.

【0040】本発明のポリアミド−ポリプロピレン系樹
脂組成物においてはさらにまた、前記成分(C)は、極
性基あるいは反応性基で変性されていないことが必要で
ある。前記成分(C)がポリアミドと反応する残基ある
いは親和性のある残基で変性されていると、得られる樹
脂組成物において、ポリオレフィン相はコアーシェル型
分散構造を形成せず、後述するポリオレフィンコアーシ
ェル構造の有利な特性が得られない。
In the polyamide-polypropylene resin composition of the present invention, it is also necessary that the component (C) is not modified with a polar group or a reactive group. When the component (C) is modified with a residue that reacts with polyamide or a residue that has an affinity, in the resulting resin composition, the polyolefin phase does not form a core-shell type dispersed structure, and the polyolefin core-shell described below is formed. No advantageous properties of the structure are obtained.

【0041】ところで、本発明の樹脂組成物は、ポリア
ミド(A)をマトリックス相とすることが不可欠であ
る。ポリアミド成分(A)が連続相を形成することによ
り、耐熱性および機械的特性における優れたポリアミド
の特性を、得られる樹脂組成物の特性に大きく反映させ
ることができ、弾性率、耐熱性および破壊強度の優れた
樹脂組成物を得ることができる。ポリアミド成分(A)
が不連続相を形成すると、得られる樹脂組成物の機械的
特性や耐熱性は低くなり、本発明の目的を達することが
できない。
In the resin composition of the present invention, it is essential that the polyamide (A) is used as the matrix phase. By forming a continuous phase with the polyamide component (A), the excellent properties of the polyamide in terms of heat resistance and mechanical properties can be largely reflected in the properties of the resin composition obtained, and the elastic modulus, heat resistance and fracture properties can be improved. A resin composition having excellent strength can be obtained. Polyamide component (A)
If a discontinuous phase is formed, the resin composition obtained has poor mechanical properties and heat resistance, and the object of the present invention cannot be achieved.

【0042】一方、本発明の樹脂組成物において、前記
の成分(B)および成分(C)で形成される分散相は、
コアーシェル構造を有する複合粒子型分散構造を呈する
ことが必要である。該コアーシェル構造において、変性
ポリオレフィン成分(B)がシェル相を、そして、未変
性ポリオレフィン成分(C)がコア相を形成することに
より、曲げ弾性率、引張および曲げ強度、および耐衝撃
性などの機械特性に優れ、かつ、溶融粘度が低く、成形
時の流動性に優れた本発明の目的を満足する樹脂組成物
を得ることができる。両ポリオレフィン成分として、い
ずれもポリアミドと親和性を有する極性基で変性された
ものを用いた場合、それぞれのポリオレフィンは、ポリ
アミドマトリックス相中で、個別に分散し、上記のコア
ーシェル構造の優位性を得ることができない。
On the other hand, in the resin composition of the present invention, the dispersed phase formed by the above-mentioned components (B) and (C) is
It is necessary to exhibit a composite particle type dispersion structure having a core-shell structure. In the core-shell structure, the modified polyolefin component (B) forms a shell phase, and the unmodified polyolefin component (C) forms a core phase, whereby mechanical properties such as flexural modulus, tensile and flexural strength, and impact resistance are obtained. It is possible to obtain a resin composition having excellent properties, low melt viscosity, and excellent fluidity during molding, which satisfies the object of the present invention. When both polyolefin components modified with polar groups having an affinity for polyamide are used, each polyolefin is dispersed individually in the polyamide matrix phase to obtain the above-mentioned superiority of the core-shell structure. I can't.

【0043】本発明の樹脂組成物における前記成分
(A)、成分(B)および成分(C)の配合割合は、ポ
リアミド(成分A)が30〜80重量%、変性ポリオレ
フィン(成分B)が5〜50重量%、および、未変性ポ
リオレフィン(成分C)が5〜65重量%(ただし、成
分(A)と成分(B)と成分(C)の合計は100重量
%)である。なお、前記成分(B)の配合割合は、好ま
しくは10〜45重量%である。そして、前記成分
(C)の好ましい配合割合としては、10〜40重量%
である。
In the resin composition of the present invention, the mixing ratio of the component (A), the component (B) and the component (C) is 30 to 80% by weight of the polyamide (component A) and 5 of the modified polyolefin (component B). ˜50 wt%, and 5 to 65 wt% unmodified polyolefin (component C) (however, the total of the component (A), the component (B) and the component (C) is 100 wt%). The blending ratio of the component (B) is preferably 10 to 45% by weight. And as a preferable compounding ratio of the said component (C), it is 10-40 weight%.
Is.

