JPH08169976A - Heat-insulating resin foam and its production - Google Patents
Heat-insulating resin foam and its productionInfo
- Publication number
- JPH08169976A JPH08169976A JP7217390A JP21739095A JPH08169976A JP H08169976 A JPH08169976 A JP H08169976A JP 7217390 A JP7217390 A JP 7217390A JP 21739095 A JP21739095 A JP 21739095A JP H08169976 A JPH08169976 A JP H08169976A
- Authority
- JP
- Japan
- Prior art keywords
- fluorinated
- heat insulating
- insulating resin
- foam
- resin foam
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【0001】[0001]
【発明の属する技術分野】本発明は、冷蔵庫、冷凍庫あ
るいは建築用断熱材等に用いる断熱性樹脂発泡体および
新規な発泡剤を用いた断熱性樹脂発泡体の製造方法に関
するものである。BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a heat insulating resin foam used for a refrigerator, a freezer or a heat insulating material for construction, and a method for producing a heat insulating resin foam using a novel foaming agent.
【0002】[0002]
【従来の技術】近年、オゾン層破壊に対しフロンが大き
く影響するということが社会的問題となり、硬質ウレタ
ンフォーム等の断熱性発泡体の発泡剤であるトリクロロ
モノフルオロメタンなど特定フロンを1995年に全廃
することが決定されている。このため、オゾン破壊係数
(ODP)の小さな物質である1,1ージクロロー1−
フルオロエタン(HCFC−141b)、1,1ージク
ロロ−2,2,2−トリフルオロエタン(HCFC−1
23)等が発泡剤として用いられ、冷蔵庫等に実用化さ
れている。しかし、HCFC−141b、HCFC12
3は、分子構造の中にクロル基を有しており、オゾン破
壊係数がゼロではない。このため、これらは、過渡的な
代替物であり、長期的使用が可能な物質に置き換える必
要がある。2. Description of the Related Art In recent years, it has become a social problem that chlorofluorocarbon has a great influence on ozone layer depletion. It has been decided to abolish it. Therefore, 1,1-dichloro-1-, which is a substance with a low ozone depletion potential (ODP)
Fluoroethane (HCFC-141b), 1,1-dichloro-2,2,2-trifluoroethane (HCFC-1
23) and the like are used as a foaming agent and are put to practical use in refrigerators and the like. However, HCFC-141b, HCFC12
No. 3 has a chloro group in its molecular structure and its ozone depletion potential is not zero. For this reason, they are transient alternatives and need to be replaced by substances that can be used in the long term.
【0003】このような長期的使用が可能な発泡剤とし
て、シクロペンタンなどの炭化水素はハロゲン元素を含
まず、それ故にオゾン層を破壊しない等、化学的、物理
的性質並びに環境に対する性質において優位性を併せ持
っている化合物である旨発表されている(1993年5
月ポリウレタン国際フォーラム93の発表予稿集197
頁、ゲルハルトハイリッヒと木原良徳によって『ペンタ
ン発泡硬質ウレタンフォーム』)。また、その燃焼性は
製造技術上の安全対策とフォーム中の難燃剤の増量によ
って解決できることが開示されている。しかし、ペンタ
ンを発泡剤としたポリウレタンフォームは、HCFC−
141b、HCFC123などの従来の発泡剤を用いた
ポリウレタンフォームと比べて断熱性が悪い上に、燃
焼、爆発に対する安全性が低いという問題がある。Hydrocarbons such as cyclopentane do not contain a halogen element as a foaming agent that can be used for a long period of time, and therefore do not destroy the ozone layer. It has been announced that it is a compound having both properties (5 May 1993).
Monthly Polyurethanes International Forum 93 Proceedings 197
Page, "Pentane foaming rigid urethane foam" by Gerhard Heilich and Yoshinori Kihara). It is also disclosed that its flammability can be solved by safety measures in manufacturing technology and by increasing the amount of flame retardant in the foam. However, the polyurethane foam using pentane as the blowing agent is
Compared with polyurethane foams using conventional foaming agents such as 141b and HCFC123, there is a problem that the heat insulation is poor and the safety against combustion and explosion is low.
【0004】一方、同様なフロン代替発泡剤に、塩素の
全く含まれていないフルオロカーボン類が着目されてお
り、EPA351614(特開平2ー86635)にお
いて全フッ化した物質であるパーフルオロヘキサンを発
泡剤として使用したフォーム等が報告されている。気泡
内の気体の対流が無視できる程度の小さい気泡を有する
発泡体で構成された断熱体においては、その熱伝導率
は、気泡内に存在する気体による熱伝導と、気泡内での
熱輻射による熱伝導、および樹脂部の固体熱伝導の和で
表される。従って、前記のパーフルオロカーボン類のよ
うな全フッ素化物を発泡剤として用いる場合には、気泡
径を小さくして輻射成分を小さくすることと、密度を下
げて樹脂部の固体熱伝導の寄与を小さくすることが重要
である。On the other hand, fluorocarbons that do not contain chlorine at all have been attracting attention as a similar CFC substitute foaming agent. In EPA351614 (Japanese Patent Laid-Open No. 2-86635), perfluorohexane, which is a fully-fluorinated substance, is used as a foaming agent. The form etc. used as are reported. The thermal conductivity of a heat-insulating body composed of a foam having small bubbles in which the convection of the gas in the bubbles is negligible depends on the heat conduction by the gas present in the bubbles and the heat radiation in the bubbles. It is represented by the sum of heat conduction and solid heat conduction of the resin part. Therefore, when a perfluorinated compound such as the above-mentioned perfluorocarbons is used as a foaming agent, the bubble diameter is reduced to reduce the radiation component, and the density is reduced to reduce the contribution of solid heat conduction in the resin portion. It is important to.
【0005】通常、気泡径については、発泡核を導入す
ることによって気泡の微細化が行われる(例えば、特開
平3−54231号公報)。発泡核としては、パ−フル
オロペンタン等のパ−フルオロアルカンが利用されてい
る。パ−フルオロアルカンを乳化剤としてポリオール組
成物をエマルジョン化し、これにさらにシリカゲル、で
んぷん等の発泡核剤を組み合わせることによって、気泡
の微細化に効果が得られる。また、発泡剤としてHCF
C123やHCFC141bと共に、5.5%以下のパ
−フルオロカ−ボンを添加したエマルジョンを気泡核と
することにより、気泡を微細化して低熱伝導率のポリウ
レタンを得る提案もある(特開平5−186629号公
報)。Regarding the cell diameter, the cells are usually made finer by introducing a foaming nucleus (for example, Japanese Patent Application Laid-Open No. 3-54231). Perfluoroalkane such as perfluoropentane is used as the foaming core. By using a perfluoroalkane as an emulsifier to emulsify the polyol composition and further combining it with a foaming nucleating agent such as silica gel or starch, it is possible to obtain an effect of making bubbles finer. Also, as a foaming agent, HCF
There is also a proposal to obtain a polyurethane having a low thermal conductivity by making an emulsion in which 5.5% or less of perfluorocarbon is added together with C123 and HCFC141b as a cell nucleus to miniaturize the cells (JP-A-5-186629). Gazette).
【0006】ところが、オゾン層破壊あるいは地球の温
暖化等のフロンによる環境破壊の観点から、パ−フルオ
ロペンタン等のパ−フルオロアルカンも、特定フロン以
上に大気中での寿命が長く、その寿命は500年以上に
なると推定されており、その使用が制限されようとして
いる。また、フッ化アルケンを発泡剤として用いた断熱
性樹脂発泡体の製造方法として、パ−フルオロ−2−ペ
ンテンを炭化水素と併用する方法(特開平5−2472
49号公報)やパ−フルオロアルキルエチレンと水を併
用する方法(特開平5−279653号公報)が提案さ
れている。一方、樹脂発泡体を一体成型する方法とし
て、水を添加してフォームの物性を整える方法がある。
水を添加して発泡させる場合の特徴は、イソシアネート
と水との反応により反応熱を生成し、なおかつ二酸化炭
素を生成することによって、発泡性を高めることであ
る。なお、イソシアネートと水の反応によって形成され
る尿素結合の樹脂成分が、ウレタン結合よりも堅牢であ
り、かつ難燃性を付与することができる。この方法は、
従来のフロンの代替物として使用する際に非常に有効で
あった。しかし、二酸化炭素が樹脂発泡体中に含まれ、
ガス熱伝導率を高くするため、低熱伝導率の発泡剤を使
用してもその性能が充分利用されないという欠点があっ
た。水添加の方法を利用し、発泡体形成後、二酸化炭素
を吸収し断熱性を向上する技術が望まれる。その技術と
して、水酸化ナトリウムやソーダ石灰を二酸化炭素反応
性試薬として添加し、二酸化炭素を吸収させて断熱性を
向上する提案がされている(特開平6−322166号
公報)。However, from the viewpoint of environmental destruction due to CFCs such as ozone layer depletion or global warming, perfluoroalkanes such as perfluoropentane also have a longer life in the atmosphere than specified CFCs, and their lifespan is longer. It is estimated to be over 500 years old and its use is about to be restricted. Further, as a method for producing a heat insulating resin foam using a fluorinated alkene as a foaming agent, a method in which perfluoro-2-pentene is used in combination with hydrocarbon (Japanese Patent Laid-Open No. 5-2472).
49) or a method of using perfluoroalkylethylene in combination with water (JP-A-5-279653). On the other hand, as a method of integrally molding a resin foam, there is a method of adjusting the physical properties of the foam by adding water.
A characteristic of foaming by adding water is that the heat of reaction is generated by the reaction between isocyanate and water, and carbon dioxide is also generated to enhance the foamability. It should be noted that the urea-bonded resin component formed by the reaction of isocyanate and water is more robust than the urethane bond and can impart flame retardancy. This method
It was very effective when used as a substitute for conventional CFCs. However, carbon dioxide is contained in the resin foam,
Since the gas thermal conductivity is increased, even if a foaming agent having a low thermal conductivity is used, its performance is not fully utilized. There is a demand for a technique that utilizes a method of adding water and absorbs carbon dioxide after foam formation to improve heat insulation. As the technique, it has been proposed to add sodium hydroxide or soda lime as a carbon dioxide reactive reagent to absorb carbon dioxide and improve the heat insulating property (Japanese Patent Laid-Open No. 6-322166).
【0007】[0007]
【発明が解決しようとする課題】本発明は、熱伝導率が
低く、オゾン破壊係数(ODP)、地球温暖化計数(G
WP)などの環境破壊能がほとんどない新規な発泡剤を
利用して、断熱性に優れ、かつ燃焼性、爆発性などの安
全性に優れた断熱性樹脂発泡体を提供することを目的と
している。また、本発明は、新規な発泡剤を使用した断
熱性樹脂発泡体の製造方法を提供することを目的とす
る。The present invention has low thermal conductivity, ozone depletion potential (ODP), and global warming potential (G).
It is intended to provide a heat insulating resin foam having excellent heat insulating properties and safety such as flammability and explosive properties by using a new foaming agent having almost no environmental damage such as WP). . Moreover, this invention aims at providing the manufacturing method of the heat insulation resin foam which uses a novel foaming agent.
【0008】[0008]
【課題を解決するための手段】本発明は、発泡剤とし
て、フッ素化ヨウ化炭化水素、パーフルオロアルケンお
よび水素含有フッ化モルフォリン誘導体からなる群から
選択される少なくとも一種の化合物を用いることを特徴
とする。本発明の断熱性樹脂発泡体は、独立気泡を有す
る発泡樹脂組成物から構成され、その独立気泡内に、前
記発泡剤の気体を含むものである。According to the present invention, at least one compound selected from the group consisting of fluorinated iodohydrocarbons, perfluoroalkenes and hydrogen-containing fluorinated morpholine derivatives is used as a foaming agent. Characterize. The heat insulating resin foam of the present invention is composed of a foamed resin composition having closed cells, and the closed cells contain the gas of the foaming agent.
【0009】また、本発明の断熱性樹脂発泡体の製造方
法は、フッ素化ヨウ化炭化水素、パーフルオロアルケン
および水素含有フッ化モルフォリン誘導体からなる群よ
り選択される少なくとも一種の化合物からなる発泡剤、
ポリオール、ポリイソシアネート、ウレタン反応用触媒
および整泡剤を含む樹脂原料組成物を混合することによ
り発泡、成型して断熱性樹脂発泡体を得るものである。The method for producing a heat insulating resin foam of the present invention is a foam comprising at least one compound selected from the group consisting of fluorinated iodohydrocarbons, perfluoroalkenes and hydrogen-containing fluorinated morpholine derivatives. Agent,
The resin raw material composition containing a polyol, a polyisocyanate, a urethane reaction catalyst and a foam stabilizer is mixed to foam and mold to obtain a heat insulating resin foam.
【0010】ここにおいて、発泡剤は、フッ素化ヨウ化
炭化水素、および、パーフルオロアルケンと水素含有フ
ッ化モルフォリン誘導体のいずれか一方の混合物である
ことが好ましい。本発明の他の好ましい発泡剤は、前記
の発泡剤にさらに炭化水素、特に沸点50℃以下の炭化
水素を混合したものである。他の好ましい例において
は、前記の発泡剤に加えてさらに水を発泡剤として用い
る。In this case, the blowing agent is preferably a mixture of a fluorinated iodohydrocarbon and a perfluoroalkene and a hydrogen-containing fluorinated morpholine derivative. Another preferable foaming agent of the present invention is a mixture of the above-mentioned foaming agent with a hydrocarbon, particularly a hydrocarbon having a boiling point of 50 ° C. or lower. In another preferred embodiment, water is further used as a foaming agent in addition to the above-mentioned foaming agent.
【0011】本発明の断熱性樹脂発泡体を形成する樹脂
としては、ポリスチレン、フェノール系樹脂も使用可能
であるが、気泡径の制御、現場発泡の容易性などからポ
リウレタンが特に好ましい。従って、以下では、ウレタ
ン反応を用いた樹脂発泡体について説明する。本発明に
おいては、発泡剤は、特にフッ素化ヨウ化炭化水素、お
よび他の発泡剤との併用が好ましい。このフッ素化ヨウ
化炭化水素を用いる場合、樹脂組成物原料中に、沸点1
00℃以上の有機カーボネート化合物、エステルおよび
エポキシドのうち少なくとも一種を添加することが好ま
しい。Polystyrene and phenol resins can be used as the resin for forming the heat insulating resin foam of the present invention, but polyurethane is particularly preferable from the viewpoint of controlling the bubble diameter and facilitating on-site foaming. Therefore, hereinafter, the resin foam using the urethane reaction will be described. In the present invention, the blowing agent is particularly preferably used in combination with a fluorinated iodohydrocarbon, and another blowing agent. When this fluorinated iodohydrocarbon is used, it has a boiling point of 1 in the resin composition raw material.
It is preferable to add at least one of an organic carbonate compound, an ester, and an epoxide at 00 ° C. or higher.
【0012】また、樹脂原料組成物に、還元剤または酸
素吸収剤を添加するのも有効である。還元剤は、界面活
性剤とともにポリイソシアネ−ト組成物中に分散させて
ポリイソシアネートエマルジョンとし、これをポリオ−
ルとを混合して樹脂原料組成物を形成することが好まし
い。好ましい還元剤は、チオ硫酸ナトリウムの水溶液で
ある。また、フッ素化ヨウ化炭化水素を発泡剤に用いる
場合、ポリオールは、少なくとも30wt%の非アミン
系ポリオールを含有することが好ましい。It is also effective to add a reducing agent or an oxygen absorbent to the resin raw material composition. The reducing agent is dispersed in a polyisocyanate composition together with a surfactant to form a polyisocyanate emulsion, which is
It is preferable to form a resin raw material composition by mixing A preferred reducing agent is an aqueous solution of sodium thiosulfate. When a fluorinated iodohydrocarbon is used as a foaming agent, the polyol preferably contains at least 30 wt% of a non-amine-based polyol.
【0013】本発明の一態様において、樹脂原料組成物
は、フッ素化ヨウ化炭化水素を混合したポリイソシアネ
ート組成物と、ポリオール、ウレタン反応用触媒、およ
び整泡剤を含むプレミックスとを混合することにより調
製される。また、他の態様においては、樹脂原料組成物
は、発泡核として、炭素数3以下の第一級アルコールま
たは第二級アルコールに溶解する塩を含んでいる。本発
明の他の態様において、断熱性樹脂発泡体の製造方法
は、フッ素化ヨウ化炭化水素と、非共役結合を有するア
ミン、アンモニウム塩または四級アンモニウム塩との錯
化合物、ポリオール、およびポリイソシアネートを含む
樹脂組成物原料を混合することにより、発泡、成形する
工程を含み、ポリオールとポリイソシアネートとの反応
熱によって、前記錯化合物からフッ素化ヨウ化炭化水素
が分離し、そのフッ素化ヨウ化炭化水素が発泡剤として
働く。前記の態様においては、前記樹脂組成物原料が、
さらに有機スズ化合物、有機酸の金属塩、芳香族アミ
ン、および有機リン化合物からなる群より選択される少
なくとも一種をウレタン反応用触媒として含むことが好
ましい。また、前記の態様においては、前記樹脂組成物
原料が、さらに前記錯化合物と等モル量までの範囲で、
かつ前記ポリオール成分100重量部に対して10重量
部以下の水を含むことが好ましい。In one embodiment of the present invention, the resin raw material composition is obtained by mixing a polyisocyanate composition mixed with a fluorinated iodohydrocarbon and a premix containing a polyol, a urethane reaction catalyst, and a foam stabilizer. It is prepared by In another embodiment, the resin raw material composition contains, as a foaming nucleus, a salt soluble in a primary alcohol or a secondary alcohol having 3 or less carbon atoms. In another aspect of the present invention, a method for producing a heat insulating resin foam is a complex compound of a fluorinated iodohydrocarbon and a non-conjugated bond amine, ammonium salt or quaternary ammonium salt, a polyol, and a polyisocyanate. A step of foaming and molding by mixing a resin composition raw material containing the fluorinated iodocarbon is separated from the complex compound by the heat of reaction between the polyol and the polyisocyanate. Hydrogen acts as a blowing agent. In the above aspect, the resin composition raw material,
Furthermore, it is preferable that at least one selected from the group consisting of an organic tin compound, a metal salt of an organic acid, an aromatic amine, and an organic phosphorus compound is contained as a urethane reaction catalyst. Further, in the above aspect, the resin composition raw material is further in a range up to an equimolar amount with the complex compound,
Further, it is preferable to contain 10 parts by weight or less of water with respect to 100 parts by weight of the polyol component.
【0014】水を発泡剤として含む断熱性樹脂発泡体の
製造方法の好ましい態様においては、樹脂原料組成物
が、エポキシドと二酸化炭素固定化触媒を含み、発泡工
程中に生成する二酸化炭素が前記エポキシドと反応して
カーボネート化合物を形成することにより、生成する発
泡体の気泡内が減圧化される工程を有する。前記の態様
においては、樹脂原料組成物が、フッ素化ヨウ化炭化水
素および二酸化炭素固定化触媒を混合したポリイソシア
ネート組成物と、ポリオール、ウレタン反応用触媒、エ
ポキシド、および整泡剤を含むプレミックスとの混合に
より形成されることが好ましい。また、前記の態様にお
いては、樹脂原料組成物が、二酸化炭素固定化触媒とフ
ッ素化ヨウ化炭化水素との錯化合物を含み、ポリオール
とポリイソシアネートとの反応熱によって、錯化合物が
分解してフッ素化ヨウ化炭化水素と二酸化炭素固定化触
媒を生成する工程を含み、生成した二酸化炭素固定化触
媒が、エポキシドと発泡工程中に生成した二酸化炭素と
の反応に作用することが好ましい。In a preferred embodiment of the method for producing a heat insulating resin foam containing water as a foaming agent, the resin raw material composition contains an epoxide and a carbon dioxide fixing catalyst, and carbon dioxide produced during the foaming step is the epoxide. And a carbonate compound to form a carbonate compound, thereby reducing the pressure inside the bubbles of the resulting foam. In the above aspect, the resin raw material composition is a premix containing a polyisocyanate composition in which a fluorinated iodohydrocarbon and a carbon dioxide-immobilized catalyst are mixed, a polyol, a urethane reaction catalyst, an epoxide, and a foam stabilizer. It is preferably formed by mixing with. Further, in the above aspect, the resin raw material composition contains a complex compound of a carbon dioxide-immobilized catalyst and a fluorinated iodohydrocarbon, and the complex compound is decomposed by the heat of reaction between the polyol and the polyisocyanate to produce fluorine. It is preferable that the method includes a step of producing a fluorinated iodohydrocarbon and a carbon dioxide-immobilized catalyst, and the produced carbon dioxide-immobilized catalyst acts on the reaction between the epoxide and the carbon dioxide produced during the foaming step.
【0015】フッ素化ヨウ化炭化水素とともに発泡剤と
して用いられる炭化水素は、ペンタン、イソペンタンお
よびシクロペンタンからなる群より選択される少なくと
も一種が好ましい。この炭化水素の好ましい混合割合
は、45〜96モル%である。整泡剤としては、ジメチ
ルシロキサンーオキシアルキレン共重合体と、分子中に
フルオロアルキル基を有するジメチルシロキサンーオキ
シアルキレン共重合体をともに用いることが好ましい。
以上に述べた樹脂原料に添加される材料のうち、還元剤
および二酸化炭素固定化触媒は、イソシアネート組成物
に混合するのが好ましい。他の材料はポリオール組成物
に混合されるのが好ましい。The hydrocarbon used as the blowing agent together with the fluorinated iodohydrocarbon is preferably at least one selected from the group consisting of pentane, isopentane and cyclopentane. The preferable mixing ratio of this hydrocarbon is 45 to 96 mol%. As the foam stabilizer, it is preferable to use both a dimethylsiloxane-oxyalkylene copolymer and a dimethylsiloxane-oxyalkylene copolymer having a fluoroalkyl group in the molecule.
Of the materials added to the resin raw material described above, the reducing agent and the carbon dioxide-immobilized catalyst are preferably mixed with the isocyanate composition. Other materials are preferably mixed into the polyol composition.
【0016】本発明で用いる新規な発泡剤は、ともに大
気中での寿命が比較的短いため、地球温暖化係数もほと
んどないか、わずかである。フッ素化ヨウ化炭化水素
は、紫外線を照射されると、ヨウ素が分子からはずれや
すいため、大気中の寿命が従来のフロンと比較して遥か
に短い。また、パーフルオロアルケンは、大気中におい
て二重結合部へのOHラジカルの反応が容易に進むた
め、寿命が短くなると予測される。水素含有フッ化モル
フォリン誘導体は、分子中の水素が酸素、窒素の近傍に
あることにより、全フッ化のモルフォリン誘導体である
パーフルオロモルフォリン、パーフルオロメチルモルフ
ォリンよりも炭素−水素の結合エネルギーが弱く分解し
やすいことにより、大気中の寿命が短いと予測される。Since both of the novel blowing agents used in the present invention have a relatively short life in the atmosphere, they have little or no global warming potential. Fluorinated iodohydrocarbons have a much shorter life in the atmosphere than conventional CFCs because iodine is likely to dissociate from the molecule when irradiated with ultraviolet rays. Further, perfluoroalkene is expected to have a short life because the reaction of OH radicals to the double bond portion easily proceeds in the atmosphere. The hydrogen-containing fluorinated morpholine derivative has a carbon-hydrogen bond more than perfluoromorpholine and perfluoromethylmorpholine, which are fluorinated morpholine derivatives, because hydrogen in the molecule is near oxygen and nitrogen. Due to its weak energy and easy decomposition, its lifetime in the atmosphere is expected to be short.
【0017】また、これらの物質は、ともに気体熱伝導
率が低く、これらを用いた樹脂発泡体は、環境負荷がな
く、断熱性の面からも、優れた断熱材となる。さらに、
これらの発泡剤は、不燃性であり、安全性の面からも有
利な材料である。特に、フッ素化ヨウ化炭化水素は、こ
れらの中で最も熱伝導率が低く、大気中の寿命が短い。
さらに、ヨウ素がついているため、燃焼に対して負の触
媒効果を有し、発泡樹脂組成物に難燃化、自己消火性を
付与することができる。また、発泡剤として可燃性のエ
ーテルや、炭化水素などを併用した場合には、混合発泡
剤自体を不燃化することが可能である。フッ素化ヨウ化
炭化水素は、不燃性であるばかりでなく、発火時にヨウ
素が遊離して消火剤として働くため、単独で用いる場合
はもとより、パーフルオロアルケンまたは水素含有フッ
化モルフォリン誘導体に混合した場合にも、不燃性かつ
自己消火性の発泡剤として働く。Further, both of these substances have low gas thermal conductivity, and the resin foam using them has no environmental load and is an excellent heat insulating material from the viewpoint of heat insulating property. further,
These foaming agents are nonflammable and are advantageous materials in terms of safety. In particular, fluorinated iodohydrocarbons have the lowest thermal conductivity among them and have a short life in the atmosphere.
Furthermore, since it has iodine, it has a negative catalytic effect on combustion and can impart flame retardancy and self-extinguishing properties to the foamed resin composition. When a flammable ether or hydrocarbon is used together as the foaming agent, the mixed foaming agent itself can be made incombustible. Fluorinated iodohydrocarbons are not only non-combustible, but also release iodine upon ignition to act as a fire extinguisher. It also acts as a non-flammable and self-extinguishing foaming agent.
【0018】現在、環境負荷のない発泡剤として注目さ
れているものの一つに炭化水素系発泡剤がある。炭化水
素としては、ペンタン、イソペンタン、シクロペンタン
などが断熱性の高い発泡剤として有用である。しかし、
炭化水素は、一般に可燃性であるため危険性が大きい。
本発明のフッ素化ヨウ化炭化水素、パーフルオロアルケ
ン、水素含有フッ化モルフォリン誘導体のうちの一種を
前記炭化水素発泡剤に混合すると、得られる樹脂発泡体
は難燃性となる。従って、この樹脂発泡体は、冷蔵庫だ
けでなく建築材用の断熱材としても有効である。フッ素
化ヨウ化炭化水素、パーフルオロアルケンおよび水素含
有フッ化モルフォリン誘導体から選ばれるものの炭化水
素発泡剤に対する混合割合は、4モル%以上55モル%
以下の範囲で、混合発泡剤のガス引火性または爆発性が
なくなる。また、特にフッ素化ヨウ化炭化水素は、難燃
性に加えて、自己消火性を有するため、上記の範囲で炭
化水素発泡剤に添加すると、難燃化だけでなく自己消火
性も付与できる。なかでも、トリフルオロアイオドメタ
ンのような沸点が0℃以下であるような化合物は、環境
負荷のない冷媒としても使用することができ、自己消火
性を有するため火災の心配が全くなくなる。すなわち、
炭化水素を冷媒として用いる際、これに混入しても冷媒
効果を損なわず不燃化することができる。このフッ素化
ヨウ化炭化水素の効果を最も生かす構成が本発明の主な
目的である。At present, a hydrocarbon-based foaming agent is one of the ones attracting attention as a foaming agent having no environmental load. As the hydrocarbon, pentane, isopentane, cyclopentane and the like are useful as a foaming agent having a high heat insulating property. But,
Hydrocarbons are generally flammable and therefore dangerous.
When one of the fluorinated iodohydrocarbons, perfluoroalkenes, and hydrogen-containing fluorinated morpholine derivatives of the present invention is mixed with the hydrocarbon blowing agent, the resulting resin foam becomes flame-retardant. Therefore, this resin foam is effective not only as a refrigerator but also as a heat insulating material for building materials. The mixing ratio of the fluorinated iodohydrocarbon, the perfluoroalkene and the hydrogen-containing fluorinated morpholine derivative to the hydrocarbon blowing agent is 4 mol% or more and 55 mol% or more.
Within the following ranges, the mixed foaming agent loses gas flammability or explosiveness. Further, in particular, fluorinated iodohydrocarbon has not only flame retardancy but also self-extinguishing property. Therefore, when it is added to the hydrocarbon foaming agent within the above range, not only flame retardancy but also self-extinguishing property can be imparted. Among them, compounds such as trifluoroiodomethane having a boiling point of 0 ° C. or lower can be used as a refrigerant having no environmental load and have self-extinguishing property, so that there is no fear of fire. That is,
When hydrocarbons are used as a refrigerant, even if they are mixed in the refrigerant, the effect of the refrigerant is not impaired and it can be made incombustible. The constitution which maximizes the effect of the fluorinated iodohydrocarbon is the main object of the present invention.
【0019】フッ素化ヨウ化炭化水素は、樹脂原料であ
るポリオ−ルに非常に溶け易いが、これを単独に発泡剤
として用いると、この発泡剤を含んだポリオ−ルプレミ
ックスとポリイソシアネ−トとの反応は、従来のフロン
発泡剤を用いる場合と比較して非常に遅くなる。そのた
め、得られるポリウレタンフォ−ムの気泡径が大きくな
る傾向がある。これに対してパーフルオロアルケンおよ
び水素含有フッ化モルフォリン誘導体は、ポリオ−ルに
溶解しにくくエマルジョンを形成する。ポリオールに分
散したパーフルオロアルケンなどの微粒子は、発泡時の
気泡核として働くため、得られるポリウレタンフォ−ム
の気泡径は小さくなる。しかし、エマルジョンの形成に
より、ポリオ−ルプレミックスの粘度が高くなり、原料
の混合性が低下する。そのため、得られる樹脂発泡体の
密度が高くなったり、破泡が起こりやすくなったりする
傾向がある。Fluorinated iodohydrocarbons are very soluble in the resin raw material, but when used alone as a foaming agent, the polyol premix and polyisocyanate containing this foaming agent are used. The reaction with is much slower than when using a conventional freon blowing agent. Therefore, the bubble diameter of the obtained polyurethane foam tends to increase. On the other hand, perfluoroalkene and hydrogen-containing morpholine fluoride derivative are difficult to dissolve in polyol and form an emulsion. Since the fine particles such as perfluoroalkene dispersed in the polyol act as a bubble nucleus during foaming, the obtained polyurethane foam has a small bubble diameter. However, the formation of the emulsion increases the viscosity of the polyol premix and reduces the mixability of the raw materials. Therefore, the density of the obtained resin foam tends to be high, or the foaming tends to occur easily.
【0020】驚くべきことに、発明者らは、ヨウ素化フ
ッ化炭化水素を、発泡剤としてパーフルオロアルケンま
たは水素含有フッ化モルフォリン誘導体と併用すること
で、ハイブリッド効果が表れ、各々の化合物を別々に発
泡剤として用いる場合よりも優れた断熱性のポリウレタ
ンフォ−ムが得られることを見いだした。これは、次の
ように考えられる。すなわち、これら2つの発泡剤を併
用すると、ポリオ−ル組成物は、パーフルオロアルケン
または水素含有フッ化モルフォリン誘導体の混合により
エマルジョンを形成するが、ポリオ−ルとの相溶性に優
れたフッ素化ヨウ化炭化水素が加わることにより、エマ
ルジョンの粘度が低下して、短時間で均一に混合し、発
泡性が向上する。これによって、気泡径が比較的小さ
く、樹脂密度が低く、かつ破泡のないポリウレタンフォ
−ムが得られるのである。Surprisingly, the present inventors have shown that by using an iodinated fluorohydrocarbon in combination with a perfluoroalkene or a hydrogen-containing fluorinated morpholine derivative as a blowing agent, a hybrid effect is exhibited, and each compound is used. It has been found that a polyurethane foam with better thermal insulation is obtained than when used separately as blowing agents. This is considered as follows. That is, when these two foaming agents are used in combination, the polyol composition forms an emulsion by mixing the perfluoroalkene or the hydrogen-containing fluorinated morpholine derivative, but is fluorinated with excellent compatibility with the polyol. By adding iodohydrocarbon, the viscosity of the emulsion is lowered, and the emulsion is uniformly mixed in a short time to improve the foamability. As a result, a polyurethane foam having a relatively small bubble diameter, a low resin density, and no bubble breakage can be obtained.
【0021】また、上記の発泡剤とともに水を添加し
て、水とイソシアネートとの反応により生成する二酸化
炭素を発泡剤として使用することも非常に有効な手段で
ある。前記の本発明の発泡剤と水の併用では、例えばフ
ッ素化ヨウ化炭化水素と水の組み合わせにより、混合発
泡中に高い反応熱が生成し、ポリオールに相溶性のよい
フッ素化ヨウ化炭化水素の気化、発泡に必要な熱量が供
給されるために、発泡性を向上することができる。ま
た、水を用いた発泡では、気泡を微細化する効果を有
し、フッ素化ヨウ化炭化水素の気泡形状が大きくなりや
すい特徴を改善するのに有効である。さらに、次によう
な効果をもたらす。すなわち、ポリオールなどの樹脂原
料に相溶性の良い発泡剤のガスは、樹脂発泡体から経時
的に透過しやすい。しかし、水発泡樹脂組成物は、架橋
密度が高くなるため、発泡剤ガスが透過しにくくなり、
経時的にも安定な断熱性能を示す。また、水発泡は、パ
ーフルオロアルケン、水素含有フッ化モルフォリン誘導
体に対しても、発泡性を向上するので、有効である。It is also a very effective means to add water together with the above-mentioned foaming agent and use carbon dioxide produced by the reaction of water and isocyanate as the foaming agent. When the blowing agent of the present invention is used in combination with water, for example, a combination of fluorinated iodohydrocarbon and water produces a high heat of reaction during mixed foaming, so that the fluorinated iodohydrocarbon having good compatibility with the polyol can be obtained. Since the amount of heat required for vaporization and foaming is supplied, the foamability can be improved. In addition, foaming with water has an effect of making bubbles finer, and is effective in improving the feature that the bubble shape of the fluorinated iodohydrocarbon tends to be large. Furthermore, the following effects are brought about. That is, the gas of the foaming agent having a good compatibility with the resin raw material such as polyol is easily permeated from the resin foam over time. However, since the water-foamed resin composition has a high cross-linking density, it becomes difficult for the foaming agent gas to permeate,
Stable heat insulation performance over time. Water foaming is also effective for perfluoroalkene and hydrogen-containing fluorinated morpholine derivatives because it improves the foamability.
【0022】また、樹脂原料に、沸点100℃以上の有
機カーボネート化合物、エステルまたはエポキシドを添
加すると、発泡性を向上するため有効である。フッ素化
ヨウ化炭化水素は、一般にフッ素化合物でありながらポ
リオール等の樹脂原料に相溶しやすい特性を有する。相
溶性が高いため、発泡過程において気泡が大きくなる傾
向があり、得られる発泡体の断熱性能を悪化する。そこ
で、カーボネート、エステル、エポキシドなどの極性非
活性水素含有化合物を混合し、その希釈効果によって、
発泡性および気泡径を整えることができる。また、上記
化合物は、ポリオールと相溶性が悪い場合、プレミック
スエマルジョンの粘度を低下することにより、発泡性お
よび気泡径を整えることができる。そのため、パーフル
オロアルケンおよび水素含有フッ化モルフォリン誘導体
を発泡剤として使用した際にも効果があるため好まし
い。Further, it is effective to add an organic carbonate compound, an ester or an epoxide having a boiling point of 100 ° C. or higher to the resin raw material because the foamability is improved. Fluorinated iodohydrocarbons are generally fluorine compounds but have the property of being easily compatible with resin raw materials such as polyols. Since the compatibility is high, bubbles tend to become large in the foaming process, which deteriorates the heat insulating performance of the obtained foam. Therefore, by mixing polar inactive hydrogen-containing compounds such as carbonate, ester, and epoxide, and by the dilution effect,
Foamability and cell size can be adjusted. Further, when the above compound has poor compatibility with the polyol, the viscosity of the premix emulsion is lowered, whereby the foamability and the cell diameter can be adjusted. Therefore, it is preferable that the perfluoroalkene and the hydrogen-containing fluorinated morpholine derivative are effective even when used as a foaming agent.
【0023】本発明の新規な発泡剤は、寿命が短いた
め、環境に対する負荷がないか非常に小さいという利点
を有するが、寿命が短い故に断熱性樹脂発泡体の気泡中
で分解したり樹脂の性能劣化を起こすことが懸念され
る。そこで、このような不都合を防ぐ手段を講じるのが
好ましい。その1つは、樹脂に還元剤を添加することで
ある。還元剤は、ヨウ素化フッ化炭化水素の分解などに
より生じるヨウ素などの酸化性物質を還元し、発泡体の
断熱性能を長期安定に保持する。また、酸素吸収剤の添
加は、断熱性樹脂発泡体の気泡中におけるヨウ素化フッ
化炭化水素の安定化に有効である。これは酸素吸収剤が
気泡中の酸素溶存量を減らし、ヨウ素化フッ化炭化水素
の酸化を抑制することによる。また、酸素吸収剤は、こ
れと同じく電子受容体としての性質を有するポリイソシ
アネートと混合すると、安定な分散液とすることが可能
である。The novel foaming agent of the present invention has an advantage that it has no or very small load on the environment because it has a short life. There is concern that performance may deteriorate. Therefore, it is preferable to take measures to prevent such inconvenience. One is to add a reducing agent to the resin. The reducing agent reduces oxidative substances such as iodine generated by decomposition of iodinated fluorohydrocarbons and the like, and keeps the heat insulating performance of the foam stable for a long period of time. Further, the addition of the oxygen absorbent is effective for stabilizing the iodinated fluorohydrocarbon in the bubbles of the heat insulating resin foam. This is because the oxygen absorbent reduces the amount of oxygen dissolved in the bubbles and suppresses the oxidation of iodinated fluorohydrocarbon. When the oxygen absorbent is mixed with polyisocyanate, which has the same property as an electron acceptor, a stable dispersion liquid can be obtained.
【0024】フッ素化ヨウ化炭化水素を発泡剤として使
用する場合は、非アミン系ポリオールを含むんでいるポ
リオール組成物を使用することが好ましい。アミンとフ
ッ素化ヨウ化炭化水素は、錯化合物を形成して、容易に
発泡しなくなり、発泡性が悪くなる。それを避けるため
には、樹脂原料中のアミン成分を低減することが必要で
ある。少なくとも30wt%の非アミン系ポリオールを
含むポリオールは、フッ素化ヨウ化炭化水素と容易には
錯化合物を形成せず、錯化合物形成による不都合がなく
なる。When a fluorinated iodohydrocarbon is used as a blowing agent, it is preferable to use a polyol composition containing a non-amine polyol. The amine and the fluorinated iodohydrocarbon form a complex compound, which does not easily foam and the foaming property deteriorates. In order to avoid this, it is necessary to reduce the amine component in the resin raw material. A polyol containing at least 30 wt% of a non-amine-based polyol does not easily form a complex compound with a fluorinated iodohydrocarbon, and the disadvantage due to the formation of the complex compound is eliminated.
【0025】本発明の1つの好ましい態様においては、
フッ素化ヨウ化炭化水素と、非共役結合を有するアミン
あるいはアンモニウム塩、または四級アンモニウム塩と
の錯化合物を含む樹脂原料を混合し、発泡させることに
よって断熱性樹脂発泡体を製造する。フッ素化ヨウ化炭
化水素は、前記アミンまたはアンモニウム塩と容易に錯
化合物を形成し安定化する。本発明者らは、この錯化合
物が、断熱性樹脂発泡体の製造および性能向上に関して
非常に有効であることを見いだした。ここに用いる錯化
合物として好ましいものは、次のようなものである。す
なわち、化合物によって結合力が大きく異なるが、室温
で固体または液体状態であり、用いるフッ素化ヨウ化炭
化水素の沸点では容易に気化せず、放置しても分離しな
い。しかし、結合力によるが、加熱すると分離しフッ素
化ヨウ化炭化水素が遊離する。また、錯化合物に水を添
加すると、上層と下層に分離し、上層は水層でありアミ
ンが溶解した液体、下層は、フッ素化ヨウ化炭化水素か
らなる液層となる。フッ素化ヨウ化炭化水素は、光に当
たると直ちにヨウ素が分離し赤く着色するが、アミン類
との錯化合物は、光に対して非常に安定であり、全く光
によって分解しないものとなる。このような錯化合物
は、発泡剤として、またウレタン反応触媒として作用す
る。実施例に各種の錯化合物の作用を示す。In one preferred embodiment of the invention,
A heat insulating resin foam is manufactured by mixing and foaming a resin raw material containing a complex compound of a fluorinated iodohydrocarbon and an amine or ammonium salt having a non-conjugated bond, or a quaternary ammonium salt. The fluorinated iodohydrocarbon easily forms and stabilizes a complex compound with the amine or ammonium salt. The present inventors have found that this complex compound is very effective in producing a heat insulating resin foam and improving performance. Preferred complex compounds used here are as follows. That is, although the binding force greatly differs depending on the compound, it is in a solid or liquid state at room temperature, does not easily vaporize at the boiling point of the fluorinated iodohydrocarbon used, and does not separate even when left standing. However, depending on the bonding force, the fluorinated iodohydrocarbon is separated upon heating and liberated. When water is added to the complex compound, it is separated into an upper layer and a lower layer, the upper layer is a water layer and a liquid in which amine is dissolved, and the lower layer is a liquid layer made of fluorinated iodohydrocarbon. When fluorinated iodohydrocarbons are exposed to light, iodine is immediately separated and colored red. However, complex compounds with amines are extremely stable to light and do not decompose at all. Such a complex compound acts as a foaming agent and as a urethane reaction catalyst. The examples show the effects of various complex compounds.