【0044】成分(A)が80重量%を越えるようにな
ると、得られる樹脂組成物の吸水性の改良効果が不十分
で、吸湿による成形品の寸法変化が大きくなるので好ま
しくない。また、成分(A)の配合割合が30重量%未
満になると、ポリアミド相(成分A)の連続性が保持さ
れなくなり、機械的特性および耐熱性の低下を来たすの
で好ましくない。
When the amount of the component (A) exceeds 80% by weight, the effect of improving the water absorption of the obtained resin composition is insufficient and the dimensional change of the molded product due to moisture absorption becomes large, which is not preferable. On the other hand, if the mixing ratio of the component (A) is less than 30% by weight, the continuity of the polyamide phase (component A) cannot be maintained, resulting in deterioration of mechanical properties and heat resistance, which is not preferable.

【0045】さらに、本発明の樹脂組成物における成分
(B)の配合割合が5重量%未満では、ポリアミド成分
とポリオレフィン成分の相溶性が悪くなるとともに、得
られる樹脂組成物において、目的とするレベルの低吸水
性と曲げ弾性率を得ることができない。また、成分
(B)の配合割合が50重量%を越えると、本発明の目
的とする機械的特性および耐熱性を有する樹脂組成物を
得ることができない。これら、樹脂組成物中における成
分(B)の配合割合が範囲を外れる場合の上述の好まし
くない現象を確実に発生させないようにするには、成分
(B)の配合割合は、前述の好ましい範囲にすべきであ
る。
Further, when the blending ratio of the component (B) in the resin composition of the present invention is less than 5% by weight, the compatibility of the polyamide component and the polyolefin component is deteriorated, and the desired level is obtained in the obtained resin composition. It is not possible to obtain low water absorption and flexural modulus. Further, if the blending ratio of the component (B) exceeds 50% by weight, a resin composition having the mechanical properties and heat resistance targeted by the present invention cannot be obtained. In order to prevent the occurrence of the above-mentioned unfavorable phenomenon when the compounding ratio of the component (B) in the resin composition is out of the range, the compounding ratio of the component (B) falls within the above-mentioned preferred range. Should.

【0046】本発明の樹脂組成物における成分(C)、
つまり未変性ポリオレフィンの配合割合が65重量%を
越える場合には、成分(C)が連続相を形成し、曲げ弾
性率が低くなり、本発明の目的を満足することができな
い。一方、成分(C)の配合割合が5重量%未満になる
と、耐衝撃性が低くなるとともに、成形時の収縮率が大
きくなり、適当でない。なお、成分(C)の配合割合に
おいても、成分(B)の場合と同様、上述の好ましくな
い現象の発生を確実に抑えるためには、前述の好ましい
範囲にすべきである。
Component (C) in the resin composition of the present invention,
That is, when the blending ratio of the unmodified polyolefin exceeds 65% by weight, the component (C) forms a continuous phase and the flexural modulus becomes low, so that the object of the present invention cannot be satisfied. On the other hand, if the blending ratio of the component (C) is less than 5% by weight, the impact resistance becomes low and the shrinkage rate at the time of molding becomes large, which is not suitable. It should be noted that the mixing ratio of the component (C) should be within the above-mentioned preferable range in order to surely suppress the occurrence of the above-mentioned unfavorable phenomenon, as in the case of the component (B).

【0047】本発明の樹脂組成物の製造方法は、特に限
定されるものではなく、種々公知の方法が用いられ得
る。例えば、前述したような本発明の配合割合で成分
(A)、(B)および(C)を室温で予備混合した後、
これら各成分の溶融が十分に進行し、かつ、分解しない
温度として、220℃以上、好ましくは240〜300
℃の温度で、溶融混練する方法を適用することができ
る。予備混合は、通常の混合に使用されるヘンシェルミ
キサーなどの高速回転混合機およびコーンブレンダー、
タンブラーなどの低速回転混合機などの使用により行う
ことができる。また、溶融混練は、単軸あるいは二軸押
出機、バンバリーミキサー、ニーダーなどの通常の溶融
混練加工機を使用して行うことができる。
The method for producing the resin composition of the present invention is not particularly limited, and various known methods can be used. For example, after pre-mixing the components (A), (B) and (C) in the mixing ratio of the present invention as described above at room temperature,
The temperature at which the melting of each of these components is sufficiently advanced and does not decompose is 220 ° C. or higher, preferably 240 to 300.
A method of melt-kneading can be applied at a temperature of ° C. Pre-mixing is a high speed rotary mixer and cone blender such as a Henschel mixer used for normal mixing,
It can be performed by using a low speed rotating mixer such as a tumbler. Further, the melt-kneading can be performed using a normal melt-kneading processing machine such as a single-screw or twin-screw extruder, a Banbury mixer, a kneader.