【0026】本発明では、この錯化合物を、固体状態あ
るいは、室温中一週間以上重量変化のない高沸点液体状
態で含む組成物として添加するのが好ましい。これによ
り、フッ素化ヨウ化炭化水素が光分解するのを防ぎ、発
泡の際、フッ素化ヨウ化炭化水素の損失を低減すること
ができる。錯化合物の結合力によっては、固体または高
沸点液体状態となるため、揮発性を抑え、発泡前原料の
貯蔵安定性を高めることができ、作業上の発泡剤の損失
およびプレミックスの劣化を抑えることができる。In the present invention, it is preferable to add the complex compound as a composition containing the complex compound in a solid state or in a high boiling point liquid state in which the weight does not change at room temperature for one week or more. This can prevent photodecomposition of the fluorinated iodohydrocarbon and reduce the loss of the fluorinated iodohydrocarbon during foaming. Depending on the binding force of the complex compound, it becomes a solid or high boiling point liquid state, so volatility can be suppressed, storage stability of the pre-foaming raw material can be improved, and loss of the foaming agent and deterioration of the premix during operation can be suppressed. be able to.
【0027】本発明の一態様による樹脂発泡体は、フッ
素化ヨウ化炭素、パーフルオロアルケンおよび水素含有
フッ化モルフォリン誘導体からなる群より選ばれる発泡
剤と二酸化炭素とを独立気泡内に含んでいる。さらに、
好ましい態様においては、樹脂原料段階で混合されたエ
ポキシドが二酸化炭素固定化触媒存在下で二酸化炭素を
固定化したカーボネート成分を含んでいる。二酸化炭素
固定化触媒としては、求核剤および/または求電子剤を
含んだ触媒が好ましい。この構成においては、発泡過程
で生成する二酸化炭素が吸収されて固定化されるため、
熱伝導率の高い二酸化炭素は、樹脂発泡体のガス熱伝導
率には寄与しない。従って、上記発泡剤の熱伝導率特性
を良好に示すことが可能である。本発明によれば、発泡
剤のガス熱伝導率が低いことによって、高断熱性の樹脂
発泡体を得ることができる。The resin foam according to one embodiment of the present invention contains carbon dioxide and a foaming agent selected from the group consisting of fluorinated carbon iodide, perfluoroalkene and hydrogen-containing fluorinated morpholine derivative in closed cells. There is. further,
In a preferred embodiment, the epoxide mixed in the resin raw material stage contains a carbonate component in which carbon dioxide is immobilized in the presence of a carbon dioxide immobilization catalyst. The carbon dioxide-immobilized catalyst is preferably a catalyst containing a nucleophile and / or an electrophile. In this configuration, carbon dioxide generated in the foaming process is absorbed and immobilized,
Carbon dioxide, which has a high thermal conductivity, does not contribute to the gas thermal conductivity of the resin foam. Therefore, it is possible to exhibit excellent thermal conductivity characteristics of the foaming agent. According to the present invention, a resin foam having a high heat insulating property can be obtained due to the low gas thermal conductivity of the foaming agent.
【0028】二酸化炭素は、原料プレミックス中に水を
添加した場合には化1に基づく反応や、化2に示すイソ
シアネート同士の結合によって放出され、発泡剤として
作用する。When water is added to the raw material premix, carbon dioxide is released by the reaction based on Chemical formula 1 or the bond between the isocyanates shown in Chemical formula 2 and acts as a foaming agent.
【0029】[0029]
【化1】 Embedded image
【0030】[0030]
【化2】 Embedded image
【0031】これらの反応は、発泡性の改善、気泡微細
化、フォーム強度増加の目的にはなくてはならない反応
であったが、二酸化炭素の放出によって気泡内ガスの熱
伝導率が高くなることが問題となっていた。化3に示す
ように二酸化炭素とエポキシドとの反応によって、カー
ボネート化合物が生成する。このカーボネート化合物
は、発泡性改善効果、可塑剤としての効果も有し、発泡
体の断熱性能向上には良い物質である。また、発泡過程
において、エポキシドが重合し、発泡体の樹脂成分とし
て強度増加を示すため好ましい。These reactions were indispensable for the purpose of improving the foamability, making the cells finer, and increasing the foam strength, but the thermal conductivity of the gas in the bubbles increased due to the release of carbon dioxide. Was a problem. As shown in Chemical formula 3, a carbonate compound is produced by the reaction between carbon dioxide and an epoxide. This carbonate compound has an effect of improving foamability and an effect as a plasticizer, and is a good substance for improving the heat insulating performance of the foam. Further, in the foaming process, the epoxide is polymerized to increase the strength as a resin component of the foam, which is preferable.
【0032】[0032]
【化3】 Embedded image
【0033】また、二酸化炭素とエポキシドの反応に
は、二酸化炭素固定化触媒として求核剤および/または
求電子剤を含む触媒を用いると、式3の反応収率を増加
するため好ましい。しかし、前記エポキシドは、二酸化
炭素を固定する前に、樹脂原料であるイソシアネートや
ポリオールと開環付加重合して、組成によってはエポキ
シドがなくなってしまう可能性があった。また、この二
酸化炭素固定化触媒は、イソシアネートを重合する作用
をも有するため、ポリイソシアネート組成物に混合でき
なかった。しかし、フッ素化ヨウ化炭化水素と前記二酸
化炭素固定化触媒とは相互作用で安定化するため、イソ
シアネート組成物中に添加して、エポキシドと隔離する
ことができる。これにより、重合に使われるエポキシド
を低減し、かつ樹脂反応も阻害されることなく、性能の
良い断熱性樹脂発泡体を形成することができる。Further, in the reaction of carbon dioxide and epoxide, it is preferable to use a catalyst containing a nucleophile and / or an electrophile as a carbon dioxide fixing catalyst because the reaction yield of the formula 3 is increased. However, before fixing carbon dioxide, the epoxide may undergo ring-opening addition polymerization with the resin raw material isocyanate or polyol, and depending on the composition, the epoxide may be lost. Further, since this carbon dioxide-immobilized catalyst also has a function of polymerizing isocyanate, it cannot be mixed with the polyisocyanate composition. However, since the fluorinated iodohydrocarbon and the carbon dioxide-immobilized catalyst are stabilized by the interaction, they can be added to the isocyanate composition and separated from the epoxide. This makes it possible to reduce the amount of epoxide used for polymerization and to form a heat-insulating resin foam having good performance without inhibiting the resin reaction.
【0034】また、非共役系のアミンあるいはアンモニ
ウム塩、または四級アンモニウム塩と、フッ素化ヨウ化
炭化水素との錯化合物を、エポキシドおよび二酸化炭素
固定化触媒とともに樹脂原料に混合する構成も、前記の
問題を解決する方法である。これにより、二酸化炭素固
定化促進および固定化率の向上とガス熱伝導率の低下を
もたらし、断熱性の高い樹脂発泡体を形成することがで
きる。すなわち、前記錯化合物は、熱で分解して生成す
るフッ素化ヨウ化炭化水素が発泡剤として作用するだけ
でなく、錯化合物としては二酸化炭素固定化のための触
媒作用を持たないが、熱などによる分解過程を経て初め
て二酸化炭素固定化触媒作用をする。このことによっ
て、ウレタン反応は二酸化炭素固定化反応とは全く別の
次元で進行する。そして、ほとんど樹脂発泡体が形成さ
れた後に二酸化炭素の固定化反応が起こるため、樹脂発
泡体として強度のあるものができ、減圧状態になっても
形状変化を起こさない。また、ハロゲンイオンを有しな
い三級アミンと、フッ素化ヨウ化炭化水素との錯化合物
を用いると、この錯化合物は二酸化炭素固定化触媒とな
りうる。Further, the composition in which a complex compound of a non-conjugated amine or ammonium salt or quaternary ammonium salt and a fluorinated iodohydrocarbon is mixed with a resin raw material together with an epoxide and a carbon dioxide fixing catalyst is also described above. Is a way to solve the problem. This promotes carbon dioxide immobilization, improves the immobilization rate, and lowers the gas thermal conductivity, so that a resin foam having a high heat insulating property can be formed. That is, the complex compound not only acts as a blowing agent by fluorinated iodohydrocarbons generated by decomposition with heat, but also does not have a catalytic action for carbon dioxide immobilization as a complex compound. It does not act as a carbon dioxide immobilization catalyst until it undergoes a decomposition process. As a result, the urethane reaction proceeds in a completely different dimension from the carbon dioxide fixing reaction. Then, since the carbon dioxide immobilization reaction occurs almost after the resin foam is formed, a strong resin foam can be formed, and the shape does not change even when the pressure is reduced. When a complex compound of a tertiary amine having no halogen ion and a fluorinated iodohydrocarbon is used, this complex compound can serve as a carbon dioxide-immobilized catalyst.
【0035】[0035]
【発明の実施の形態】以下、本発明の断熱性樹脂発泡体
およびその製造方法について、さらに詳細に説明する。
本発明に用いる新規な発泡剤は、フッ素化ヨウ化炭化水
素、パーフルオロアルケンおよび水素含有フッ化モルフ
ォリン誘導体からなる群より選ばれる。この発泡剤は、
従来使用されてきた樹脂原料および製法において、発泡
剤として充分性能を発揮する。発泡剤のフッ素化ヨウ化
炭化水素は、炭素数4以下であり、かつ沸点が65℃以
下の化合物であること好ましい。そのようなフッ素化ヨ
ウ化炭化水素としては、アイオドトリフルオロメタン
(化学式CF3I:沸点ー22.5℃)(かっこ内には
化学式と沸点を記す。以下同じ)、アイオドペンタフル
オロエタン(CF3CF2I:12〜13℃)、1ーアイ
オドヘプタフルオロプロパン(CF3CF2CF2I:3
9℃)、2ーアイオドヘプタフルオロプロパン(CF3
CFICF3:39℃)、アイオド−1,1,2,2−
テトラフルオロエタン(C2HF4I:41℃)、2−ア
イオド−1,1,1−トリフルオロエタン(C2H2F3
I:55℃)、アイオドトリフルオロエチレン(C2F3
I:30℃)、1−アイオド−1,1,2,3,3,3
−ヘキサフルオロプロパン(CF3CHFCF2I)、2
−アイオドノナフルオロ−t−ブタン((CF3)3C
I:61℃)などがある。BEST MODE FOR CARRYING OUT THE INVENTION The heat insulating resin foam and the method for producing the same according to the present invention will be described in more detail below.
The novel blowing agent used in the present invention is selected from the group consisting of fluorinated iodohydrocarbons, perfluoroalkenes and hydrogen-containing fluorinated morpholine derivatives. This foaming agent
In the resin raw material and the manufacturing method that have been used conventionally, it exerts sufficient performance as a blowing agent. The fluorinated iodohydrocarbon as the foaming agent is preferably a compound having 4 or less carbon atoms and a boiling point of 65 ° C or less. Examples of such fluorinated iodohydrocarbons include iodotrifluoromethane (chemical formula CF 3 I: boiling point-22.5 ° C.) (the chemical formula and boiling point are shown in parentheses; the same applies hereinafter), iodopentafluoroethane ( CF 3 CF 2 I: 12 to 13 ° C.) 1-iodoheptafluoropropane (CF 3 CF 2 CF 2 I: 3)
9 ° C) 2-iodoheptafluoropropane (CF 3
CFICF 3 : 39 ° C), iodo-1, 1, 2, 2-
Tetrafluoroethane (C 2 HF 4 I: 41 ° C.), 2-iodo-1,1,1-trifluoroethane (C 2 H 2 F 3
I: 55 ° C.), iodotrifluoroethylene (C 2 F 3
I: 30 ° C.), 1-iodo-1,1,2,3,3,3
- hexafluoropropane (CF 3 CHFCF 2 I), 2
- Eye odo nonafluorobutyl -t- butane ((CF 3) 3 C
I: 61 ° C.).
【0036】発泡剤として有用なパーフルオロアルケン
としては、ヘキサフルオロプロペンの二量体であり、例
えば、パーフルオロ−4−メチル−2−ペンテン、パー
フルオロ−2−メチル−2−ペンテンおよびこれらの混
合組成物があり、この混合組成物は、沸点48〜51
℃、分子量300.04であり、分子中に炭素−炭素不
飽和結合を1個含む全フッ化炭素からなる。また、ヘキ
サフルオロプロペンダイマーの他に、パーフルオロー2
ーペンテン、(パーフルオロブチル)エチレン、(パー
フルオロプロピル)エチレン、および、オクタフルオロ
シクロペンタンより選ばれる化合物は、発泡剤として適
度な沸点を有するため好ましい。発泡剤として有用な水
素含有フッ化モルフォリン誘導体は、例えば、モノヒド
ロパーフルオロモルフォリンまたはモノヒドロパーフル
オロメチルモルフォリンのいずれか、あるいは、これら
の混合物がある。モノヒドロパーフルオロモルフォリン
としては、3H−オクタフルオロモルフォリン(分子量
231)、2H−オクタフルオロモルフォリン(分子量
231)があり、その沸点は、パーフルオロモルフォリ
ンの沸点が34.5℃であることから、30〜40℃で
あると推定される。モノヒドロパーフルオロメチルモル
フォリンとしては、オクタフルオロ−4−ジフルオロメ
チル−モルフォリン(分子量281、沸点66〜67
℃)、3H−ヘプタフルオロ−4−トリフルオロメチル
−モルフォリン(分子量281、沸点63.5〜64.
5℃)、2H−ヘプタフルオロ−4−トリフルオロメチ
ル−モルフォリン(分子量281、沸点70℃以下)が
あり、これらは、沸点が70℃以下であり、ウレタンフ
ォームの発泡剤として発泡性が良好である。また、各発
泡剤を混合することが可能である。特に、フッ素化ヨウ
化炭化水素に、他のパーフルオロアルケンまたは水素含
有フッ化モルフォリン誘導体を混合する構成は、ハイブ
リッド効果によって樹脂発泡体の気泡形状を微細化し、
さらに自己消火性を付与することができる。Perfluoroalkenes useful as blowing agents are dimers of hexafluoropropene, such as perfluoro-4-methyl-2-pentene, perfluoro-2-methyl-2-pentene and their derivatives. There is a mixed composition, which has a boiling point of 48-51.
It has a molecular weight of 300.04 at a temperature of 300.degree. C. and is composed of total fluorocarbon containing one carbon-carbon unsaturated bond in the molecule. In addition to hexafluoropropene dimer, perfluoro-2
A compound selected from -pentene, (perfluorobutyl) ethylene, (perfluoropropyl) ethylene, and octafluorocyclopentane is preferable because it has a proper boiling point as a foaming agent. Hydrogen-containing fluorinated morpholine derivatives useful as effervescent agents are, for example, either monohydroperfluoromorpholine or monohydroperfluoromethylmorpholine, or mixtures thereof. As monohydroperfluoromorpholine, there are 3H-octafluoromorpholine (molecular weight 231) and 2H-octafluoromorpholine (molecular weight 231), and the boiling point of perfluoromorpholine is 34.5 ° C. Therefore, it is estimated to be 30 to 40 ° C. As monohydroperfluoromethylmorpholine, octafluoro-4-difluoromethyl-morpholine (molecular weight 281, boiling point 66 to 67) is used.
C.) 3H-heptafluoro-4-trifluoromethyl-morpholine (molecular weight 281, boiling point 63.5-64.
5 ° C.), 2H-heptafluoro-4-trifluoromethyl-morpholine (molecular weight 281, boiling point 70 ° C. or lower), which have a boiling point of 70 ° C. or lower and have good foamability as a foaming agent for urethane foam. Is. Further, it is possible to mix each foaming agent. In particular, the configuration in which the fluorinated iodohydrocarbon is mixed with another perfluoroalkene or a hydrogen-containing fluorinated morpholine derivative, the bubble shape of the resin foam is miniaturized by the hybrid effect,
Further, self-extinguishing property can be imparted.
【0037】以上に述べた本発明の発泡剤は、以下に示
すケトン、エーテル、エステルまたは炭化水素類と混合
して使用することによって、樹脂発泡体の強度や断熱性
能など、発泡体の物性を向上することができる。これら
ケトンなどの化合物は、前記発泡剤の樹脂原料に対する
相溶性改質、樹脂原料の粘度最適化、前記発泡剤との共
沸混合物となって沸点が下がるなどによって、発泡体の
物性向上に寄与するのである。本発明に適用されるケト
ンとしては、例えば、アセトン(分子量58.08、沸
点56℃)、2−ブタノン(分子量72.1、沸点80
℃)等がある。また、本発明に適用されるエーテルとし
ては、例えば、フラン(分子量68.1、沸点32
℃)、2ーメチルフラン(分子量82.1、沸点63〜
66℃)、テトラハイドロフラン(分子量72.1、沸
点66℃)、2−メチルテトラハイドロフラン(分子量
86.1、沸点78〜80℃)、1,3ージオキソラン
(分子量74.1、沸点74〜75℃)、2,5−ジヒ
ドロフラン(分子量70.1、沸点66〜67℃)等が
ある。The above-mentioned foaming agent of the present invention is used by mixing with the following ketones, ethers, esters or hydrocarbons to improve the physical properties of the foam such as the strength and heat insulation performance of the resin foam. Can be improved. These compounds such as ketones contribute to the improvement of the physical properties of the foam by modifying the compatibility of the foaming agent with the resin raw material, optimizing the viscosity of the resin raw material, and lowering the boiling point by forming an azeotropic mixture with the foaming agent. To do. Examples of the ketone applied to the present invention include acetone (molecular weight 58.08, boiling point 56 ° C.), 2-butanone (molecular weight 72.1, boiling point 80).
℃) etc. Further, as the ether applied to the present invention, for example, furan (molecular weight 68.1, boiling point 32
℃) 2-methylfuran (molecular weight 82.1, boiling point 63 ~
66 ° C.), tetrahydrofuran (molecular weight 72.1, boiling point 66 ° C.), 2-methyltetrahydrofuran (molecular weight 86.1, boiling point 78 to 80 ° C.), 1,3-dioxolane (molecular weight 74.1, boiling point 74 to 75 ° C.), 2,5-dihydrofuran (molecular weight 70.1, boiling point 66 to 67 ° C.) and the like.
【0038】本発明に適用されるエステルとしては、例
えば、酢酸メチル(分子量74.1、沸点57.5
℃)、酢酸エチル(分子量88.1、沸点76.5〜7
7.5℃)、蟻酸メチル(分子量60.1、沸点34
℃)、蟻酸エチル(分子量74.1、沸点52〜54
℃)等がある。本発明に適用される炭化水素としては、
例えば、シクロペンタン(分子量70.2、沸点49.
3℃)、イソペンタン(分子量72.2、沸点28
℃)、ノルマルペンタン(分子量72.2、沸点36.
1℃)、3−メチルペンタン(分子量86.2、沸点6
4℃)、シクロヘキサン(分子量84.2、沸点80.
7℃)、ネオヘキサン(分子量86.2、沸点49°
C)、イソヘキサン(分子量86.2、沸点63.3
℃)、ノルマルヘキサン(分子量86.2、沸点69.
7℃)等がある。特に、シクロペンタン、イソペンタン
およびノルマルペンタンは、熱伝導率が低く、独自に充
分発泡剤として機能するが、上記本発明の発泡剤と混合
することにより、発泡体の断熱性能を向上することがで
きる。また、これらの炭化水素は、可燃性、爆発性であ
るため取り扱いに危険性が伴うが、本発明の発泡剤と組
み合わせると、炭化水素の可燃性は低下し、難燃性、自
己消火性となる利点がある。Examples of the ester applicable to the present invention include methyl acetate (molecular weight: 74.1, boiling point: 57.5).
° C), ethyl acetate (molecular weight 88.1, boiling point 76.5-7)
7.5 ° C), methyl formate (molecular weight 60.1, boiling point 34
° C), ethyl formate (molecular weight 74.1, boiling point 52-54
℃) etc. Hydrocarbons applicable to the present invention include:
For example, cyclopentane (molecular weight 70.2, boiling point 49.
3 ° C), isopentane (molecular weight 72.2, boiling point 28)
C.), normal pentane (molecular weight 72.2, boiling point 36.
1 ° C), 3-methylpentane (molecular weight 86.2, boiling point 6)
4 ° C.), cyclohexane (molecular weight 84.2, boiling point 80.
7 ° C, neohexane (molecular weight 86.2, boiling point 49 °
C), isohexane (molecular weight 86.2, boiling point 63.3
C.), normal hexane (molecular weight 86.2, boiling point 69.
7 ° C) and so on. In particular, cyclopentane, isopentane, and normal pentane have low thermal conductivity, and independently function sufficiently as a foaming agent, but by mixing with the above-mentioned foaming agent of the present invention, the heat insulating performance of the foam can be improved. . Further, these hydrocarbons are flammable and explosive, and therefore are dangerous to handle, but when combined with the foaming agent of the present invention, the flammability of the hydrocarbon is lowered, and the flame retardancy and self-extinguishing properties are reduced. There are advantages.
【0039】水を発泡剤に使用することも好ましい。水
を発泡剤に使用すると、前記本発明の発泡剤の発泡性を
向上することが可能であり、これにより、微細な気泡を
有し、低密度の樹脂発泡体を形成することができる。ポ
リオール、触媒、整泡剤等の原料組成によって、上記に
示した混合発泡剤の効果が異なるから、適宜混合用の発
泡剤の種類および添加量を選択する必要がある。本発明
の発泡剤を使用する際に添加される還元剤としては、珪
酸、亜燐酸、硼酸、炭酸、チオ酸、例えばチオ硫酸の金
属塩などがある。特に、チオ硫酸ナトリウムは好ましい
還元剤である。これらは、気泡核としても作用するた
め、細かく砕いたミクロンオーダーの微粒子として添加
されることが好ましい。また、原料中に溶解していて、
発泡反応中に析出し、樹脂発泡体中に微粉末状態で含ま
れるのが好ましい。これらの微粉末は、界面活性剤と共
に添加され、互いに凝集せず、原料中で還元性を失わな
いものが好ましい。界面活性剤は、樹脂原料に添加され
るシリコン整泡剤が最も好ましく、一般に使用されるア
ニオン性、カチオン性、非イオン性界面活性剤いずれで
もよい。前記の還元剤は、界面活性剤と共にポリイソシ
アネート中に分散することが好ましい。この還元剤は、
発泡剤の分解によって生成する酸化性物質が樹脂に対し
て悪影響を及ぼすのを防ぐ作用をする。また、還元剤
は、微粒粉体として原料中に混合されるか、または発泡
過程で析出するため、発泡剤の気泡核として作用する。
界面活性剤は、前記粉体の安定な分散形態を得るために
必要である。It is also preferred to use water as the blowing agent. When water is used as the foaming agent, it is possible to improve the foamability of the foaming agent of the present invention, and thereby, a resin foam having fine cells and low density can be formed. Since the effect of the mixed foaming agent described above varies depending on the raw material composition of the polyol, the catalyst, the foam stabilizer, etc., it is necessary to appropriately select the type and the addition amount of the foaming agent for mixing. Examples of the reducing agent added when the foaming agent of the present invention is used include silicic acid, phosphorous acid, boric acid, carbonic acid, thioacids such as metal salts of thiosulfate. In particular, sodium thiosulfate is the preferred reducing agent. Since these also act as bubble nuclei, it is preferable to add them as finely crushed micron-order fine particles. Also, it is dissolved in the raw material,
It is preferably precipitated during the foaming reaction and contained in the resin foam in a fine powder state. These fine powders are preferably added together with a surfactant, do not aggregate with each other, and do not lose reducibility in the raw material. The surfactant is most preferably a silicone foam stabilizer added to the resin raw material, and may be any commonly used anionic, cationic or nonionic surfactant. The reducing agent is preferably dispersed in the polyisocyanate together with the surfactant. This reducing agent
It acts to prevent the oxidizing substances produced by the decomposition of the foaming agent from adversely affecting the resin. Further, the reducing agent acts as a bubble nucleus of the foaming agent because it is mixed in the raw material as a fine powder or is precipitated during the foaming process.
Surfactants are necessary to obtain a stable dispersion form of the powder.
【0040】前記の還元剤を含んだ本発明の好ましい製
造方法においては、チオ硫酸ナトリウムを溶解させた
水、または有機塩を溶解させたアルコ−ルもしくは水
を、界面活性剤とともにポリイソシアネ−トに分散させ
てエマルジョンとする。そして、このエマルジョンを、
発泡剤を含有するポリオ−ル組成物と混合し、発泡させ
ることによってポリウレタンフォ−ムを製造する。この
とき、エマルジョン中の前記水またはアルコール粒子
は、気泡核として働くうえに、ポリオ−ルとポリイソシ
アネ−トの混合による発熱でエマルジョンが崩壊し始め
ると、水またはアルコールはポリイソシアネ−トと反応
する。このため、水またはアルコールに溶解しているチ
オ硫酸ナトリウムまたは有機塩が析出し、これも気泡核
として働く。これによって、得られる発泡体の気泡はさ
らに小さくなる。In the preferred production method of the present invention containing the reducing agent, water in which sodium thiosulfate is dissolved or alcohol or water in which an organic salt is dissolved is added to a polyisocyanate together with a surfactant. Disperse into an emulsion. And this emulsion,
A polyurethane foam is produced by mixing with a polyol composition containing a foaming agent and foaming. At this time, the water or alcohol particles in the emulsion act as bubble nuclei, and when the emulsion starts to disintegrate due to the heat generated by mixing the polyol and polyisocyanate, the water or alcohol reacts with the polyisocyanate. Therefore, sodium thiosulfate or an organic salt dissolved in water or alcohol is deposited, which also acts as a bubble nucleus. This further reduces the bubbles in the resulting foam.
【0041】また、本発明の発泡剤は、例えばフッ素化
ヨウ化炭化水素等は分解し易く、樹脂形成反応中に一部
分解してヨウ素を遊離し、これが樹脂の劣化や樹脂に接
触する金属の腐食の原因になることが懸念される。しか
し、ヨウ素は、樹脂中に均一に分散したチオ硫酸ナトリ
ウムと反応して還元され、無害となる。Further, the foaming agent of the present invention is easily decomposed, for example, fluorinated iodohydrocarbon, and is partially decomposed during the resin formation reaction to liberate iodine, which deteriorates the resin or causes metal contact with the resin. There is concern that it may cause corrosion. However, iodine reacts with sodium thiosulfate uniformly dispersed in the resin to be reduced and becomes harmless.
【0042】ところで、フッ素化ヨウ化炭化水素を発泡
剤として樹脂を発泡させた場合には、ポリオ−ルとポリ
イソシアネ−トとの反応が遅くなり、他の発泡剤を用い
た場合に比較して気泡径が大きくなる。従って、フッ素
化ヨウ化炭化水素を発泡剤の一部として用いる場合に
は、特に前記のアルコ−ルとそれに溶解する塩を含有し
たポリオ−ル組成物を用いることが好ましい。このと
き、塩が気泡核として働く他、アルコ−ルがポリイソシ
アネ−トと反応することで樹脂化反応が加速される結
果、得られるポリウレタンフォ−ムの気泡径が小さくな
る。この作用は、通常の発泡剤を用いる場合に比較して
顕著となる。By the way, when the resin is foamed using the fluorinated iodohydrocarbon as the foaming agent, the reaction between the polyol and the polyisocyanate is delayed, and compared with the case where other foaming agents are used. The bubble diameter becomes large. Therefore, when the fluorinated iodohydrocarbon is used as a part of the foaming agent, it is particularly preferable to use the polyol composition containing the alcohol and the salt dissolved therein. At this time, in addition to the salt acting as a bubble nucleus, the resin reaction is accelerated by the reaction of the alcohol with the polyisocyanate, and as a result, the bubble diameter of the obtained polyurethane foam becomes small. This effect becomes more remarkable as compared with the case of using a normal foaming agent.
【0043】さらに、本発明の製造方法においては、炭
素数3以下の第一級あるいは第二級アルコ−ルに溶解す
る塩を原料に含ませておき、これら塩を発泡核として作
用させることができる。ポリオ−ルに加える炭素数3以
下の第一級または第二級アルコ−ルとしては、一価アル
コ−ルとしてメチルアルコ−ル、エチルアルコ−ル、イ
ソプロピルアルコ−ル、アリルアルコ−ル、二価アルコ
−ルとしてエチレングリコ−ル、1,3−プロパンジオ
−ル、三価アルコ−ルとしてグリセリン等がある。ま
た、前記塩としては、前記のアルコ−ルに5〜10重量
%程度以上溶解するものであれば有機塩、無機塩にかか
わらず好適に用いることができる。例えば、メチルアル
コ−ルに対しては、ヨウ化カルシウム、ヨウ化ナトリウ
ム、塩化リチウム、ヨウ化リチウム、ヨウ化カリウム、
臭化ストロンチウウム、臭化バリウム、臭化カルシウ
ム、臭化ナトリウム、硝酸カルシウム、硝酸マグネシウ
ム、塩化銅、ヨウ化マグネシウム、臭化ニッケル、安息
香酸カリウム、安息香酸リチウム、安息香酸亜鉛、安息
香酸アンモニウム、オレイン酸アンモニウム、酢酸リチ
ウム、酢酸カリウム、プロピオン酸カリウム、酪酸カリ
ウム、酪酸ナトリウム等を用いることができる。また、
エチルアルコ−ルに対しては、塩化カリウム、ヨウ化カ
リウム、ヨウ化ナトリウム、チオシアン酸ナトリウム、
臭化ストロンチウム、臭化ナトリウム、ヨウ化バリウ
ム、臭化カルシウム、硝酸カルシウム、塩化銅、塩化第
二鉄、臭化リチウム、ヨウ化マグネシウム、臭化アンモ
ニウム等を用いることができる。さらに、プロピルアル
コ−ルに対しては、ヨウ化リチウム、ヨウ化ナトリウ
ム、臭化カルシウム、塩化銅が、またイソピルアルコ−
ルに対しては、塩化銅等がそれぞれ用いられる。一般的
には樹脂の架橋密度を向上する効果も有する多価アルコ
−ルが好ましく、中でもエチレングリコ−ルが好まし
い。溶解する塩としては、溶解度が特に高い、炭酸カリ
ウム、塩化バリウム、ヨウ化カリウム、塩化リチウム、
臭化ナトリウムおよび塩化カルシウムが好ましい。気泡
核剤として気泡の微細化と架橋密度向上の効果を得るた
めには、上記多価アルコールをある程度以上添加する必
要がある。その量は、ポリオ−ル100重量部に対して
塩を0.5部が好ましい。この構成により、高い樹脂強
度を有し、かつ微細な気泡を有する発泡体を得ることが
できる。Further, in the production method of the present invention, a salt soluble in a primary or secondary alcohol having a carbon number of 3 or less may be included in the raw material, and these salts may act as foam nuclei. it can. Examples of primary or secondary alcohols having 3 or less carbon atoms added to the polyol include monohydric alcohols such as methyl alcohol, ethyl alcohol, isopropyl alcohol, allyl alcohol, and divalent alcohol. Examples of the glycol include ethylene glycol, 1,3-propanediol, and trivalent alcohol such as glycerin. Further, as the above-mentioned salt, any salt which can be dissolved in the above alcohol in an amount of about 5 to 10% by weight or more can be suitably used regardless of whether it is an organic salt or an inorganic salt. For example, for methyl alcohol, calcium iodide, sodium iodide, lithium chloride, lithium iodide, potassium iodide,
Strontium bromide, barium bromide, calcium bromide, sodium bromide, calcium nitrate, magnesium nitrate, copper chloride, magnesium iodide, nickel bromide, potassium benzoate, lithium benzoate, zinc benzoate, ammonium benzoate, olein Ammonium acid, lithium acetate, potassium acetate, potassium propionate, potassium butyrate, sodium butyrate and the like can be used. Also,
For ethyl alcohol, potassium chloride, potassium iodide, sodium iodide, sodium thiocyanate,
Strontium bromide, sodium bromide, barium iodide, calcium bromide, calcium nitrate, copper chloride, ferric chloride, lithium bromide, magnesium iodide, ammonium bromide and the like can be used. Further, for propyl alcohol, lithium iodide, sodium iodide, calcium bromide, copper chloride, and isopropyl alcohol can be used.
Copper chloride or the like is used for each of these. Generally, polyvalent alcohol which also has the effect of improving the crosslink density of the resin is preferable, and ethylene glycol is particularly preferable. As the soluble salt, particularly high solubility, potassium carbonate, barium chloride, potassium iodide, lithium chloride,
Sodium bromide and calcium chloride are preferred. In order to obtain the effects of making bubbles finer and increasing the crosslink density as a bubble nucleating agent, it is necessary to add the polyhydric alcohol to a certain extent or more. The amount is preferably 0.5 part of salt with respect to 100 parts by weight of polyol. With this configuration, it is possible to obtain a foam having high resin strength and fine bubbles.
【0044】本発明の発泡剤を使用する場合に、原料の
粘度低下、および発泡剤の原料との相溶性の改善を目的
として、以下に示すカーボネート化合物、エステルまた
はエポキシドを樹脂原料に加えることが好ましい。これ
らの添加剤は、容易に気化しないことが好ましく、沸点
が100℃以上の化合物がよい。また、樹脂原料の30
wt%以下の割合で添加するのが、樹脂の熱伝導率を低
くするために好ましい。ここに用いる有機カーボネート
化合物としては、ジメチルカーボネート、プロピレンカ
ーボネート、1,2−ブチレンカーボネート、へキシレ
ンカーボネート、スチレンカーボネート、ビニルエチレ
ンカーボネート、フェニルエチレンカーボネートなどが
好ましく、エポキシドと二酸化炭素の付加反応によって
生成したカーボネート化合物も好ましい。エステルとし
てはフタル酸エステル、燐酸エステル、アジピン酸エス
テル、アゼライン酸エステル、セバチン酸エステル、ア
クリル酸エステル、メタクリル酸エステル等が使用され
る。エポキシドとしては、エポキシブチルステアレー
ト、エポキシオクチルステアレート、安息香酸グリシジ
ルエステルなどが代表的なものである。後述するような
二酸化炭素を固定化するエポキシドも好ましい。When the foaming agent of the present invention is used, the following carbonate compound, ester or epoxide may be added to the resin raw material for the purpose of reducing the viscosity of the raw material and improving the compatibility of the foaming agent with the raw material. preferable. It is preferable that these additives do not easily vaporize, and compounds having a boiling point of 100 ° C. or higher are preferable. In addition, 30 of resin raw materials
It is preferable to add it in a proportion of not more than wt% in order to reduce the thermal conductivity of the resin. The organic carbonate compound used here is preferably dimethyl carbonate, propylene carbonate, 1,2-butylene carbonate, hexylene carbonate, styrene carbonate, vinyl ethylene carbonate, phenyl ethylene carbonate, or the like, which is produced by an addition reaction of epoxide and carbon dioxide. Carbonate compounds are also preferred. As the ester, phthalic acid ester, phosphoric acid ester, adipic acid ester, azelaic acid ester, sebacic acid ester, acrylic acid ester, methacrylic acid ester and the like are used. Typical epoxides are epoxy butyl stearate, epoxy octyl stearate, glycidyl benzoate and the like. An epoxide that fixes carbon dioxide as described below is also preferable.
【0045】また、本発明の発泡剤の酸化、分解を抑制
するための酸素吸収剤として、Cu、Cu2O、Fe、
マグネタイト、コバルト、ニッケル、亜鉛、Na2S2O
3などを混合したフォームは、長期にわたって高い断熱
性を保持するために好ましい。また、Cu、Na2S2O
3などは、遊離ヨウ素を還元し、フォームを安定に保つ
効果もある。Further, as an oxygen absorbent for suppressing the oxidation and decomposition of the blowing agent of the present invention, Cu, Cu 2 O, Fe
Magnetite, cobalt, nickel, zinc, Na 2 S 2 O
A foam in which 3 or the like is mixed is preferable because it retains a high heat insulating property for a long time. In addition, Cu, Na 2 S 2 O
3 etc. also has the effect of reducing free iodine and keeping the foam stable.
【0046】また、フッ素化ヨウ化炭化水素を発泡剤と
して使用する場合、発泡性をよりよくするためには、ポ
リオールとしては非アミン系ポリオールを用いることが
好ましい。一般に、断熱材に使用されているウレタン原
料であるポリオールは、重合反応開始剤のアミン、反応
調製剤のエタノールアミンなどを添加した組成物として
使用される。しかし、これらのアミン系ポリオールは、
フッ素化ヨウ化炭化水素と相互作用するため避ける必要
がある。そこで、非アミン系のポリオールを使用して断
熱性を向上するのが好ましい。そのようなポリオールと
しては、多価アルコール、糖類を反応開始剤にしたアル
キレンオキシドを付加して得られるポリエーテルポリオ
ールや、多価アルコールー多価カルボン酸縮合系、ある
いは環状エステル開環重合体系のポリエステルポリオー
ルが好ましく、二個以上のフェノール性水酸基を有する
化合物なども使用できる。また、多価アルコールがその
まま混合された組成物でもよい。フッ素化ヨウ化炭化水
素をポリイソシアネートに混合した組成物として樹脂発
泡体を製造する方法は、フッ素化ヨウ化炭化水素がポリ
イソシアネート中に安定に分散できるという特徴があ
り、断熱性樹脂発泡体の製造にあたってポリオールでな
く、ポリイソシアネート中に前記発泡剤をエマルジョン
化して添加する方法である。また、この方法により気泡
を細かくできるため好ましい。When a fluorinated iodohydrocarbon is used as a foaming agent, a non-amine type polyol is preferably used as the polyol in order to improve the foamability. In general, a polyol, which is a urethane raw material used for a heat insulating material, is used as a composition to which an amine as a polymerization reaction initiator, ethanolamine as a reaction preparation agent and the like are added. However, these amine-based polyols
It should be avoided as it interacts with fluorinated iodohydrocarbons. Therefore, it is preferable to improve the heat insulating property by using a non-amine type polyol. Examples of such polyols include polyhydric alcohols, polyether polyols obtained by adding alkylene oxides using saccharides as reaction initiators, polyhydric alcohol-polycarboxylic acid condensation systems, or polyesters of cyclic ester ring-opening polymer systems. Polyols are preferable, and compounds having two or more phenolic hydroxyl groups can also be used. Further, a composition in which polyhydric alcohol is directly mixed may be used. The method for producing a resin foam as a composition in which a fluorinated iodohydrocarbon is mixed with polyisocyanate is characterized in that the fluorinated iodohydrocarbon can be stably dispersed in the polyisocyanate. It is a method of emulsifying the foaming agent in polyisocyanate instead of polyol in the production. In addition, this method is preferable because bubbles can be made finer.
【0047】フッ素化ヨウ化炭化水素と、非共役系のア
ミンあるいはアンモニウム塩、または四級アンモニウム
塩等の塩基は、容易に錯化合物を形成する。その錯化合
物は、化合物の組み合わせにより錯形成状態が異なる。
例えば、ヘプタフルオロー2ーアイオドプロパンとN,
N,N’,N’−テトラメチルヘキサメチレンジアミン
とは、相互作用が非常に強く、ヨウ素とアミンをモル比
1対1で混合すると茶褐色の固体が生成する。これを単
離し水に溶解すると、二層に分離し、上層は水と前記テ
トラメチルヘキサメチレンジアミンから成り、下層は少
量のテトラメチルヘキサメチレンジアミンと前記ヘプタ
フルオロー2ーアイオドプロパンからなることが確認さ
れた。このことから、錯化合物が形成されていると考え
られる。この錯化合物は、光に対して分解することはな
かった。The fluorinated iodohydrocarbon and a base such as a non-conjugated amine or ammonium salt, or a quaternary ammonium salt easily form a complex compound. The complex compound has a different complex formation state depending on the combination of compounds.
For example, heptafluoro-2-iodopropane and N,
The interaction with N, N ′, N′-tetramethylhexamethylenediamine is very strong, and a dark brown solid is produced when iodine and amine are mixed at a molar ratio of 1: 1. When this was isolated and dissolved in water, it was separated into two layers, and it was confirmed that the upper layer was composed of water and the tetramethylhexamethylenediamine, and the lower layer was composed of a small amount of tetramethylhexamethylenediamine and the heptafluoro-2-iodopropane. Was done. From this, it is considered that the complex compound is formed. This complex compound did not decompose with light.
【0048】また、芳香族系アミンの一種であるイミダ
ゾール化合物を同様にヘプタフルオロー2ーアイオドプ
ロパンと混合すると、どのような混合比においても錯化
合物の固体は形成されなかった。しかし、その混合物を
加熱すると、通常40℃で沸騰するはずのヘプタフルオ
ロー2ーアイオドプロパンが、70℃以上に加熱しても
沸騰せず、80℃以上でようやく沸騰した。これに水を
添加すると、二層に分離し、ヘプタフルオロー2ーアイ
オドプロパンの沸点付近で沸騰した。この分離層の上層
はやはり水とアミンの混合物であり、下層は、アイオド
プロパンが主成分であった。このようなことから、弱い
相互作用で錯化合物を形成していると考えられる。ま
た、ヘプタフルオロー2ーアイオドプロパンの異性体で
あるヘプタフルオロー1ーアイオドプロパンをN,N,
N’,N’−テトラメチルヘキサメチレンジアミンと混
合すると、固体錯化合物は得られず、80℃以上でも沸
騰しない液体となった。水を加えると、二層に分離する
ことから、弱いながらも錯化合物を形成していると考え
られる。When an imidazole compound, which is a kind of aromatic amine, was mixed with heptafluoro-2-iodopropane in the same manner, no complex compound solid was formed at any mixing ratio. However, when the mixture was heated, heptafluoro-2-iodopropane, which should normally boil at 40 ° C., did not boil when heated to 70 ° C. or higher, and finally boiled at 80 ° C. or higher. When water was added to this, it separated into two layers and boiled around the boiling point of heptafluoro-2-iodopropane. The upper layer of this separation layer was again a mixture of water and amine, and the lower layer was mainly composed of iodopropane. From this, it is considered that a complex compound is formed by weak interaction. In addition, heptafluoro-1-iodopropane, which is an isomer of heptafluoro-2-iodopropane, was converted into N, N,
When mixed with N ′, N′-tetramethylhexamethylenediamine, a solid complex compound was not obtained, and a liquid did not boil even at 80 ° C. or higher. When water is added, it separates into two layers, so it is considered that a complex compound is formed although it is weak.