【0048】本発明のポリアミド−ポリプロピレン系樹
脂組成物は、成形性および物性を損なわない範囲で繊維
状、粉末状、フレーク状あるいはマット状などの各種形
状の強化材や充填剤を添加配合することができる。これ
ら強化材および充填剤の具体例としては、ガラス繊維、
アスベスト繊維、炭素繊維、シリカ繊維、シリカ・アル
ミナ繊維、アルミナ繊維、ジルコニア繊維、窒化ホウ素
繊維、窒化ケイ素繊維、塩基性硫酸マグネシウム繊維、
ホウ素繊維、ステンレス繊維、アルミニウム、チタン、
銅、真ちゅう、マグネシウムなどの無機質および金属繊
維、およびポリアミド、ポリエステル、ポリアクリロニ
トリル、セルロースなどの有機質繊維、銅、鉄、ニッケ
ル、亜鉛、錫、鉛、ステンレス、アルミニウム、金、銀
などの金属粉末、ヒュームドシリカ、ケイ酸アルミニウ
ム、ガラスビーズ、カーボンブラック、石英粉末、タル
ク、酸化チタン、酸化鉄、炭酸カルシウム、酸化マグネ
シウム、酸化カルシウム、硫酸マグネシウム、ケイソウ
土などが挙げられる。繊維状物質の場合は、平均繊維径
が0.1〜30μm、繊維長/繊維径の比が10以上の
ものが好ましく使用される。これらの強化材および充填
剤は、公知のシランカップリング剤やチタネート系カッ
プリング剤などで表面処理されたものでもよい。
The polyamide-polypropylene resin composition of the present invention may be added with various types of reinforcing agents and fillers in various shapes such as fibrous, powdery, flake-like or matte-like form within a range not impairing moldability and physical properties. You can Specific examples of these reinforcing materials and fillers include glass fiber,
Asbestos fiber, carbon fiber, silica fiber, silica-alumina fiber, alumina fiber, zirconia fiber, boron nitride fiber, silicon nitride fiber, basic magnesium sulfate fiber,
Boron fiber, stainless fiber, aluminum, titanium,
Inorganic and metal fibers such as copper, brass and magnesium, and organic fibers such as polyamide, polyester, polyacrylonitrile and cellulose, metal powders such as copper, iron, nickel, zinc, tin, lead, stainless steel, aluminum, gold and silver, Examples include fumed silica, aluminum silicate, glass beads, carbon black, quartz powder, talc, titanium oxide, iron oxide, calcium carbonate, magnesium oxide, calcium oxide, magnesium sulfate and diatomaceous earth. In the case of a fibrous substance, those having an average fiber diameter of 0.1 to 30 μm and a fiber length / fiber diameter ratio of 10 or more are preferably used. These reinforcing materials and fillers may be surface-treated with known silane coupling agents or titanate coupling agents.

【0049】前記強化材および充填剤の使用量は、本発
明の樹脂組成物100重量部に対して1〜300重量
部、好ましくは10〜250重量部である。使用量が1
重量部未満では、強化材および充填剤の添加効果が認め
られず、300重量部を越えると、ポリアミド−ポリプ
ロピレン系樹脂組成物の成形性や機械的物性の低下が生
じるので、いずれの場合も好ましくない。なお、これら
の強化材や充填剤は、単独でも、2種類以上を混合して
用いてもよい。
The amount of the reinforcing material and the filler used is 1 to 300 parts by weight, preferably 10 to 250 parts by weight, based on 100 parts by weight of the resin composition of the present invention. 1 usage
If the amount is less than parts by weight, the effect of adding the reinforcing material and the filler is not recognized, and if it exceeds 300 parts by weight, the moldability and mechanical properties of the polyamide-polypropylene resin composition are deteriorated. Absent. These reinforcing materials and fillers may be used alone or in combination of two or more.