【0049】このように、フッ素化ヨウ化炭化水素とア
ミンとの錯化合物は、用いる化合物によっては液体状態
または固体状態であり、その結合力にも違いがあること
を利用し、多くの機能を有する断熱性樹脂発泡体を形成
することができる。一般的な傾向として、用いられるア
ミン化合物が、低級のものほど強い結合力を有し、用い
られるフッ素化ヨウ化炭化水素が、ヨウ素の極性が高い
化合物ほど強い結合力を示す。As described above, the complex compound of a fluorinated iodohydrocarbon and an amine is in a liquid state or a solid state depending on the compound to be used, and the bonding force is different. It is possible to form a heat insulating resin foam having the above. As a general tendency, the lower the amine compound used, the stronger the bond strength, and the more fluorinated iodohydrocarbon used, the stronger the iodine bond, the stronger the bond strength.
【0050】本発明に適用するのに好適な錯化合物は、
樹脂反応熱で容易に分解するものであり、分解により生
成するフッ素化ヨウ化炭化水素が発泡剤として機能す
る。そのような好ましい錯化合物は、フッ素化ヨウ化炭
化水素と、非共役系の三級アミン、アンモニウム塩およ
び四級アンモニウム塩のうちの一種との錯化合物の中か
ら選ばれる。この錯化合物を、ウレタン反応触媒ととも
に用いる場合、前記錯化合物は感温型ウレタン反応触媒
としても機能する。通常、三級アミンがウレタン反応触
媒として用いられる。このような三級アミンとフッ素化
ヨウ化炭化水素との錯化合物が本発明にとって最も好ま
しい。この錯化合物は、それ自体はウレタン反応に対す
る触媒活性は非常に低いが、樹脂反応熱が発生して錯化
合物がアミンとフッ素化ヨウ化炭化水素に分離すると、
分離したアミンがウレタン反応触媒として作用する。そ
のとき、フッ素化ヨウ化炭化水素は、気化して発泡剤と
なるか、樹脂反応が終わると再びアミンと錯化合物を形
成して発泡樹脂組成物中に存在することが好ましい。従
来は、ウレタン反応触媒であるアミンが樹脂中に残存す
ると、樹脂の劣化や断熱性能の悪化をもたらしていた。
しかし、前記のように、フッ素化ヨウ化炭化水素が、樹
脂反応終了後、再びアミンと錯化合物を形成する場合
は、そのような不都合をなくすもできる。また、一級、
二級アミンは、一般にウレタン反応触媒として使用され
ていないが、フッ素化ヨウ化炭化水素との錯化合物は、
ウレタン反応の弱触媒となり、さらには、イソシアネー
トと反応して樹脂となるため好ましい。Complex compounds suitable for use in the present invention are:
It is easily decomposed by heat of resin reaction, and the fluorinated iodohydrocarbon produced by the decomposition functions as a foaming agent. Such preferred complex compounds are selected from complex compounds of fluorinated iodohydrocarbons with one of non-conjugated tertiary amines, ammonium salts and quaternary ammonium salts. When this complex compound is used together with a urethane reaction catalyst, the complex compound also functions as a temperature-sensitive urethane reaction catalyst. Usually, tertiary amines are used as urethane reaction catalysts. Such a complex compound of a tertiary amine and a fluorinated iodohydrocarbon is most preferred for the present invention. This complex compound itself has a very low catalytic activity for the urethane reaction, but when the resin reaction heat is generated and the complex compound is separated into amine and fluorinated iodohydrocarbon,
The separated amine acts as a urethane reaction catalyst. At this time, it is preferable that the fluorinated iodohydrocarbon is present in the foamed resin composition by vaporizing to become a foaming agent or forming a complex compound with the amine again after the resin reaction is completed. Conventionally, when amine, which is a urethane reaction catalyst, remains in the resin, it causes deterioration of the resin and deterioration of heat insulating performance.
However, as described above, when the fluorinated iodohydrocarbon forms a complex compound with the amine again after the completion of the resin reaction, such inconvenience can be eliminated. Also, first grade,
Secondary amines are not commonly used as urethane reaction catalysts, but complex compounds with fluorinated iodohydrocarbons
It is preferable because it serves as a weak catalyst for the urethane reaction and further reacts with isocyanate to form a resin.
【0051】また、この錯化合物は、水の添加によって
分解するため、水を用いた制御が可能である。そして、
錯化合物が感温型ウレタン反応触媒となる場合、水を添
加して錯化合物を分解すると、ウレタン反応に対する活
性が高まることを利用して、発泡反応を制御することが
可能である。水は、発泡剤としても作用するため、ポリ
オール100重量部に対して、10重量部以下で添加す
ることが最も好ましい。Further, since this complex compound is decomposed by addition of water, control using water is possible. And
When the complex compound serves as a temperature-sensitive urethane reaction catalyst, it is possible to control the foaming reaction by utilizing the fact that when the complex compound is decomposed by adding water, the activity for the urethane reaction is increased. Since water also acts as a foaming agent, it is most preferable to add 10 parts by weight or less to 100 parts by weight of the polyol.
【0052】第一級アミンとして使用される物質として
は、エチルアミン、ブチルアミン、プロピルアミン、ヘ
キシルアミン等のアルキルアミン、エタノールアミン等
のアミノアルコール、アミノベンゼン、アミノベンズイ
ミダゾール等に代表される芳香環に一級アミンの付加し
た化合物、アントラニル酸などのアミノ基含有有機酸等
が好ましい。第二級アミンとしては、前記第一級アミン
のアルキル基付加化合物、環状アミン、スルファミン
酸、アミノ酸等が好ましい。第三級アミンとしては、前
記第二級アミンのアルキル基付加物などが適している。
特に、ウレタン反応触媒活性を示す化合物として、一般
的な三級アミン化合物も適している。一般に使用される
アミン系ウレタン反応触媒は、N,N,N’,N’−テ
トラメチルヘキサメチレンジアミン、N,N,N’,
N’,N’−ペンタメチルジエチレントリアミン、トリ
メチルアミノエチルピペラジン、N,N’,N”−トリ
ス(3−ジメチルアミノプロピル)ヘキサヒドロ−sー
トリアジン、Nートリオキシエチレン−N,N−ジメチ
ルアミン、トリエチレンジアミン、N,Nージメチルヘ
キシルアミン、N,Nージメチルベンジルアミン、N−
メチルモルフォリン等が好ましい。Examples of the substance used as the primary amine include alkylamines such as ethylamine, butylamine, propylamine and hexylamine, amino alcohols such as ethanolamine, aromatic rings represented by aminobenzene, aminobenzimidazole and the like. A compound to which a primary amine is added, an amino group-containing organic acid such as anthranilic acid, and the like are preferable. The secondary amine is preferably an alkyl group addition compound of the above primary amine, a cyclic amine, sulfamic acid, an amino acid or the like. As the tertiary amine, an alkyl group adduct of the secondary amine and the like are suitable.
In particular, a general tertiary amine compound is also suitable as a compound having urethane reaction catalytic activity. Commonly used amine-based urethane reaction catalysts include N, N, N ′, N′-tetramethylhexamethylenediamine, N, N, N ′,
N ', N'-pentamethyldiethylenetriamine, trimethylaminoethylpiperazine, N, N', N "-tris (3-dimethylaminopropyl) hexahydro-s-triazine, N-trioxyethylene-N, N-dimethylamine, tri Ethylenediamine, N, N-dimethylhexylamine, N, N-dimethylbenzylamine, N-
Methylmorpholine and the like are preferable.
【0053】アンモニウム塩および四級アンモニウム塩
としては、一般に、アミンの有機酸塩、フェノール塩、
ハロゲン塩が望ましく、テトラブチルアンモニウムブロ
マイド、テトラブチルアンモニウムアイオダイド、1,
8ージアザビシクロ−(5,4,0)ウンデセンー7の
フェノール塩などは、ウレタン反応触媒としてだけでな
く、エポキシドが二酸化炭素と反応してこれを固定化す
る二酸化炭素固定化触媒としても使用できるため好まし
い。前記錯化合物に添加可能なウレタン反応触媒は、有
機スズ化合物、有機酸の金属塩、芳香族アミン、有機リ
ン化合物が好ましい。これらの化合物は、フッ素化ヨウ
化炭化水素などハロゲンと相互作用しにくく、ウレタン
反応触媒活性を低下することがないためである。Ammonium salts and quaternary ammonium salts are generally organic acid salts of amines, phenol salts,
Halogen salts are desirable, tetrabutylammonium bromide, tetrabutylammonium iodide, 1,
Phenol salts of 8-diazabicyclo- (5,4,0) undecene-7 and the like are preferable because they can be used not only as a urethane reaction catalyst, but also as a carbon dioxide-immobilized catalyst in which an epoxide reacts with carbon dioxide to immobilize it. . The urethane reaction catalyst that can be added to the complex compound is preferably an organic tin compound, a metal salt of an organic acid, an aromatic amine, or an organic phosphorus compound. This is because these compounds do not easily interact with halogens such as fluorinated iodohydrocarbons and do not lower the urethane reaction catalyst activity.
【0054】有機スズ化合物としては、ジブチル錫ジラ
ウレート、ジブチル錫ジアセテート、ジオクチル錫ジバ
ーサテート、ジオクチル錫ジラウレート、ジオクチル錫
ジアセテート、酸化ジオクチル錫、ジオクチル錫ジアル
キルメルカプタンなどが好ましい。有機酸の金属塩とし
ては、ステアリン酸亜鉛、酢酸カリウム、オクチル酸カ
リウム、ぎ酸のアルカリ金属塩などが好ましい。これら
の触媒は、樹脂中においてイソシアヌレート構造を作る
のに効果的であり、難燃性を付与するため好ましい。芳
香族アミンは、アミンでありながら、フッ素化ヨウ化炭
化水素との相互作用は非常に弱く、ウレタン反応触媒活
性を低下することがないため好ましい。一般的な芳香族
アミンは、弱触媒として作用する。特に、骨格としてピ
ロール、イミダゾール、ピリミジン、トリアジン、ベン
ズイミダゾールを有する化合物などが好ましい。有機リ
ン化合物は、フォスフォレンオキシド骨格を有する化合
物が好ましく、カルボジイミド結合によって樹脂発泡体
の強度を増加するのに適している。また、テトラフェニ
ルフォスフォナート、トリフェニルメチルフォスフォナ
ート、テトラブチルフォスフォナートなどはウレタン反
応触媒としてだけでなく、二酸化炭素固定化触媒として
も作用するため好ましい。As the organic tin compound, dibutyltin dilaurate, dibutyltin diacetate, dioctyltin diversate, dioctyltin dilaurate, dioctyltin diacetate, dioctyltin oxide, dioctyltin dialkylmercaptan and the like are preferable. As the metal salt of an organic acid, zinc stearate, potassium acetate, potassium octylate, an alkali metal salt of formic acid and the like are preferable. These catalysts are preferable because they are effective in forming an isocyanurate structure in the resin and impart flame retardancy. Aromatic amines are preferable because they are amines but have a very weak interaction with fluorinated iodohydrocarbons and do not lower the urethane reaction catalyst activity. Common aromatic amines act as weak catalysts. In particular, compounds having pyrrole, imidazole, pyrimidine, triazine, benzimidazole as a skeleton and the like are preferable. The organic phosphorus compound is preferably a compound having a phospholene oxide skeleton and is suitable for increasing the strength of the resin foam by a carbodiimide bond. Further, tetraphenylphosphonate, triphenylmethylphosphonate, tetrabutylphosphonate and the like are preferable because they act not only as a urethane reaction catalyst but also as a carbon dioxide fixing catalyst.
【0055】本発明において、二酸化炭素をエポキシド
と反応させて固定化することによって、樹脂発泡体中に
カーボネート化合物を生成させのに使用される好ましい
化合物を以下に示す。樹脂原料組成物中に添加され、二
酸化炭素を固定化するエポキシドとしては、沸点が低く
発泡剤としても作用するプロピレンオキシド、ブチレン
オキシドなどがある。また、オクチレンオキシド、へキ
シレンオキシドなどのアルキル鎖にエポキシ環を有する
化合物;メチルグリシジルエーテル、ブチルグリシジル
エーテル、フェニルグリシジルエーテル、メタクリル酸
グリシジルエーテルなどのグリシジルエーテル化合物;
エピクロルヒドリン、グリシドール、スチレンオキシ
ド、N−(2,3−エポキシプロピル)フタルイミド、
3ーグリシジルオキシプロピルトリメチルシランなど
は、常温で単官能の液体または固体のエポキシドであ
り、二酸化炭素を固定するだけでなく、樹脂組成物中に
おいて前述の添加剤として作用するため好ましい。In the present invention, preferable compounds used for forming a carbonate compound in a resin foam by reacting carbon dioxide with an epoxide to immobilize it are shown below. Examples of the epoxide added to the resin raw material composition to fix carbon dioxide include propylene oxide and butylene oxide, which have a low boiling point and also act as a foaming agent. Further, compounds having an epoxy ring in the alkyl chain such as octylene oxide and hexylene oxide; glycidyl ether compounds such as methyl glycidyl ether, butyl glycidyl ether, phenyl glycidyl ether, and methacrylic acid glycidyl ether;
Epichlorohydrin, glycidol, styrene oxide, N- (2,3-epoxypropyl) phthalimide,
3-Glycidyloxypropyltrimethylsilane and the like are monofunctional liquid or solid epoxides at room temperature, and are preferable because they not only fix carbon dioxide but also act as the aforementioned additives in the resin composition.
【0056】また、多官能のエポキシドは、ハイドロキ
ノンジグリシジルエーテル、レゾルシンジグリシジルエ
ーテル、ネオペンチルグリシジルエーテル、ペンタエリ
スリトールポリグリシジルエーテル、オルトフタル酸ジ
グルシジルエーテル、ソルビトールテトラグリシジルエ
ーテル、ヘキサメチレンジオールジグリシジルエーテル
などの他に、ポリグリセロールトリグリシジルエーテル
などがある。これらの多官能のエポキシドは、重合して
樹脂素材となりうるので、二酸化炭素を固定するだけで
なく発泡樹脂組成物原料としても好ましい。The polyfunctional epoxides include hydroquinone diglycidyl ether, resorcin diglycidyl ether, neopentyl glycidyl ether, pentaerythritol polyglycidyl ether, orthophthalic acid diglycidyl ether, sorbitol tetraglycidyl ether, hexamethylene diol diglycidyl ether, etc. Besides, there are polyglycerol triglycidyl ether and the like. Since these polyfunctional epoxides can be polymerized into a resin material, they are preferable not only for fixing carbon dioxide but also as a raw material for a foamed resin composition.
【0057】二酸化炭素固定化触媒としての求核剤に
は、塩素、臭素、ヨウ素等のハロゲンのイオンが好まし
く、オニウム塩であることが好ましい。オニウム塩のな
かでも効果的なものは、臭化テトラブチルアンモニウ
ム、ヨウ化テトラブチルアンモニウムなどに代表される
アンモニウム塩である。また、テトラフェニルフォスフ
ォニウムブロマイド、トリフェニルメチルフォスフォニ
ウムブロマイドに代表されるホスフォニウム塩、トリブ
チルスルフォニウムブロマイドに代表されるスルフォニ
ウム塩も好ましい。また、アミン化合物とハロゲン化物
の錯化合物も用いられる。発泡剤のフッ素化ヨウ化炭化
水素と、アミンあるいはアンモニウム塩、または四級ア
ンモニウム塩との錯化合物も用いられる。また、三級ア
ミン、アンモニウム塩または四級アンモニウム塩とフッ
素化ヨウ化炭化水素との錯化合物は、容易にハロゲンイ
オンを生成するため好ましい。As the nucleophilic agent as the carbon dioxide fixing catalyst, halogen ions such as chlorine, bromine and iodine are preferable, and onium salts are preferable. Among the onium salts, effective ones are ammonium salts represented by tetrabutylammonium bromide and tetrabutylammonium iodide. Further, phosphonium salts represented by tetraphenylphosphonium bromide, triphenylmethylphosphonium bromide, and sulfonium salts represented by tributylsulfonium bromide are also preferable. Further, a complex compound of an amine compound and a halide is also used. A complex compound of a fluorinated iodohydrocarbon as a blowing agent and an amine or ammonium salt or a quaternary ammonium salt is also used. Further, a complex compound of a tertiary amine, an ammonium salt or a quaternary ammonium salt and a fluorinated iodohydrocarbon is preferable because it easily produces a halogen ion.
【0058】二酸化炭素固定化触媒としての求電子剤に
は、亜鉛化合物、錫化合物が用いられる。亜鉛化合物と
しては、塩化亜鉛、臭化亜鉛、ヨウ化亜鉛、酢酸亜鉛、
ステアリン酸亜鉛、亜鉛アセチルアセトナート、クエン
酸亜鉛などがある。また、錫化合物としては、塩化錫な
どのハロゲン化錫;ジブチル錫ジラウレート、ジオクチ
ル錫ジバーサテート、ジブチル錫ジアセテートなどの有
機スズ化合物が好ましい。これらは、ウレタン反応触媒
としても使用される物質であるため本発明に有用であ
る。また、ハロゲン化アルカリを二酸化炭素固定化触媒
として使用することもできる。なかでも臭化リチウム、
ヨウ化リチウム、塩化リチウム;ナトリウム、カリウム
のハロゲン化物は好ましい。また、塩化鉄、塩化銅、塩
化コバルト、塩化マンガン、塩化クロムなども好ましい
二酸化炭素固定化触媒である。Zinc compounds and tin compounds are used as electrophiles as carbon dioxide fixing catalysts. Zinc compounds include zinc chloride, zinc bromide, zinc iodide, zinc acetate,
Examples include zinc stearate, zinc acetylacetonate, and zinc citrate. As the tin compound, tin halides such as tin chloride; organotin compounds such as dibutyltin dilaurate, dioctyltin diversate and dibutyltin diacetate are preferable. These are useful in the present invention because they are substances that are also used as urethane reaction catalysts. Also, an alkali halide can be used as a carbon dioxide-immobilized catalyst. Lithium bromide,
Halides of lithium iodide, lithium chloride; sodium and potassium are preferred. Further, iron chloride, copper chloride, cobalt chloride, manganese chloride, chromium chloride and the like are also preferable carbon dioxide fixed catalysts.
【0059】本発明では、前記求核剤および/または求
電子剤からなる二酸化炭素固定化触媒をフッ素化ヨウ化
炭化水素とともにイソシアネートに混合した組成物とす
る。また、エポキシドはポリオールに混合する。これら
のイソシアネート組成物とポリオール組成物とを混合し
て発泡反応を行わせるのが好ましい。これによって二酸
化炭素固定化反応を活性化し、高効率化することができ
る。すなわち、エポキシドが、二酸化炭素を充分固定化
するためには、二酸化炭素固定化触媒を二酸化炭素に接
するまで安定に保存することが有用である。イソシアネ
ート中に二酸化炭素固定化触媒を添加し、さらにフッ素
化ヨウ化炭化水素を混合することによって、二酸化炭素
固定化触媒を安定に保存できるのである。また、二酸化
炭素固定化触媒は、フッ素化ヨウ化炭化水素と相互作用
して安定化しているため、この状態では二酸化炭素固定
化触媒効果はない。イソシアネート組成物とポリオール
組成物が混合されて、樹脂反応熱によってフッ素化ヨウ
化炭化水素が気化すると、二酸化炭素固定化触媒作用を
起こす。The present invention provides a composition in which a carbon dioxide-immobilized catalyst comprising the nucleophile and / or the electrophile is mixed with isocyanate together with fluorinated iodohydrocarbon. Also, the epoxide is mixed with the polyol. It is preferable to mix these isocyanate composition and polyol composition to carry out the foaming reaction. As a result, the carbon dioxide immobilization reaction can be activated and the efficiency can be increased. That is, in order for the epoxide to sufficiently immobilize carbon dioxide, it is useful to store the carbon dioxide-immobilized catalyst stably until it comes into contact with carbon dioxide. The carbon dioxide-immobilized catalyst can be stably stored by adding the carbon dioxide-immobilized catalyst to the isocyanate and further mixing the fluorinated iodohydrocarbon. Further, since the carbon dioxide-immobilized catalyst interacts with the fluorinated iodohydrocarbon and is stabilized, there is no carbon dioxide-immobilized catalyst effect in this state. When the isocyanate composition and the polyol composition are mixed and the fluorinated iodohydrocarbon is vaporized by the heat of the resin reaction, a carbon dioxide-immobilizing catalytic action occurs.
【0060】また、あらかじめ、フッ素化ヨウ化炭化水
素と二酸化炭素固定化触媒を錯化合物として添加する
と、なお効率良くエポキシドと二酸化炭素が反応するの
で好ましい。また、フッ素化ヨウ化化炭化水素がアミン
と錯化合物を形成し、遊離のアイオドイオンを生成し二
酸化炭素固定化触媒となる構成も好ましい。この場合も
エポキシドと二酸化炭素固定化触媒を互いに隔離するこ
とが好ましい。錯形成によって安定化しているため、不
要な反応が起こらず、効率良くエポキシドが二酸化炭素
と反応する。また、二酸化炭素固定後は、反応熱で活性
であった二酸化炭素固定化触媒が、ゆっくりとフッ素化
ヨウ化炭化水素と錯化合物に戻り活性を失うことも、樹
脂劣化を引き起こさないために好ましい。Further, it is preferable to previously add the fluorinated iodohydrocarbon and the carbon dioxide-immobilized catalyst as a complex compound because the epoxide and the carbon dioxide react more efficiently. Further, it is also preferable that the fluorinated iodinated hydrocarbon forms a complex compound with an amine to generate a free iodo ion to serve as a carbon dioxide-immobilized catalyst. Also in this case, it is preferable to separate the epoxide and the carbon dioxide-immobilized catalyst from each other. Since it is stabilized by complex formation, unnecessary reaction does not occur and the epoxide reacts efficiently with carbon dioxide. Further, it is also preferable that the carbon dioxide-immobilized catalyst, which was active by the heat of reaction after the carbon dioxide is immobilized, slowly returns to the complex compound with the fluorinated iodohydrocarbon and loses the activity because it does not cause resin deterioration.
【0061】本発明に用いられる整泡剤の役割は、原料
の相溶性を高めること、および気泡核となって樹脂原料
の表面張力を低下させて発泡中の気泡を安定化させるこ
とである。特に、シリコン系界面活性剤が用いられる。
本発明では、発泡剤がフッ素を有する化合物であるた
め、気泡を安定化するために、ジメチルシロキサンーオ
キシアルキレン共重合体と分子中にフルオロアルキル基
を有するジメチルシロキサンーオキシアルキレン共重合
体とを含む整泡剤を用いることが好ましい。従来のシリ
コン系界面活性剤では、フッ素系発泡剤を使用した際、
気泡が安定化しにくく、発泡課程において不均一化、破
泡などが起こる。フッ素系アルキル基を有している整泡
剤は、本発明の発泡剤と混合しやすく、なおかつ従来の
気泡安定化効果を有するものである。本発明において整
泡剤として用いられるシリコン系界面活性剤には、化4
に示されるものがある。The role of the foam stabilizer used in the present invention is to increase the compatibility of the raw materials and to serve as cell nuclei to reduce the surface tension of the resin raw material and stabilize the bubbles during foaming. In particular, a silicon-based surfactant is used.
In the present invention, since the foaming agent is a compound having fluorine, in order to stabilize the bubbles, a dimethylsiloxane-oxyalkylene copolymer and a dimethylsiloxane-oxyalkylene copolymer having a fluoroalkyl group in the molecule are used. It is preferable to use a foam stabilizer containing the same. With conventional silicone-based surfactants, when using a fluorine-based foaming agent,
Bubbles are difficult to stabilize, resulting in non-uniformity and foam breaking during the foaming process. The foam stabilizer having a fluorinated alkyl group is easy to mix with the foaming agent of the present invention and has a conventional bubble stabilizing effect. The silicone-based surfactant used as the foam stabilizer in the present invention includes:
There is something shown in.
【0062】[0062]
【化4】 [Chemical 4]
【0063】(ただし、R、R’、R”は、各々独立に
−H、−COCH3、−(CH2)xCH3または−(CF2)y
CF3であり、Meはメチル基である。また、a、bは
1〜10、x、yは1〜18である) 本発明に用いるポリオールは、フッ素化ヨウ化炭化水素
を発泡剤として使用する目的以外は、従来使われている
ポリエーテル系ポリオール、ポリエステル系ポリオール
が適している。このほか、硬度を得るため、または反応
性を制御する目的で、多価アルコールから合成される水
酸基を多く分子内に有するポリオールが適している。ま
た、ポリオール分子内に、水酸基とともに三級アミン、
リン、またはハロゲンを含む触媒含有ポリオール、難燃
性ポリオール、芳香族系ポリオールも適している。発泡
性を向上するために、ポリオールに水を添加すること
は、好ましい技術である。本発明における沸点の比較的
高い発泡剤とともに水を添加した場合には、低密度フォ
ームを形成し、気泡を均一かつ微細化することができ
る。同様に、アルコ−ルを添加することにより、アルコ
ールがイソシアネートと反応する際の反応熱によって、
水と同じく発泡剤の発泡性を向上することができるため
好ましい。利用できるアルコールとしては、メタノー
ル、エタノール、エチレングリコール、グリセリン、ペ
ンタエリスリトール、α−メチル−D−グルコシド、ト
リメチロールプロパン、ソルビトール、シュークロース
などが適している。[0063] (wherein, R, R ', R "are each independently -H, -COCH 3, - (CH 2 ) x CH 3 or - (CF 2) y
CF 3 and Me is a methyl group. Further, a and b are 1 to 10 and x and y are 1 to 18) The polyol used in the present invention is a conventionally used polyether except for the purpose of using a fluorinated iodohydrocarbon as a foaming agent. Suitable are polyols and polyester polyols. In addition, a polyol having a large number of hydroxyl groups synthesized from a polyhydric alcohol in its molecule is suitable for obtaining hardness or controlling reactivity. In the polyol molecule, a tertiary amine together with a hydroxyl group,
Catalyst-containing polyols containing phosphorus or halogen, flame-retardant polyols, aromatic polyols are also suitable. Adding water to the polyol to improve foamability is a preferred technique. When water is added together with the blowing agent having a relatively high boiling point in the present invention, a low-density foam can be formed, and bubbles can be made uniform and fine. Similarly, by adding alcohol, due to the heat of reaction when the alcohol reacts with the isocyanate,
Like water, the foamability of the foaming agent can be improved, which is preferable. Suitable alcohols that can be used include methanol, ethanol, ethylene glycol, glycerin, pentaerythritol, α-methyl-D-glucoside, trimethylolpropane, sorbitol and sucrose.
【0064】本発明に用いられるイソシアネートは、ジ
フェニルメタンジイソシアネート系、トリレンジイソシ
アネート系、キシリレンジイソシアネート、メタキシリ
レンジイソシアネート、ヘキサメチレンジイソシアネー
ト、リジンジイソシアネート、イソホロンジイソシアネ
ート、トリメチルヘキサメチレンジイソシアネート、ダ
イマー酸ジイソシアネート等が適している。本発明にお
いて用いられるウレタン反応用触媒は、ゲル化触媒、泡
化触媒、遅延触媒等ウレタン原料の反応性によって最も
効果的な触媒を選ぶ必要がある。一般に用いられる触媒
は、三級アミン、有機金属化合物であるが、アミン系触
媒には、モノアミン類、ジアミン類、トリアミン類、環
状アミン類、アルコールアミン類、エーテルアミン類な
どがある。有機金属化合物では、有機すず化合物が最も
よく用いられる。本発明においては、発泡剤の沸点が室
温から70℃であるので、一般的処方用の触媒が利用さ
れる。しかし、極端に共沸点が低い場合や高い場合に
は、使い分けたり、各種の触媒を混合することが必要で
ある。また、水もイソシアネートと反応して尿素結合を
形成し、ウレタンの物性に大きく寄与するので、架橋密
度向上のために添加することもよい。As the isocyanate used in the present invention, diphenylmethane diisocyanate type, tolylene diisocyanate type, xylylene diisocyanate, metaxylylene diisocyanate, hexamethylene diisocyanate, lysine diisocyanate, isophorone diisocyanate, trimethylhexamethylene diisocyanate, dimer acid diisocyanate and the like are suitable. ing. As the urethane reaction catalyst used in the present invention, it is necessary to select a most effective catalyst such as a gelling catalyst, a foaming catalyst, and a delay catalyst depending on the reactivity of the urethane raw material. Commonly used catalysts are tertiary amines and organometallic compounds, and amine-based catalysts include monoamines, diamines, triamines, cyclic amines, alcohol amines and ether amines. Of the organometallic compounds, organotin compounds are most often used. In the present invention, since the boiling point of the blowing agent is from room temperature to 70 ° C., a general formulation catalyst is used. However, when the azeotropic point is extremely low or high, it is necessary to use properly or mix various catalysts. Further, water also reacts with isocyanate to form a urea bond, which greatly contributes to the physical properties of urethane, and therefore may be added to improve the crosslink density.
【0065】本発明で用いられる難燃剤には、ホスフェ
ート、臭素ーリン化合物、有機臭素化合物等がある。特
に、トリス(β−クロルエチル)ホスフェート、トリク
レジルホスフェート、トリキシレニルホスフェートなど
のリン系の難燃剤は、燃焼時に発生する有毒ガスも少な
く本発明に適している。また、加水分解防止剤、酸化防
止剤などの添加剤を加えることによって、長期の物性安
定効果が得られる。本発明の発泡剤は、沸点が40〜7
0℃程度であるので、従来のポリオール組成物に単独発
泡剤として混合し、適度な性能を有する発泡フォームを
得ることが容易であり、従来例であるシクロペンタン発
泡フォームよりも10〜40%熱伝導率が低い発泡体が
得られる。The flame retardants used in the present invention include phosphates, bromine-phosphorus compounds, organic bromine compounds and the like. In particular, phosphorus-based flame retardants such as tris (β-chloroethyl) phosphate, tricresyl phosphate, and trixylenyl phosphate are suitable for the present invention because they produce little toxic gas during combustion. Further, by adding additives such as a hydrolysis inhibitor and an antioxidant, a long-term physical property stabilizing effect can be obtained. The foaming agent of the present invention has a boiling point of 40 to 7
Since it is about 0 ° C., it is easy to obtain a foamed foam having a proper performance by mixing it with a conventional polyol composition as a sole foaming agent, and to heat the foamed foam by 10 to 40% as compared with the conventional cyclopentane foamed foam. A foam with low conductivity is obtained.
【0066】以下、具体的に実施例に適用して説明す
る。 [実施例1]表1に示すように各種処方の原料を用いて
ポリウレタンフォームを作製し、その熱伝導率、他の物
性を測定し。ここで、原料中のポリオールAは、アミン
系ポリエーテルポリオール組成物で水酸基価449mg
KOH/gのもの、ポリオールBは、ソルビトール系ポ
リエーテルポリオールで水酸基価420mgKOH/g
のものである。また、整泡剤Aは、シリコン系界面活性
剤(武田薬品の商品名TY19)、整泡剤Bは、フッ素
化シリコン系界面活性剤(信越化学の商品名X−70−
090)である。触媒Aは、N,N,N’,N’−テト
ラメチルヘキサメチレンジアミンを主とする触媒(花王
のカオライザーNo.1)、触媒Bはイミダゾール系複
合触媒(花王のカオライザーNo.300)である。発
泡剤Aは、ヘプタフルオロ−2−アイオドプロパン、発
泡剤Bは、ヘプタフルオロ−2−アイオドプロパンとシ
クロペンタンをモル比1対2で混合したもの、発泡剤C
は、シクロペンタンである。イソシアネートは、表1中
にMDIとして示したが、イソシアネート基をグラム当
たり31.4wt%含む組成物(武田薬品の商品名ルプ
ラネートM−20S)である。添加剤Aは、プロピレン
カーボネートである。Hereinafter, the present invention will be specifically described with reference to the embodiments. [Example 1] As shown in Table 1, polyurethane foams were prepared by using raw materials of various formulations, and their thermal conductivity and other physical properties were measured. Here, the polyol A in the raw material is an amine-based polyether polyol composition having a hydroxyl value of 449 mg.
KOH / g, Polyol B is a sorbitol-based polyether polyol with a hydroxyl value of 420 mg KOH / g
belongs to. Further, the foam stabilizer A is a silicon-based surfactant (trade name TY19 of Takeda Pharmaceutical Co., Ltd.), and the foam stabilizer B is a fluorinated silicon-based surfactant (trade name X-70- of Shin-Etsu Chemical).
090). The catalyst A is a catalyst mainly containing N, N, N ′, N′-tetramethylhexamethylenediamine (Kao's Kaolizer No. 1), and the catalyst B is an imidazole-based composite catalyst (Kao's Kaolizer No. 300). . The foaming agent A is heptafluoro-2-iodopropane, the foaming agent B is a mixture of heptafluoro-2-iodopropane and cyclopentane in a molar ratio of 1: 2, and the foaming agent C.
Is cyclopentane. The isocyanate, which is shown as MDI in Table 1, is a composition containing 31.4 wt% of isocyanate groups per gram (Takeda's trade name Luplanate M-20S). Additive A is propylene carbonate.
【0067】発泡体は次のようにして作製した。まず、
試料No.1ー5以外は、ポリオールに整泡剤、触媒、
水および発泡剤を混合したプレミックスを作成した。そ
して、調合したポリオールプレミックス成分とイソシア
ネート成分を所定の配合割合で混合し、高圧発泡機によ
って混合攪拌し、図1のような外箱1と内箱3とによっ
て構成された空間部に充填して発泡させ、ポリウレタン
フォーム2を得た。なお、試料No.1ー5について
は、発泡剤と整泡剤はイソシアネートに混合した。The foam was prepared as follows. First,
Sample No. Except for 1-5, a foam stabilizer, a catalyst,
A premix was prepared by mixing water and a foaming agent. Then, the prepared polyol premix component and isocyanate component are mixed at a predetermined mixing ratio, mixed and stirred by a high-pressure foaming machine, and filled in a space portion constituted by an outer box 1 and an inner box 3 as shown in FIG. And foamed to obtain polyurethane foam 2. Sample No. For 1-5, the foaming agent and foam stabilizer were mixed with the isocyanate.
【0068】なお、比較例としてシクロペンタンを発泡
剤とするフォームの例(試料No.1ー6)を表中に記
載した。各試料の処方の目的を以下に示す。試料No.
1ー1は、発泡剤フッ素化ヨウ化炭化水素と水発泡を併
用した例である。試料No.1ー2は、非アミン系ポリ
オールであるソルビトール系ポリエーテルポリオールを
用い、さらにカーボネート化合物を添加して発泡性を向
上する目的の処方である。試料No.1ー3は、発泡剤
として、フッ素化ヨウ化炭化水素とシクロペンタンの混
合物を使用し、難燃化を目的とした処方である。試料N
o.1ー4は、発泡剤としてフッ素化ヨウ化炭化水素を
用いた他は、シクロペンタンを発泡剤とする比較例と同
じ組成としたものである。試料No.1ー5は、非アミ
ン系ポリオールおよび整泡剤を用いた処方である。比較
例の試料No.1ー6は、水を添加していない最適な配
合としている。これに対して、本発明の実施例の試料N
o.1ー1〜1ー3、1ー5では、水の添加によるイソ
シアネートと水との反応を考慮して、イソシアネートの
量を試料No.1ー6よりも多くし、また、触媒につい
ても水の添加を考慮した触媒Bが使用されている。As a comparative example, an example of foam using cyclopentane as a foaming agent (Sample No. 1-6) is shown in the table. The purpose of formulation of each sample is shown below. Sample No.
No. 1-1 is an example in which a foaming agent fluorinated iodohydrocarbon and water foaming are used in combination. Sample No. Nos. 1 and 2 are formulations for the purpose of improving foamability by using a sorbitol-based polyether polyol which is a non-amine-based polyol and further adding a carbonate compound. Sample No. Nos. 1 to 3 are formulations using a mixture of fluorinated iodohydrocarbon and cyclopentane as a foaming agent and aiming at flame retardancy. Sample N
o. Nos. 1 to 4 had the same composition as that of the comparative example using cyclopentane as the foaming agent except that fluorinated iodohydrocarbon was used as the foaming agent. Sample No. 1-5 is a formulation using a non-amine-based polyol and a foam stabilizer. Sample No. of the comparative example. Nos. 1 to 6 are optimum blends with no water added. On the other hand, the sample N of the embodiment of the present invention
o. In Nos. 1-1 to 1-3 and 1-5, the amount of isocyanate was adjusted to be the same as that of Sample No. 1 in consideration of the reaction between isocyanate and water due to the addition of water. The catalyst B is used in an amount larger than 1-6 and considering the addition of water.
【0069】なお、以下の各表1〜5において、各試料
の原料の配合量は重量部で表している。また、フォーム
の諸物性の単位は次の通りである。 フォーム密度の単位:kg/m3 熱伝導率:シクロペンタンフォーム(試料No.1ー
6)を1としたときの比 気泡径の単位:μm 圧縮強度の単位:kg重/cm2 In each of the following Tables 1 to 5, the blending amount of the raw material of each sample is expressed in parts by weight. The unit of physical properties of the foam is as follows. Unit of foam density: kg / m 3 Thermal conductivity: Ratio when cyclopentane foam (Sample No. 1-6) is set to 1 Unit of cell diameter: μm Unit of compressive strength: kg weight / cm 2
【0070】[0070]
【表1】 [Table 1]
【0071】表1に示されるように、ヘプタフルオロ−
2−アイオドプロパンを発泡剤に用いたフォーム(試料
No.1ー4)は、従来例であるシクロペンタンを発泡
剤としたフォームと比較して、同じ原料処方で、約10
%程度低い熱伝導率を示した。しかし、フォーム密度が
高く、気泡径も大きかった。一方、水を添加した処方の
試料No.1ー1によるものは、熱伝導率が低く、密
度、気泡形状などの物性が改善された。さらに熱伝導率
の低いフォームを形成するため、ポリオールの70%を
ソルビトール系ポリエーテルポリオールとしたものを使
用する(試料No.1ー2)と、フォームはさらに低い
熱伝導率を示した。これは、試料No.1ー1よりも発
泡性が向上し、フォームの密度が低減されたことによ
る。また、気泡径が均一、かつ微細化した。これは、添
加剤として使用したプロピレンカーボネートの影響と思
われる。このようにフォームの熱伝導率が、シクロペン
タンを発泡剤とする比較例のフォームと比べて約30%
以上低くすることができた。ポリオールの改善や添加剤
によって断熱性能が大幅に向上した。As shown in Table 1, heptafluoro-
The foam using 2-iodopropane as the foaming agent (Sample No. 1-4) has about 10% of the same raw material formulation as the conventional foam using cyclopentane as the foaming agent.
It showed a low thermal conductivity of about%. However, the foam density was high and the cell diameter was also large. On the other hand, the sample No. of the prescription with water added. The sample No. 1-1 had a low thermal conductivity, and the physical properties such as density and bubble shape were improved. In order to form a foam having a lower thermal conductivity, when a sorbitol-based polyether polyol was used in 70% of the polyol (Sample No. 1-2), the foam exhibited a lower thermal conductivity. This is sample No. This is because the foamability was improved and the foam density was reduced as compared with 1-1. In addition, the bubble diameter was uniform and miniaturized. This is likely due to the propylene carbonate used as an additive. Thus, the thermal conductivity of the foam is about 30% as compared with the foam of the comparative example using cyclopentane as the blowing agent.
I was able to lower it. The improvement of the polyol and additives have significantly improved the heat insulation performance.
【0072】次に、シクロペンタンとの混合物を発泡剤
に用いた試料No.1ー3のフォームは、ほぼ試料N
o.1ー2に準じた性能を有し、シクロペンタン単独を
発泡剤とした比較例よりも低い熱伝導率が得られた。フ
ォームの燃焼性を評価するために、フォームを1×1×
5cmに切り出したサンプルに着火したところ、比較例
の試料No.1ー6は完全に燃えたが、試料No.1ー
3では、着火してすぐに消火した。ヘプタフルオロ−2
−アイオドプロパンを発泡剤とした試料No.1ー2で
は、同じく消火するため、フッ素化ヨウ化炭化水素が可
燃性のシクロペンタンに混合されて、難燃性および自己
消火の機能を示すことがわかった。さらに、発泡剤と他
の組成物との相溶性を改質するために、整泡剤を変えて
フォームを形成した。フッ素系界面活性剤だけを添加し
た処方では、発泡途中に気泡がつぶれてしまい、気泡が
大きくなることによって熱伝導率が高くなった。しか
し、このフッ素系界面活性剤と従来用いられているシリ
コン系界面活性剤を重量比1対2の割合で混合したもの
を用いた他は試料No.1ー1と同じ処方とすると、プ
レミックスの相溶性が改善され、発泡性が高まると同時
に気泡が安定化されるため、270ミクロンの微細な気
泡を有したフォームを得ることができた。このフォーム
の熱伝導率は0.73であった。Next, in the case of Sample No. 1 in which a mixture with cyclopentane was used as a foaming agent. Foams 1-3 are almost sample N
o. The performance was similar to that of 1-2, and the thermal conductivity was lower than that of the comparative example using cyclopentane alone as the foaming agent. To evaluate the flammability of the foam, use the foam 1 × 1 ×
When the sample cut to 5 cm was ignited, the sample No. Sample Nos. 1-6 burned completely, but sample No. In 1-3, the fire was extinguished immediately after it ignited. Heptafluoro-2
-Sample No. using iodopropane as a foaming agent. In Nos. 1 and 2, fluorinated iodohydrocarbons were also mixed with flammable cyclopentane for extinguishing fire, and it was found that they exhibited flame retardancy and self-extinguishing functions. Further, the foam stabilizer was changed to form a foam in order to modify the compatibility of the foaming agent with other compositions. In the formulation in which only the fluorine-based surfactant was added, the bubbles were crushed during foaming, and the bubbles became large, resulting in high thermal conductivity. However, sample No. 1 was used except that this fluorine-based surfactant and a conventionally used silicon-based surfactant were mixed at a weight ratio of 1: 2. When the same formulation as 1-1 was used, the compatibility of the premix was improved, the foamability was enhanced, and the cells were stabilized at the same time, so that a foam having fine cells of 270 microns could be obtained. The thermal conductivity of this foam was 0.73.