【0050】さらに、本発明のポリアミド−ポリプロピ
レン系樹脂組成物に、必要に応じて、ヒンダードフェノ
ール、ハイドロキノン、チオエーテル、ホスファイト、
アミン類およびこれらの置換体や銅化合物などの酸化防
止剤や熱安定剤、レゾルシノール、サリシレート、ベン
ゾトリアゾール、ベンゾフェノンなどの紫外線吸収剤、
ステアリン酸およびその塩、ステアリルアルコールなど
の離型剤、水酸化マグネシウム、水酸化カルシウム、ハ
イドロタルサイトなどの無機難燃剤、ハロゲン系、リン
酸エステル系、メラミンあるいはシアヌル酸系の有機難
燃剤、三酸化アンチモンなどの難燃助剤、ドデシルベン
ゼンスルフォン酸ナトリウム、ポリアルキレングリコー
ルなどの帯電防止剤、その他結晶化促進剤、染料、顔料
などの添加剤を1種類以上添加することが可能である。
Furthermore, if necessary, the polyamide-polypropylene resin composition of the present invention may contain a hindered phenol, hydroquinone, thioether, phosphite,
Antioxidants and heat stabilizers such as amines and their substitution products and copper compounds, UV absorbers such as resorcinol, salicylate, benzotriazole and benzophenone,
Stearic acid and its salts, release agents such as stearyl alcohol, inorganic flame retardants such as magnesium hydroxide, calcium hydroxide and hydrotalcite, halogen-based, phosphate ester-based, melamine or cyanuric acid-based organic flame retardants, It is possible to add one or more flame retardant aids such as antimony oxide, antistatic agents such as sodium dodecylbenzene sulfonate, polyalkylene glycols, and other additives such as crystallization accelerators, dyes and pigments.

【0051】また、本発明のポリアミド−ポリプロピレ
ン系樹脂組成物は、本発明の目的を損なわない範囲で、
適量のポリエチレン、エチレン・プロピレン共重合体、
エチレン・1−ブテン共重合体、エチレン・4−メチレ
ン−1−ペンテン共重合体、エチレン・1−オクテン共
重合体、エチレン・酢酸ビニル共重合体、エチレン・ビ
ニルアルコール共重合体、ポリ酢酸ビニル、ポリ塩化ビ
ニルなどのビニル化合物重合体、ポリ1−ブテン、ポリ
4−メチル−1−ペンテンなどのポリオレフィン、ポリ
アミド、ポリアミドエラストマー、ポリエステルエラス
トマー、ポリエチレンテレフタレート、ポリブチレンテ
レフタレートなどの熱可塑性ポリエステル、ポリカーボ
ネート、ポリサルフォン、ポリフェニレンエーテル、ポ
リフェニレンサルファイドなどの熱可塑性樹脂や、フェ
ノール樹脂、メラミン樹脂、尿素樹脂、シリコーン樹
脂、エポキシ樹脂などの熱硬化性樹脂を添加することが
できる。
Further, the polyamide-polypropylene resin composition of the present invention is within the range not impairing the object of the present invention.
Proper amount of polyethylene, ethylene-propylene copolymer,
Ethylene / 1-butene copolymer, ethylene-4-methylene-1-pentene copolymer, ethylene / 1-octene copolymer, ethylene / vinyl acetate copolymer, ethylene / vinyl alcohol copolymer, polyvinyl acetate , Vinyl compound polymer such as polyvinyl chloride, polyolefin such as poly 1-butene, poly 4-methyl-1-pentene, polyamide, polyamide elastomer, polyester elastomer, polyethylene terephthalate, thermoplastic polyester such as polybutylene terephthalate, polycarbonate, Thermoplastic resins such as polysulfone, polyphenylene ether and polyphenylene sulfide, and thermosetting resins such as phenol resin, melamine resin, urea resin, silicone resin and epoxy resin can be added.

【0052】本発明のポリアミド−ポリプロピレン系樹
脂組成物は、前記の(A)、(B)および(C)の3成
分の他に、必要により添加する、前述したような添加剤
を所定量配合してなる樹脂組成物であるが、その配合の
順序については特に制限はなく、各成分を同時に配合し
てもよく、また、前記(A)、(B)および(C)の成
分を先ず配合して混合物を製造した後、添加剤などの他
の成分を配合してもよい。
The polyamide-polypropylene resin composition of the present invention contains, in addition to the above-mentioned three components (A), (B) and (C), a predetermined amount of the above-mentioned additive which is optionally added. However, the order of compounding is not particularly limited, and each component may be compounded at the same time, and the components (A), (B) and (C) are first compounded. After the mixture is produced by the above process, other components such as additives may be added.

【0053】上述のようにして得られた本発明のポリア
ミド−ポリプロピレン系樹脂組成物は、射出成形、圧縮
成形および押出成形などにより各種用途の成形品に加工
することができる。
The polyamide-polypropylene resin composition of the present invention obtained as described above can be processed into molded articles for various uses by injection molding, compression molding, extrusion molding and the like.

【0054】[0054]

【実施例】以下に、実施例および比較例に基づいて本発
明をさらに詳しく説明する。ただし、本発明はその要旨
を越えない限り、これら実施例に限定されるものではな
い。なお、以下の各実施例および比較例に記載する機械
的性質の測定は、下記に準じて行った。 (1)引張特性(引張強度および引張弾性率):AST
M D638 (2)曲げ弾性率:ASTM D790 (3)荷重たわみ温度:ASTM D648、荷重4.
6kg/cm2 (4)アイゾット衝撃強さ:ASTM D256
EXAMPLES The present invention will be described in more detail based on the following examples and comparative examples. However, the present invention is not limited to these examples as long as the gist thereof is not exceeded. The mechanical properties described in each of the following Examples and Comparative Examples were measured according to the following. (1) Tensile properties (tensile strength and tensile modulus): AST
M D638 (2) Flexural modulus: ASTM D790 (3) Deflection temperature under load: ASTM D648, load 4.
6kg / cm 2 (4) Izod impact strength: ASTM D256

【0055】(5)溶融粘度 ノズル直径/長さ=1/10(mm/mm)のノズルを
装着したプランジャー式キャピラリーレオメーターを用
い、設定温度280℃、剪断速度240sec -1におい
て測定した。
(5) Melt viscosity A nozzle having a nozzle diameter / length = 1/10 (mm / mm) is used.
Use the attached plunger-type capillary rheometer
Setting temperature 280 ° C, shear rate 240 sec -1smell
Measured.

【0056】(6)成形収縮率 ASTM 1号試験片(厚さ1/8インチ)を作製し、
流れ方向における成形試験片両端間の寸法と同方向の金
型内寸法との差の金型内寸法に対する割合を、流れ方向
の収縮率(%)として求めた。
(6) Molding Shrinkage ASTM No. 1 test piece (thickness 1/8 inch) was prepared,
The ratio of the difference between the dimension between both ends of the molded test piece in the flow direction and the dimension in the mold in the same direction to the dimension in the mold was determined as the shrinkage rate (%) in the flow direction.

【0057】(7)成形時反り 厚さ2mm、直径100mmの円板試験片を射出成形に
より作製し、三次元測定機を用いて、この試験片の直径
両端の最大反り量(mm)を測定した。
(7) Warpage during molding A disc test piece having a thickness of 2 mm and a diameter of 100 mm was produced by injection molding, and the maximum warp amount (mm) at both ends of the diameter of the test piece was measured using a three-dimensional measuring machine. did.

【0058】(8)吸水性 ASTM 4号試験片(厚さ1mm)の試験片を用い、
温度40℃、相対湿度90%の恒温恒湿器中に、190
時間静置し、成形後の絶対乾燥時(絶乾時)と吸水後の
重量から吸水重量増加率として、下記数式1により求め
た。
(8) Water Absorption Using a test piece of ASTM No. 4 test piece (thickness 1 mm),
190 in a thermo-hygrostat at a temperature of 40 ° C and a relative humidity of 90%.
It was allowed to stand for a period of time, and it was determined by the following mathematical formula 1 as the rate of increase in water absorption weight from the absolute dry time (in absolute dry condition) after molding and the weight after water absorption.

【0059】[0059]

【数1】 [Equation 1]

【0060】また、以下の各実施例および比較例におい
て用いられたポリアミド(成分A)、変性ポリオレフィ
ン(成分B)および未変性ポリオレフィン(成分C)の
諸物性は、下記の方法に従って測定した。 (a)相対粘度(ηr) JIS K6810に従い、98%硫酸溶液中のポリマ
ー濃度1g/dlの溶液中で25℃において測定した。
The physical properties of the polyamide (component A), modified polyolefin (component B) and unmodified polyolefin (component C) used in the following examples and comparative examples were measured according to the following methods. (A) Relative viscosity (ηr) According to JIS K6810, it was measured at 25 ° C. in a solution having a polymer concentration of 1 g / dl in a 98% sulfuric acid solution.

【0061】(b)ポリオレフィン共重合組成13 C−NMRスペクトルより、エチレン、プロピレン、
1−ブテンからなる3個のモノマー単位の連鎖分率から
エチレン単位の含有量を算出し、モル分率で表わした。
(B) Polyolefin copolymer composition From 13 C-NMR spectrum, ethylene, propylene,
The content of ethylene units was calculated from the chain fraction of three monomer units consisting of 1-butene, and expressed as a mole fraction.

【0062】(c)成分C中における3個の、エチレン
以外のオレフィン単位の連鎖分率13 C−NMRスペクトルより、α−オレフィンコモノマ
ーのトライアッドの連鎖の総量に対するPPPまたはB
BB(ただし、Pはプロピレン単位、Bは1−ブテン単
位を示す)の連鎖の分率を算出し、モル分率で表わし
た。
(C) From the chain fraction 13 C-NMR spectrum of three olefin units other than ethylene in component C, PPP or B for the total amount of triad chains of α-olefin comonomer is obtained.
The chain fraction of BB (wherein P represents a propylene unit and B represents a 1-butene unit) was calculated and expressed as a mole fraction.