【0073】試料No.1ー5では、前記の混合物整泡
剤を使い、これと発泡剤とをイソシアネートに混合した
イソシアネートプレミックスとした。このイソシアネー
トプレミックスをポリオール組成物と混合し発泡させ
た。この処方によると、得られるフォームの熱伝導率
は、シクロペンタンを発泡剤とする比較例より約40%
低くなり、断熱材として最適な物性を示すウレタンフォ
ームを得ることができた。また、この整泡剤と添加剤A
を組み合わせて添加することにより、熱伝導率が0.6
程度まで低下したが、フォーム強度は0.95kg/m
3で若干強度が低くなった。次に、試料No.1ー5の
処方のイソシアネートプレミックス中に、マグネタイト
粉体5部を分散した場合、得られたフォームの熱伝導率
は、比較例の0.66であり、マグネタイト添加によっ
てほとんどフォーム熱伝導率は変わりがなかった。ま
た、3ケ月経過後のフォーム熱伝導率は、0.67と断
熱性の劣化はほとんど認められかった。一方、酸素吸収
剤のマグネタイトを添加しなかった場合は、3ケ月経過
後には熱伝導率が0.75とかなり断熱性が低下した。
従って、酸素吸収剤を添加すると、長期的にも、良好な
断熱性能を示すことがわかった。Sample No. In Nos. 1-5, the mixture foam stabilizer was used, and an isocyanate premix was prepared by mixing the foam stabilizer with an isocyanate. This isocyanate premix was mixed with the polyol composition and foamed. According to this formulation, the thermal conductivity of the resulting foam is about 40% compared to the comparative example using cyclopentane as the blowing agent.
It was possible to obtain a urethane foam having a low property and exhibiting the optimum physical properties as a heat insulating material. In addition, this foam stabilizer and additive A
When added in combination, the thermal conductivity of 0.6
Foam strength is 0.95 kg / m
At 3 , the strength became slightly lower. Next, sample No. When 5 parts of magnetite powder was dispersed in the isocyanate premix having the formulation of 1-5, the thermal conductivity of the obtained foam was 0.66 of the comparative example, and almost no foam thermal conductivity was obtained by adding magnetite. It didn't change. In addition, the foam thermal conductivity after the lapse of 3 months was 0.67, and almost no deterioration of the heat insulating property was recognized. On the other hand, when magnetite, which is an oxygen absorber, was not added, the thermal conductivity was 0.75, which was a considerable decrease in thermal insulation after 3 months.
Therefore, it was found that the addition of the oxygen absorbent shows good heat insulating performance even in the long term.
【0074】[実施例2]実施例1に準じて、発泡体を
作製し、その特性を評価した。表2に原材料の処方およ
び得られたフォームの特性を示す。発泡剤Dはヘキサフ
ルオロプロペンダイマー、発泡剤Eは、ヘプタフルオロ
ー2ーアイオドプロパンとヘキサフルオロプロペンダイ
マーのモル比1対1の混合物、発泡剤Fは、ヘプタフル
オロー2ーアイオドプロパンとヘキサフルオロプロペン
ダイマーとシクロペンタンのモル比1対1対2の混合物
である。他の材料については、表1と同じ物質を示す。Example 2 A foam was prepared according to Example 1 and its characteristics were evaluated. Table 2 shows the raw material formulation and the properties of the resulting foam. The foaming agent D is hexafluoropropene dimer, the foaming agent E is a mixture of heptafluoro-2-iodopropane and hexafluoropropene dimer in a molar ratio of 1: 1, and the foaming agent F is heptafluoro-2-iodopropane and hexafluoropropene dimer. And cyclopentane in a molar ratio of 1: 1: 2. For other materials, the same substances as in Table 1 are shown.
【0075】各試料の処方目的を以下に示す。試料N
o.2ー1は、発泡剤パーフルオロアルケンと水発泡を
併用する処方である。試料No.2ー2は、パーフルオ
ロアルケンとフッ素化ヨウ化炭化水素の混合物を発泡剤
とする処方である。試料No.2ー3は、パーフルオロ
アルケンとフッ素化ヨウ化炭化水素とシクロペンタンの
三元発泡剤の処方である。試料No.2ー4は、発泡剤
にパーフルオロアルケンを使用した他は比較例と同じ処
方である。試料No.2ー5は、混合物整泡剤と水発泡
の併用効果を目的とした処方である。試料No.1ー6
は、実施例1に用いた比較例である。The purpose of prescribing each sample is shown below. Sample N
o. No. 2-1 is a formulation in which a blowing agent perfluoroalkene and water foaming are used in combination. Sample No. No. 2-2 is a formulation using a mixture of perfluoroalkene and fluorinated iodohydrocarbon as a foaming agent. Sample No. 2-3 is a ternary foaming agent formulation of perfluoroalkene, fluorinated iodohydrocarbon and cyclopentane. Sample No. Nos. 2-4 have the same formulation as the comparative example except that perfluoroalkene was used as the blowing agent. Sample No. No. 2-5 is a formulation intended for the combined effect of the mixture foam stabilizer and water foaming. Sample No. 1-6
Is a comparative example used in Example 1.
【0076】[0076]
【表2】 [Table 2]
【0077】ヘキサフルオロプロペンダイマーを発泡剤
とした試料No.2ー4によるフォームは、プレミック
スがエマルジョン状態であり、3〜4時間で分離する不
安定な組成物であるため、発泡密度が高く気泡も不均一
であった。試料No.2ー1では、水の添加量を3部と
し、ヘプタフルオロプロペンダイマーの量を少なくして
いる。この処方によると、発泡性を少なからず向上させ
ることができた。しかし、ガス中に50%近く炭酸ガス
が含まれる。このために、熱伝導率は大きくなり、比較
例よりわずかに低い程度であった。一方、試料No.2
ー3によるフォームは、熱伝導率が比較例(シクロペン
タンを発泡剤とする)より37%程度低い値を示した。
これは、ヘプタフルオロー2ーアイオドプロパンとシク
ロペンタンが、プレミックスのエマルジョンの粘度をか
なり低くする作用があること、およびエマルジョンが気
泡核となっていることにより、気泡が均一かつ微細化し
たためである。また、試料No.2ー3の発泡剤は、共
沸に近い挙動を示してかなり沸点が低くなり、低沸点化
合物を使って発泡した際と類似の良好な発泡性を示した
ものと考えられる。また、フォームの燃焼性を評価した
ところ、可燃性のシクロペンタンが混合されているにも
関わらず、試料No.2ー1、2、4のヘプタフルオロ
プロペンダイマーおよび二酸化炭素の混合発泡剤の場合
と同じ燃焼性を示し、シクロペンタンを用いた試料N
o.1ー6よりはるかに難燃性であった。Sample No. using hexafluoropropene dimer as a foaming agent The foam according to No. 2-4 was an unstable composition in which the premix was in an emulsion state and separated in 3 to 4 hours, so that the foam density was high and the bubbles were non-uniform. Sample No. In No. 2-1, the amount of water added is 3 parts and the amount of heptafluoropropene dimer is reduced. According to this formulation, the foamability could be improved to some extent. However, the gas contains nearly 50% carbon dioxide gas. For this reason, the thermal conductivity was high and was slightly lower than that of the comparative example. On the other hand, sample No. Two
The foam of No. 3 had a thermal conductivity of about 37% lower than that of the comparative example (using cyclopentane as the foaming agent).
This is because heptafluoro-2-iodopropane and cyclopentane have a function of considerably lowering the viscosity of the emulsion of the premix, and the emulsion is a cell nucleus, so that the bubbles are uniform and fine. . In addition, the sample No. It is considered that the 2-3 foaming agents exhibit a behavior close to that of azeotrope and have a considerably low boiling point, and exhibit a good foaming property similar to that when foaming using a low boiling point compound. In addition, when the flammability of the foam was evaluated, it was found that sample No. Sample N using cyclopentane showing the same flammability as the mixed blowing agent of 2-1, 2,4 heptafluoropropene dimer and carbon dioxide
o. It was far more flame retardant than 1-6.
【0078】整泡剤を変えて、フッ素化シリコン界面活
性剤(整泡剤B)を用いた場合は、フォームの反応成長
中に泡がつぶれていく現象が起き、フォームを形成する
ことができなかった。しかし、試料No.2ー5で、フ
ッ素化シリコン界面活性剤とシリコン系界面活性剤(整
泡剤A)とを混合した整泡剤を使ったところ、プレミッ
クスのエマルジョンの安定性が向上し、1週間以上相分
離を起こすことなく、エマルジョン形態を保持してい
た。また、得られたフォームは、微細な気泡を有し、熱
伝導率は比較例の約30%程度低い値であった。試料N
o.2ー5では、発泡剤はヘキサフルオロプロペンダイ
マ−単独であるが、混合整泡剤を同時に使用することに
よって、水の量を減らしてフォームを得ることができ
る。その場合は、炭酸ガスが減るため、熱伝導率はさら
に約5%程度低くすることが可能であった。試料No.
2ー4の処方にプロピレンカーボネートを添加したとこ
ろ、得られたフォームは、密度が約41kg/m3とな
り、熱伝導率も15%程度低くなり、添加剤の効果があ
った。同様に、ヘプタフルオロプロペンダイマーの異性
体を単離し、それぞれを発泡剤としてフォームを作り評
価したところ、ほぼ同じ断熱性能のフォームが得られ
た。When a fluorinated silicone surfactant (foam stabilizer B) is used in place of the foam stabilizer, a phenomenon occurs in which the foam collapses during the reaction growth of the foam, and the foam can be formed. There wasn't. However, the sample No. In 2-5, when a foam stabilizer prepared by mixing a fluorinated silicone surfactant and a silicon-based surfactant (foam stabilizer A) was used, the stability of the premix emulsion was improved and the phase was maintained for 1 week or longer. The emulsion morphology was retained without separation. Further, the obtained foam had fine cells, and the thermal conductivity thereof was about 30% lower than that of the comparative example. Sample N
o. In 2-5, the foaming agent is hexafluoropropene dimer alone, but the amount of water can be reduced to obtain the foam by using the mixed foam stabilizer at the same time. In that case, since the carbon dioxide gas decreased, the thermal conductivity could be further reduced by about 5%. Sample No.
When propylene carbonate was added to the formulation No. 2-4, the resulting foam had a density of about 41 kg / m 3 and a thermal conductivity of about 15% lower, which was effective as an additive. Similarly, when isomers of heptafluoropropene dimer were isolated and foams were made by using each as a foaming agent and evaluated, foams having almost the same heat insulation performance were obtained.
【0079】[実施例3]水素含有フッ化モルフォリン
誘導体を発泡剤に用いた例を示す。発泡体の作製は、実
施例1と同様である。表3に各試料の処方および得られ
たフォームの特性をまとめた。発泡剤Gは、3H−オク
タフルオロモルフォリンであり、発泡剤Hは3H−ヘプ
タフルオロ−4−トリフルオロメチルモルフォリン、発
泡剤Iは、3Hーヘプタフルオロ−4−トリフルオロメ
チルモルフォリンとシクロペンタンのモル比1対1の混
合物であり、発泡剤Jは、3H−ヘプタフルオロ−4−
トリフルオロメチルモルフォリンとイソペンタンのモル
比1対1の混合物である。添加剤Bは、ネオペンチルジ
グリシジルエーテルである。整泡剤Cは、整泡剤AとB
の重量比3対1の混合物である。その他の材料は、表1
と同じ物質を示す。[Example 3] An example in which a hydrogen-containing fluorinated morpholine derivative is used as a foaming agent is shown. The production of the foam is the same as in Example 1. Table 3 summarizes the formulation of each sample and the properties of the resulting foam. The blowing agent G is 3H-octafluoromorpholine, the blowing agent H is 3H-heptafluoro-4-trifluoromethylmorpholine, and the blowing agent I is 3H-heptafluoro-4-trifluoromethylmorpholine and cyclopentane. It is a mixture with a molar ratio of 1: 1 and the blowing agent J is 3H-heptafluoro-4-.
It is a mixture of trifluoromethylmorpholine and isopentane in a molar ratio of 1: 1. Additive B is neopentyl diglycidyl ether. The foam stabilizer C is the foam stabilizers A and B.
Is a mixture with a weight ratio of 3: 1. Other materials are listed in Table 1.
Indicates the same substance as.
【0080】表中の各処方の目的について説明する。試
料No.3ー1およびNo.3ー2は、発泡剤水素含有
フッ化モルフォリン誘導体と水発泡を併用した処方で、
それぞれ異なる水素含有フッ化モルフォリン誘導体を用
いたものである。試料No.3ー3は、水素含有フッ化
モルフォリン誘導体とシクロペンタンの混合物を発泡剤
とする処方である。試料No.3ー4は、水素含有フッ
化モルフォリン誘導体とイソペンタンの混合物を発泡剤
とする処方である。試料No.3ー5は、添加剤とし
て、エポキシドを混合し、水を用いずに発泡する処方で
ある。試料No.1ー6は、実施例1で用いた比較例で
ある。The purpose of each prescription in the table will be described. Sample No. 3-1 and No. 3-2 is a formulation in which a foaming agent hydrogen-containing fluorinated morpholine derivative and water foaming are used in combination.
Each of the different hydrogen-containing fluorinated morpholine derivatives is used. Sample No. No. 3-3 is a formulation using a mixture of a hydrogen-containing fluorinated morpholine derivative and cyclopentane as a foaming agent. Sample No. No. 3-4 is a formulation using a mixture of hydrogen-containing fluorinated morpholine derivative and isopentane as a foaming agent. Sample No. No. 3-5 is a formulation in which an epoxide is mixed as an additive and foaming is performed without using water. Sample No. Nos. 1 to 6 are comparative examples used in Example 1.
【0081】[0081]
【表3】 [Table 3]
【0082】発泡剤が3H−オクタフルオロモルフォリ
ン単独で、水発泡を併用した試料No.3ー1によるフ
ォーム、および3H−オクタフルオロモルフォリンの代
わりに3H−ヘプタフルオロ−4−トリフルオロメチル
モルフォリンを用いた試料No.3ー2の処方によるフ
ォームは、水を添加しない場合より熱伝導率は低くなっ
た。しかし、フォーム密度が比較的高く、気泡径も大き
かった。なお、ポリオールと発泡剤との相溶性は比較的
良好で、比較例(試料No.1ー6)の場合と同じよう
な粘度の低いプレミックスエマルジョンが得られた。フ
ォームの熱伝導率は、比較例より10%以上低くなった
が、フォーム密度が高かった。従って、さらに性能を向
上するにはフォームの改質を行う必要がある。Sample No. 3 in which the foaming agent was 3H-octafluoromorpholine alone and water foaming was also used. Sample No. 3 using foam according to 3-1 and 3H-heptafluoro-4-trifluoromethylmorpholine in place of 3H-octafluoromorpholine. The foam according to the formulation of 3-2 had lower thermal conductivity than that in the case where water was not added. However, the foam density was relatively high and the cell diameter was also large. The compatibility between the polyol and the foaming agent was relatively good, and a premix emulsion having a low viscosity similar to that of the comparative example (Sample No. 1-6) was obtained. The thermal conductivity of the foam was 10% or more lower than that of the comparative example, but the foam density was high. Therefore, it is necessary to modify the foam to further improve the performance.
【0083】発泡剤Hは、沸点が少し高いために発泡性
が悪く、得られるフォームの密度が高くなる。そこで、
発泡剤Hに、沸点の低い物質のシクロペンタンおよびイ
ソペンタンをそれぞれ混合した試料No.3ー3および
No.3ー4の処方に従って発泡させたところ、発泡性
が向上することにより、得られたフォームの密度は低く
なり、それにともなって、熱伝導率も低くなった。試料
No.3ー3において、熱伝導率の低いフォームが得ら
れ、その値は、比較例より30%近く低減することがで
きた。しかし、混合する発泡剤シクロペンタンの熱伝導
率が、モルフォリン誘導体よりも高いため、フォームの
熱伝導率は、高い熱伝導率を有する発泡剤シクロペンタ
ンに引きずられて高くなる。そこで、試料No.3ー3
の処方において、シクロペンタンの代わりにヘプタフル
オロー1ーアイオドプロパンを用いたところ、その混合
効果によって、得られたフォームの熱伝導率は非常に低
くなり、比較例より30%以上も低くなった。Since the foaming agent H has a slightly high boiling point, it has a poor foaming property and the density of the obtained foam is high. Therefore,
Sample No. 1 in which cyclopentane and isopentane having low boiling points were mixed in the foaming agent H, respectively. 3-3 and No. When foamed according to the formulation of No. 3-4, the density of the obtained foam was lowered due to the improvement of the foamability, and the thermal conductivity was also reduced accordingly. Sample No. In 3-3, a foam having low thermal conductivity was obtained, and the value could be reduced by nearly 30% as compared with the comparative example. However, since the thermal conductivity of the blowing agent cyclopentane to be mixed is higher than that of the morpholine derivative, the thermal conductivity of the foam is increased by being dragged by the blowing agent cyclopentane having a high thermal conductivity. Therefore, the sample No. 3-3
In the above formulation, when heptafluoro-1-iodopropane was used instead of cyclopentane, the thermal conductivity of the obtained foam was very low due to the mixing effect, and was 30% or more lower than that of the comparative example.
【0084】次に、エポキシドを添加し、モルフォリン
誘導体のみを発泡剤として使用することによって、熱伝
導率のより低いフォームを得る目的の処方による試料N
o.3ー5で発泡体を得た。発泡剤は、3H−オクタフ
ルオロモルフォリンを使って、添加剤としてネオペンチ
ルジグリシジルエーテルを5部添加してプレミックスを
つくった。このプレミックスをイソシアネ−トと混合す
ると、エポキシドを添加していない場合と比べて、泡化
する時間が速くなっており、発泡性が他の処方にも増し
て良好となった。得られたフォームは、密度が低くな
り、整泡剤の添加によって気泡径も細かく均一になって
いるため、非常に性能のよいウレタンフォームであっ
た。Next, by adding an epoxide and using only a morpholine derivative as a foaming agent, a foam having a lower thermal conductivity was prepared.
o. A foam was obtained in 3-5. As a foaming agent, 3H-octafluoromorpholine was used, and 5 parts of neopentyl diglycidyl ether was added as an additive to prepare a premix. When this premix was mixed with an isocyanate, the foaming time was shorter than that in the case where no epoxide was added, and the foamability was better than in other formulations. The obtained foam had a low density and the cell diameter was made fine and uniform by the addition of the foam stabilizer, so that it was a urethane foam having very good performance.
【0085】[実施例4]次に、それぞれの発泡剤の添
加に加えて、さらに添加物の効果を確認するための例を
示す。各試料の処方および得られたフォームの特性を表
4に示す。発泡剤Kは、ヘプタフルオロー2ーアイオド
プロパンとテトラブチルアンモニウムブロマイドとの錯
化合物(液体状態)である。添加剤Cは、炭酸カリウム
であり、C’はエチレングリコールであり、添加剤Cは
C’に溶解した液体として同時に使用される。また、添
加剤Dは、チオ硫酸ナトリウムであり、添加剤D’は、
それを溶解する水である。Example 4 Next, in addition to the addition of each foaming agent, an example for confirming the effect of the additive will be shown. The formulation of each sample and the properties of the resulting foam are shown in Table 4. The foaming agent K is a complex compound (liquid state) of heptafluoro-2-iodopropane and tetrabutylammonium bromide. Additive C is potassium carbonate, C ′ is ethylene glycol, and additive C is simultaneously used as a liquid dissolved in C ′. Further, the additive D is sodium thiosulfate, and the additive D ′ is
It is water that dissolves it.