【0063】(d)無水マレイン酸変性量 1785cm-1および840cm-1での赤外吸収スペク
トルの吸光度比より算出した。
(D) Maleic anhydride modification amount It was calculated from the absorbance ratio of infrared absorption spectra at 1785 cm -1 and 840 cm -1 .

【0064】(e)X線結晶化度 厚さ0.5mmのプレスシートを用い、2θ=5〜35
°の範囲のX線回折強度曲線において、2θ=16°を
ピークとする滑らかな曲線により、結晶部と非晶部とに
分離し、結晶部の面積の割合を求め、これをX線結晶化
度とした。
(E) X-ray crystallinity Using a press sheet having a thickness of 0.5 mm, 2θ = 5 to 35
In the X-ray diffraction intensity curve in the range of °, a smooth curve having a peak at 2θ = 16 ° is used to separate the crystalline part and the amorphous part, the ratio of the area of the crystalline part is determined, and this is X-ray crystallized. I took it.

【0065】(f)MFR メルトインデクサーを使用し、ASTM D1238に
従って、荷重2.16kg、230℃において測定し
た。
(F) Measured at 230 ° C. under a load of 2.16 kg according to ASTM D1238 using an MFR melt indexer.

【0066】実施例1〜5 ポリアミド(成分A)として、ナイロン66(PA6
6、ηr=2.51)と、変性ポリオレフィン(成分
B)として、表1に示すプロピレン含量、MFR、変性
基種および変性量、および曲げ弾性率を有する5種類の
変性された結晶性ポリプロピレン系樹脂(以下「PP」
と略記)のうち、PP1(無水マレイン酸変性ホモP
P、MFR:30g/10min、無水マレイン酸変性
量:0.2wt%、曲げ弾性率:1.9GPa)と、未
変性ポリオレフィン(成分C)として、表2に示すエチ
レン含量、3個のプロピレン単位の連鎖分率、X線結晶
化度、MFR、引張弾性率、変性基種および変性量を有
する5種類のエチレン−α−オレフィン共重合体ゴム
(以下「EPR」と略記)のうち、EPR1(エチレン
含量:82モル%、すなわち、プロピレン含量:18モ
ル%、MFR:9g/10min、引張弾性率:10M
Pa)とを、それぞれ表3に示す割合で、タンブラーを
用いてドライブレンド後、30mmφ二軸押出機を使用
して280℃で溶融混練し、樹脂組成物を得た。そし
て、得られた樹脂組成物を乾燥後、射出成形して物性測
定用の試験片を作製した。得られた樹脂組成物の物性を
表3に示す。
Examples 1 to 5 As a polyamide (component A), nylon 66 (PA6)
6 and ηr = 2.51), and as modified polyolefin (component B), five types of modified crystalline polypropylene systems having the propylene content, MFR, modifying group species and modification amount, and flexural modulus shown in Table 1. Resin (hereinafter "PP"
Abbreviated), PP1 (maleic anhydride modified homo P
P, MFR: 30 g / 10 min, maleic anhydride modification amount: 0.2 wt%, flexural modulus: 1.9 GPa) and ethylene content shown in Table 2 as an unmodified polyolefin (component C), three propylene units Of 5 kinds of ethylene-α-olefin copolymer rubbers (hereinafter abbreviated as “EPR”) having chain fraction, X-ray crystallinity, MFR, tensile elastic modulus, modifying group species and modifying amount of EPR1 ( Ethylene content: 82 mol%, that is, propylene content: 18 mol%, MFR: 9 g / 10 min, tensile elastic modulus: 10 M
Pa) and each of the ratios shown in Table 3 were dry blended using a tumbler and then melt-kneaded at 280 ° C. using a 30 mmφ twin-screw extruder to obtain a resin composition. Then, the obtained resin composition was dried and injection-molded to prepare a test piece for measuring physical properties. Table 3 shows the physical properties of the obtained resin composition.

【0067】[0067]

【表1】 [Table 1]

【0068】[0068]

【表2】 [Table 2]

【0069】[0069]

【表3】 [Table 3]

【0070】実施例6および7 成分BとしてPP1に代えて、実施例6および7におい
て、それぞれ、表1に示すPP2(ホモPP)およびP
P3(ブロックPP)を用いたこと、そして各成分の配
合割合を、実施例6および7とも、成分Aについては7
0重量%に変えて55重量%、成分Bについては20重
量%に変えて30重量%、成分Cについては10重量%
に変えて15重量%としたことの他は、実施例1と同様
にして表4に示す物性の樹脂組成物を得た。
Examples 6 and 7 Instead of PP1 as the component B, PP2 (homo PP) and P shown in Table 1 were obtained in Examples 6 and 7, respectively.
P3 (block PP) was used, and the blending ratio of each component was set to 7 for component A in both Examples 6 and 7.
55% by weight for 0% by weight, 30% by weight for 20% by weight for component B, 10% by weight for C
Was changed to 15% by weight, and a resin composition having the physical properties shown in Table 4 was obtained in the same manner as in Example 1.

【0071】比較例1および2 比較例1および2において、成分BとしてPP1に代え
て、それぞれ、表1に示すPP4(ランダムPP)およ
びPP5(ホモPP)を用いたことの他は、実施例6と
同様にして表4に示す物性の樹脂組成物を得た。
Comparative Examples 1 and 2 In Comparative Examples 1 and 2, PP4 (random PP) and PP5 (homo PP) shown in Table 1 were used instead of PP1 as the component B, respectively. A resin composition having the physical properties shown in Table 4 was obtained in the same manner as in 6.

【0072】[0072]

【表4】 [Table 4]

【0073】実施例8〜10 実施例8、9および10において、成分CとしてEPR
1に代えて、それぞれ、表2に示すEPR2、EPR3
およびEPR4を用いたこと、および、成分A、成分B
および成分Cを表5に示す配合割合としたことの他は、
実施例1と同様にして表5に示す物性の樹脂組成物を得
た。
Examples 8 to 10 EPR as component C in Examples 8, 9 and 10
1 instead of EPR2 and EPR3 shown in Table 2, respectively.
And using EPR4, and component A, component B
And that the composition ratio of Component C is shown in Table 5,
A resin composition having the physical properties shown in Table 5 was obtained in the same manner as in Example 1.

【0074】比較例3 成分CとしてEPR2に代えて、表2に示す無水マレイ
ン酸変性EPR(EPR5)を用いた他は、実施例8と
同様にして表5に示す物性の樹脂組成物を得た。
Comparative Example 3 A resin composition having the physical properties shown in Table 5 was obtained in the same manner as in Example 8 except that maleic anhydride-modified EPR (EPR5) shown in Table 2 was used as the component C instead of EPR2. It was

【0075】[0075]

【表5】 [Table 5]

【0076】実施例11 成分Aの配合割合を70重量%に変えて55重量%、成
分Bの配合割合を20重量%に変えて40重量%、そし
て成分Cの配合割合を10重量%に変えて5重量%とし
たことの他は、実施例1と同様にして表6に示す物性の
樹脂組成物を得た。
Example 11 The blending ratio of component A was changed to 70% by weight, 55% by weight, the blending ratio of component B was changed to 20% by weight, 40% by weight, and the blending ratio of component C was changed to 10% by weight. Was obtained in the same manner as in Example 1 except that the resin composition having the physical properties shown in Table 6 was obtained.

【0077】比較例4 成分Bを配合しなかったこと、および、成分Cの配合割
合を5重量%に変えて45重量%としたことの他は、実
施例11と同様にして表6に示す樹脂組成物を得た。
Comparative Example 4 Table 6 is the same as Example 11 except that the component B was not compounded and the compounding ratio of the component C was changed to 5% by weight to 45% by weight. A resin composition was obtained.

【0078】比較例5 成分Bの配合割合を40重量%に変えて45重量%と
し、そして成分Cを配合しなかったことの他は、実施例
11と同様にして表6に示す物性の樹脂組成物を得た。
Comparative Example 5 Resin having the physical properties shown in Table 6 was obtained in the same manner as in Example 11 except that the blending ratio of the component B was changed to 40% by weight to 45% by weight and the component C was not blended. A composition was obtained.

【0079】比較例6 成分Aの配合割合を70重量%に変えて25重量%、お
よび、成分Bの配合割合を20重量%に変えて65重量
%とした以外は、実施例1と同様にして表6に示す物性
の樹脂組成物を得た。
Comparative Example 6 The same as Example 1 except that the mixing ratio of the component A was changed to 70% by weight and 25% by weight, and the mixing ratio of the component B was changed to 20% by weight and 65% by weight. A resin composition having the physical properties shown in Table 6 was obtained.

【0080】[0080]

【表6】 [Table 6]

【0081】実施例12〜15ならびに比較例7および
8 成分Aとして、ナイロン66に代えてナイロン6(PA
6、ηr=2.3)を用い、成分A、成分Bおよび成分
Cの配合割合を70重量%、20重量%および10重量
%に変えて、それぞれ、表7に示す配合割合とした他
は、実施例1と同様にして樹脂組成物を得た。得られた
樹脂組成物の物性を表7に示す。
Examples 12 to 15 and Comparative Examples 7 and 8 As Component A, instead of nylon 66, nylon 6 (PA
6, ηr = 2.3) was used, and the mixing ratios of Component A, Component B, and Component C were changed to 70% by weight, 20% by weight, and 10% by weight, and the mixing ratios shown in Table 7 were obtained, respectively. A resin composition was obtained in the same manner as in Example 1. Table 7 shows the physical properties of the obtained resin composition.

【0082】[0082]

【表7】 [Table 7]

【0083】[0083]

【発明の効果】ポリアミド、不飽和カルボン酸およびそ
の誘導体で変性された結晶性ポリプロピレン系樹脂と未
変性のエチレン−α−オレフィン共重合体とを特定の割
合で配合してなり、ポリアミドをマトリックス相とする
本発明の樹脂組成物は、従来公知のポリアミド系樹脂組
成物に比べて、低吸水性、寸法安定性、軽量性、剛性お
よび靱性などの機械特性に優れ、かつ、成形加工性に優
れたポリアミド−ポリプロピレン系樹脂組成物であり、
機械部品、自動車部品、電気・電子部品などの広い分野
で使用できる。特に自動車用電装部品に好適に使用され
るものである。
EFFECT OF THE INVENTION A crystalline polypropylene resin modified with polyamide, an unsaturated carboxylic acid and its derivative and an unmodified ethylene-α-olefin copolymer are blended in a specific ratio, and the polyamide is used as a matrix phase. The resin composition of the present invention is excellent in mechanical properties such as low water absorption, dimensional stability, lightness, rigidity and toughness as compared with conventionally known polyamide resin compositions, and is excellent in molding processability. A polyamide-polypropylene resin composition,
It can be used in a wide range of fields such as mechanical parts, automobile parts, and electric / electronic parts. Particularly, it is preferably used for electric parts for automobiles.

───────────────────────────────────────────────────── フロントページの続き (72)発明者 松富 豊 大阪府枚方市中宮北町3番10号 宇部興産 株式会社枚方研究所内 ─────────────────────────────────────────────────── ─── Continuation of the front page (72) Inventor Yutaka Matsutomi 3-10 Nakamiyakitamachi, Hirakata-shi, Osaka Ube Industries Ltd. Hirakata Laboratory

Claims (1)

【特許請求の範囲】[Claims] 【請求項1】 ポリアミド(A)、変性ポリオレフィン
(B)および未変性ポリオレフィン(C)からなる樹脂
組成物において、該樹脂組成物全体に対して、ポリアミ
ド(A)が30〜80重量%、変性ポリオレフィン樹脂
(B)が5〜50重量%、および未変性ポリオレフィン
(C)が5〜65重量%(ただし、(A)と(B)と
(C)の合計は100重量%)からなり、ポリアミド
(A)がマトリックス相を形成する一方、変性ポリオレ
フィン(B)と未変性ポリオレフィン(C)とがコアー
シェル型粒子構造の分散相を呈する樹脂組成物であっ
て、かつ、変性ポリオレフィン(B)がα、β−不飽和
カルボン酸およびその誘導体で変性された、23℃にお
ける曲げ弾性率が1GPa以上の結晶性ポリプロピレン
系樹脂であり、そして、未変性ポリオレフィン(C)が
23℃における引張弾性率が200MPa以下である、
エチレン−α−オレフィン共重合体であることを特徴と
するポリアミド−ポリプロピレン系樹脂組成物。
1. A resin composition comprising a polyamide (A), a modified polyolefin (B) and an unmodified polyolefin (C), wherein 30 to 80% by weight of the polyamide (A) is modified with respect to the entire resin composition. The polyolefin resin (B) is 5 to 50% by weight, and the unmodified polyolefin (C) is 5 to 65% by weight (however, the total of (A), (B) and (C) is 100% by weight). (A) forms a matrix phase, while the modified polyolefin (B) and the unmodified polyolefin (C) are resin compositions exhibiting a dispersed phase having a core-shell type particle structure, and the modified polyolefin (B) is α , A crystalline polypropylene resin modified with a β-unsaturated carboxylic acid and its derivative and having a flexural modulus at 23 ° C. of 1 GPa or more, and Sex polyolefin (C) is a tensile modulus at 23 ° C. is not more than 200 MPa,
A polyamide-polypropylene resin composition, which is an ethylene-α-olefin copolymer.
JP6171187A 1994-05-20 1994-07-22 Polyamide-polypropylene resin composition Expired - Fee Related JP3013971B2 (en)