【0086】表中の各試料の処方について説明する。試
料No.4ー1は、フッ素化ヨウ化炭化水素とパーフル
オロアルケンの混合物を発泡剤とする処方である。試料
No.4ー2は、エチレングリコールに溶解した炭酸カ
リウムを添加し、気泡の微細化を行う処方である。試料
No.4ー3は、還元剤としてチオ硫酸ナトリウムを水
溶液で添加する処方である。チオ硫酸ナトリウム水溶液
は、原料調製段階でイソシアネートに混合した。試料N
o.4ー4は、フッ素化ヨウ化炭化水素とアミン化合物
の錯化合物を利用して、それを発泡剤の一部として使用
する目的の処方であり、発泡剤液体として添加されるパ
ーフルオロアルケンの量は錯化合物を形成しているフッ
素化ヨウ化炭化水素1モルに対して1モルである。ま
た、反応制御剤としての水を加えた例である。試料N
o.4ー5は、比較のために混合発泡剤に水を添加した
処方である。試料No.1ー6は、実施例1で用いた比
較例である。The formulation of each sample in the table will be described. Sample No. 4-1 is a formulation using a mixture of a fluorinated iodohydrocarbon and a perfluoroalkene as a foaming agent. Sample No. No. 4-2 is a formulation in which potassium carbonate dissolved in ethylene glycol is added to make bubbles fine. Sample No. No. 4-3 is a formulation in which sodium thiosulfate as a reducing agent is added in an aqueous solution. The sodium thiosulfate aqueous solution was mixed with isocyanate at the raw material preparation stage. Sample N
o. 4-4 is a prescription for the purpose of using a complex compound of a fluorinated iodohydrocarbon and an amine compound and using it as a part of a foaming agent. The amount of perfluoroalkene added as a foaming agent liquid. Is 1 mol per 1 mol of the fluorinated iodohydrocarbon forming a complex compound. In addition, it is an example in which water is added as a reaction control agent. Sample N
o. Nos. 4 and 5 are formulations in which water was added to the mixed foaming agent for comparison. Sample No. Nos. 1 to 6 are comparative examples used in Example 1.
【0087】[0087]
【表4】 [Table 4]
【0088】各発泡剤を混合した試料においても、比較
例より20%以上低い伝導率の断熱性発泡体が得られ
た。また、水を添加した試料No.4ー5によるフォー
ムは、気泡径が細かくなることによって、試料No.4
ー1に比べて、密度が低くなるとともに熱伝導率が低く
なった。実施例1、2および3と同様に、さらに、異な
る発泡剤を添加することによって、フォームの熱伝導率
の他、強度等の物性を改善できることが確認された。ま
た、試料No.4ー2のフォームは、添加剤としてエチ
レングリコールに溶解した塩が気泡核になっていると考
えられ、気泡径が非常に小さくなっていた。さらに、チ
オ硫酸ナトリウムの水溶液をイソシアネートに添加する
と、得られるフォームの気泡径はさらに微細化する。Also in the sample in which each foaming agent was mixed, a heat insulating foam having a conductivity lower than that of the comparative example by 20% or more was obtained. In addition, sample No. The foam according to Sample Nos. 4-5 has a small bubble diameter, and thus the sample No. Four
Compared with -1, the density was lower and the thermal conductivity was lower. It was confirmed that, similarly to Examples 1, 2 and 3, by adding different foaming agents, physical properties such as strength as well as thermal conductivity of the foam can be improved. In addition, the sample No. In the foam of No. 4-2, the salt dissolved in ethylene glycol as an additive is considered to be a cell nucleus, and the cell diameter was very small. Furthermore, when an aqueous solution of sodium thiosulfate is added to isocyanate, the foam diameter of the obtained foam is further refined.
【0089】試料No.4ー4では、アミン化合物とフ
ッ素化ヨウ化炭化水素との錯化合物を添加して、錯化合
物中のヘプタフルオロ−2−アイオドプロパンを発泡剤
として考慮し、発泡剤全量を試料No.4ー1と同じ量
にし、さらに水を少量添加したものである。良い発泡密
度を有する熱伝導率の低い硬質ウレタンフォームが形成
された。フォームを日光の当たる場所に放置して熱伝導
率の経時変化を調べたところ、比較例では、1ヶ月経過
してもほとんど熱伝導率は変化しなかった。ヘプタフル
オロ−2−アイオドプロパンを混合した発泡剤を用いて
得たウレタンでは、試料No.4ー1、2、5でかなり
熱伝導率は上昇していた。これは、ヘプタフルオロ−2
−アイオドプロパンの分解が関与しているものと思われ
る。一方、試料No.4ー3では、熱伝導率は変化しな
かった。添加したチオ硫酸ナトリウムがヘプタフルオロ
ー2ーアイオドプロパンの分解を抑えているものと考え
られる。また、フォーム強度を1ヶ月後に測定すると、
試料No.4ー3以外は、少なからず強度低下が見られ
た。Sample No. In No. 4-4, a complex compound of an amine compound and a fluorinated iodohydrocarbon was added to consider heptafluoro-2-iodopropane in the complex compound as a foaming agent, and the total amount of the foaming agent was Sample No. The same amount as 4-1 was added, and a small amount of water was added. A low thermal conductivity rigid urethane foam with good foam density was formed. When the foam was left in a place exposed to sunlight and the change in thermal conductivity with time was examined, in the comparative example, the thermal conductivity hardly changed even after one month. In the urethane obtained by using the foaming agent mixed with heptafluoro-2-iodopropane, Sample No. The thermal conductivity increased considerably in 4-1, 2, and 5. This is heptafluoro-2
-It seems that the decomposition of iodopropane is involved. On the other hand, sample No. In 4-3, the thermal conductivity did not change. It is considered that the added sodium thiosulfate suppresses the decomposition of heptafluoro-2-iodopropane. Also, when measuring the foam strength after one month,
Sample No. Except for 4-3, a considerable decrease in strength was observed.
【0090】試料No.4ー4では、ヘプタフルオロー
2ーアイオドプロパンとテトラブチルアンモニウムブロ
マイドとの錯化合物を添加した。ヘプタフルオロ−2−
アイオドプロパンの総量は、試料No.4ー1に準じ
て、ヘキサフルオロプロペンダイマーとモル比で1対1
とした。その結果、従来と同じポリオール原料を使用し
て発泡性も向上でき、なおかつ気泡も比較的細かなフォ
ームが得られた。Sample No. In 4-4, a complex compound of heptafluoro-2-iodopropane and tetrabutylammonium bromide was added. Heptafluoro-2-
For the total amount of iodopropane, the sample No. According to 4-1, the molar ratio to hexafluoropropene dimer is 1: 1
And As a result, it was possible to obtain a foam in which the foaming property could be improved by using the same polyol raw material as the conventional one and the cells had relatively fine bubbles.
【0091】[実施例5]エポキシドを添加した実施例
を示す。各試料の処方および得られたフォームの特性を
表5に示す。発泡剤Lは、ヘプタフルオロー2ーアイオ
ドプロパンとテトラメチルヘキサメチレンジアミンとの
錯化合物であり、錯化合物中の発泡剤と単独で添加した
発泡剤を合わせた量は、試料No.5ー2および5ー3
と同じである。触媒Cはジブチル錫ジラウレートであ
る。添加剤Eはフェニルグリシジルエーテル、添加剤F
は二酸化炭素固定化触媒臭化テトラブチルアンモニウム
である。その他は、前記の実施例と同じである。Example 5 An example in which an epoxide is added will be shown. The formulation of each sample and the properties of the resulting foam are shown in Table 5. The foaming agent L is a complex compound of heptafluoro-2-iodopropane and tetramethylhexamethylenediamine, and the total amount of the foaming agent in the complex compound and the foaming agent added alone is equal to that of the sample No. 5-2 and 5-3
Is the same as Catalyst C is dibutyltin dilaurate. Additive E is phenyl glycidyl ether, Additive F
Is a carbon dioxide-immobilized catalyst tetrabutylammonium bromide. Others are the same as the above-mentioned embodiment.
【0092】各試料の処方を以下に説明する。試料N
o.5ー1は、フッ素化ヨウ化炭化水素を発泡剤として
使用した通常の処方である。試料No.5ー2は、フッ
素化ヨウ化炭化水素発泡剤に、エポキシドを添加して、
水とイソシアネートとの反応で発生する二酸化炭素を吸
収し、固定化する作用をさせる目的の処方である。試料
No.5ー3は、試料No.5ー2に準じた処方である
が、二酸化炭素固定化触媒を溶解したエポキシドと発泡
剤(フッ素化ヨウ化炭化水素)を混合したポリオールを
調製し、これをイソシアネートと混合する方法で発泡さ
せる例である。試料No.5ー4は、フッ素化ヨウ化炭
化水素を二酸化炭素固定化触媒と混合して生成した錯化
合物をイソシアネートに添加して、高収率の二酸化炭素
固定を期待する処方である。試料No.5ー5は、発泡
剤としてシクロペンタンを使用して、エポキシドを添加
して二酸化炭素を固定化する処方である。試料No.1
ー6は、実施例1で用いた比較例である。The formulation of each sample is described below. Sample N
o. No. 5-1 is a normal formulation using fluorinated iodohydrocarbon as a foaming agent. Sample No. 5-2 is the addition of epoxide to the fluorinated iodohydrocarbon blowing agent,
It is a formulation for the purpose of absorbing and fixing carbon dioxide generated by the reaction between water and isocyanate. Sample No. 5-3 is sample No. An example in which a polyol prepared by mixing an epoxide in which a carbon dioxide-immobilized catalyst is dissolved and a foaming agent (fluorinated iodohydrocarbon) is prepared according to 5-2, and is mixed with an isocyanate to foam. Is. Sample No. No. 5-4 is a formulation in which a complex compound produced by mixing fluorinated iodohydrocarbon with a carbon dioxide-immobilized catalyst is added to isocyanate to expect high yield of carbon dioxide immobilization. Sample No. No. 5-5 is a formulation in which cyclopentane is used as a foaming agent and epoxide is added to fix carbon dioxide. Sample No. 1
-6 is a comparative example used in Example 1.
【0093】[0093]
【表5】 [Table 5]
【0094】試料No.5ー5は、比較例の処方に水1
部を添加したものであり、添加剤EおよびFを添加する
ことにより、発泡樹脂中の二酸化炭素が吸収され、熱伝
導率を10%以上低下することができた。この熱伝導率
は、7日経過すると、さらに約20%も低下した。フォ
ーム中の二酸化炭素をガスクロマトグラフィーで分析す
ると、初期に発生していた二酸化炭素量はほとんどなく
なっていた。発泡剤にヘプタフルオロー2ーアイオドプ
ロパンと水の混合物を用い、添加剤EおよびFを加えた
試料No.5ー2によるフォームは、発泡剤の熱伝導率
が低いため、試料No.5ー1と同様に、比較例より低
いフォーム熱伝導率である。さらに、試料No.5ー2
では、二酸化炭素が吸収された結果、1週間後には比較
例より33%も熱伝導率が低下した。試料No.5ー3
でも、ほぼ同様であった。試料No.5ー2および5ー
3のフォームを赤外吸収スペクトルで分析すると、エポ
キシドはほぼ100%が二酸化炭素と反応したカーボネ
ート化合物となっており、高い収率で二酸化炭素が固定
化されたものと考えられる。Sample No. 5-5 is water 1 in the formulation of the comparative example
By adding the additives E and F, carbon dioxide in the foamed resin was absorbed and the thermal conductivity could be reduced by 10% or more. This thermal conductivity further decreased by about 20% after 7 days. When the carbon dioxide in the foam was analyzed by gas chromatography, the amount of carbon dioxide initially generated was almost gone. A mixture of heptafluoro-2-iodopropane and water was used as a foaming agent, and the additives E and F were added thereto. The foam according to Sample No. 5-2 has a low thermal conductivity of the foaming agent. Similar to 5-1, it has a lower foam thermal conductivity than the comparative example. Further, the sample No. 5-2
Then, as a result of the absorption of carbon dioxide, the thermal conductivity decreased by 33% from the comparative example one week later. Sample No. 5-3
But it was almost the same. Sample No. When the 5-2 and 5-3 foams were analyzed by infrared absorption spectrum, almost 100% of the epoxide was a carbonate compound reacted with carbon dioxide, and it is considered that carbon dioxide was immobilized at a high yield. To be
【0095】試料No.5ー4では、ヘプタフルオロー
2ーアイオドプロパンとテトラメチルヘキサメチレンジ
アミンとの錯化合物を添加して得たフォームである。こ
の場合は、二酸化炭素の固定化速度が速く、製造1日後
には、ガス分析によると、二酸化炭素は90%以上が固
定化されていることがわかった。フォームの密度が低く
改善されていることから、前記錯化合物がウレタン反応
用触媒として作用しているものと考えられる。また、錯
化合物が、遊離のヨウ素を生成して、固定化触媒として
作用している効果も考えられる。試料No.5ー3およ
び5ー4は、1カ月経過後においても、さらに時間を経
て熱伝導率が低下した。なお、本発明による断熱性樹脂
発泡体を用いた例として、冷蔵庫用箱体を図1に示す。
金属製の外箱1と硬質樹脂製内箱3を組み合せて構成し
ている。硬質樹脂製内箱3は、成型性のため熱可塑性樹
脂である。この熱可塑性樹脂は、本発明の発泡ポリウレ
タン断熱体2により侵されないことが望ましく、ABS
樹脂等が適している。Sample No. No. 5-4 is a foam obtained by adding a complex compound of heptafluoro-2-iodopropane and tetramethylhexamethylenediamine. In this case, the immobilization rate of carbon dioxide was high, and it was found that 90% or more of carbon dioxide was immobilized by gas analysis one day after the production. Since the foam has a low density and is improved, it is considered that the complex compound acts as a urethane reaction catalyst. In addition, it can be considered that the complex compound produces free iodine and acts as an immobilized catalyst. Sample No. In 5-3 and 5-4, the thermal conductivity decreased further after a lapse of one month. As an example of using the heat insulating resin foam according to the present invention, a refrigerator box is shown in FIG.
It is configured by combining an outer box 1 made of metal and an inner box 3 made of hard resin. The hard resin inner box 3 is a thermoplastic resin because of its moldability. It is desirable that this thermoplastic resin not be attacked by the polyurethane foam insulation 2 of the present invention.
Resins and the like are suitable.
【0096】[0096]
【発明の効果】本発明で用いる発泡剤は、フッ素化ヨウ
化炭化水素、パーフルオロアルケンおよび水素含有フッ
化モルフォリン誘導体のうちの少なくとも一種からなる
ものである。この発泡剤は、気体熱伝導率が低く指定フ
ロンHCFC141bに劣らぬものであり、オゾン破壊
係数(ODP)や地球温暖化係数(GWP)といった環
境破壊能がきわめて低く、フォームとしての性能も従来
通り断熱性に優れた樹脂発泡体を与える。特に、フッ素
化ヨウ化炭化水素は、難燃性および自己消火性を有する
ところから、炭化水素など爆発の危険性の高い発泡剤に
混合することにより、安全な混合発泡剤として使用する
ことができる。The foaming agent used in the present invention comprises at least one of a fluorinated iodohydrocarbon, a perfluoroalkene and a hydrogen-containing fluorinated morpholine derivative. This foaming agent has a low gas thermal conductivity and is not inferior to the designated CFC HCFC141b, has extremely low environmental destructive potential such as ozone depletion potential (ODP) and global warming potential (GWP), and has the same performance as a conventional foam. A resin foam having excellent heat insulation is provided. In particular, since fluorinated iodohydrocarbon has flame retardancy and self-extinguishing property, it can be used as a safe mixed foaming agent by mixing it with a foaming agent having high risk of explosion such as hydrocarbon. .
【0097】また、前記の発泡剤に、カーボネート化合
物、エステル、またはエポキシドを添加すると発泡性が
向上する。還元剤、または酸素吸収剤の添加により、フ
ォームの性能を長期的に維持することができる。前記の
発泡剤は、水、ケトン、エーテル、エステル、炭化水素
類を混合して混合発泡剤とすることによって、プレミッ
クスの改質、発泡性の向上、気泡の均一微細化などによ
り、さらに断熱性能の高い樹脂発泡体を与える。If a carbonate compound, an ester, or an epoxide is added to the above-mentioned foaming agent, the foamability is improved. By adding a reducing agent or an oxygen absorbent, the performance of the foam can be maintained for a long time. The above-mentioned foaming agent is a mixture of water, a ketone, an ether, an ester, and a hydrocarbon to form a mixed foaming agent, whereby the premix is modified, the foaming property is improved, and the bubbles are uniformly miniaturized. It gives a high performance resin foam.
【図1】本発明による硬質ポリウレタンフォームを充填
した断熱箱体の一例を示す断面図である。FIG. 1 is a cross-sectional view showing an example of a heat insulating box body filled with a rigid polyurethane foam according to the present invention.
───────────────────────────────────────────────────── フロントページの続き (72)発明者 鈴木 正明 大阪府門真市大字門真1006番地 松下電器 産業株式会社内 (72)発明者 岸本 良雄 大阪府門真市大字門真1006番地 松下電器 産業株式会社内 ─────────────────────────────────────────────────── ─── Continuation of the front page (72) Inventor Masaaki Suzuki, 1006 Kadoma, Kadoma City, Osaka Prefecture, Matsushita Electric Industrial Co., Ltd. (72) Yoshio Kishimoto, 1006 Kadoma, Kadoma City, Osaka Matsushita Electric Industrial Co., Ltd.
Claims (27)
成され、その独立気泡内に、フッ素化ヨウ化炭化水素、
パーフルオロアルケンおよび水素含有フッ化モルフォリ
ン誘導体からなる群より選択される少なくとも一種の化
合物からなる発泡剤の気体を含むことを特徴とする断熱
性樹脂発泡体。1. A foamed resin composition having closed cells, wherein fluorinated iodohydrocarbon is contained in the closed cells.
A heat insulating resin foam comprising a gas of a foaming agent composed of at least one compound selected from the group consisting of a perfluoroalkene and a hydrogen-containing fluorinated morpholine derivative.
素、および、パーフルオロアルケンと水素含有フッ化モ
ルフォリン誘導体のいずれか一方である請求項1に記載
の断熱性樹脂発泡体。2. The heat insulating resin foam according to claim 1, wherein the foaming agent is one of a fluorinated iodohydrocarbon, and a perfluoroalkene and a hydrogen-containing fluorinated morpholine derivative.
求項1に記載の断熱性樹脂発泡体。3. The heat insulating resin foam according to claim 1, wherein the foamed resin composition contains a reducing agent.
む請求項1に記載の断熱性樹脂発泡体。4. The heat insulating resin foam according to claim 1, wherein the foamed resin composition contains an oxygen absorbent.
を有するアミンあるいはアンモニウム塩または四級アン
モニウム塩との錯化合物を含んでいることを特徴とする
断熱性樹脂発泡体。5. A heat insulating resin foam comprising a complex compound of a fluorinated iodohydrocarbon and an amine having a non-conjugated bond or an ammonium salt or a quaternary ammonium salt.
下であり、かつ、沸点65℃以下である請求項1、2ま
たは5に記載の断熱性樹脂発泡体。6. The heat insulating resin foam according to claim 1, wherein the fluorinated iodohydrocarbon has a carbon number of 4 or less and a boiling point of 65 ° C. or less.
リフルオロメタン、アイオドペンタフルオロエタン、1
ーアイオドヘプタフルオロプロパン、2ーアイオドヘプ
タフルオロプロパン、アイオド−1,1,2,2−テト
ラフルオロエタン、2−アイオド−1,1,1−トリフ
ルオロエタン、アイオドトリフルオロエチレン、1−ア
イオド−1,1,2,3,3,3−ヘキサフルオロプロ
パン、および2−アイオドノナフルオロ−t−ブタンか
らなる群より選択される少なくとも一種である請求項6
に記載の断熱性樹脂発泡体。7. The fluorinated iodohydrocarbons are iodotrifluoromethane, iodopentafluoroethane, 1
-Iodoheptafluoropropane, 2-iodoheptafluoropropane, iodo-1,1,2,2-tetrafluoroethane, 2-iodo-1,1,1-trifluoroethane, iodotrifluoroethylene, 1 7. At least one selected from the group consisting of iodo-1,1,2,3,3,3-hexafluoropropane, and 2-iodononafluoro-t-butane.
The heat-insulating resin foam according to.
ロプロペンダイマー、パーフルオロー2ーペンテン、
(パーフルオロブチル)エチレン、(パーフルオロプロ
ピル)エチレン、およびオクタフルオロシクロペンタン
からなる群より選択される少なくとも一種である請求項
1または2に記載の断熱性樹脂発泡体。8. A perfluoroalkene is hexafluoropropene dimer, perfluoro-2-pentene,
The heat insulating resin foam according to claim 1, which is at least one selected from the group consisting of (perfluorobutyl) ethylene, (perfluoropropyl) ethylene, and octafluorocyclopentane.
モノヒドロパーフルオロモルフォリンおよびモノヒドロ
パーフルオロメチルモルフォリンからなる群より選択さ
れる少なくとも一種である請求項1または2に記載の断
熱性樹脂発泡体。9. A hydrogen-containing fluorinated morpholine derivative,
The heat insulating resin foam according to claim 1, which is at least one selected from the group consisting of monohydroperfluoromorpholine and monohydroperfluoromethylmorpholine.
ン、イソペンタンおよびシクロペンタンからなる群より
選択される少なくとも一種の炭化水素を含む請求項1、
2または5に記載の断熱性樹脂発泡体。10. The closed cell further contains at least one hydrocarbon selected from the group consisting of pentane, isopentane and cyclopentane.
The heat insulating resin foam according to 2 or 5.
ル%である請求項10に記載の断熱性樹脂発泡体。11. The heat insulating resin foam according to claim 10, wherein the content of the hydrocarbon is 45 to 96 mol%.
ロアルケンおよび水素含有フッ化モルフォリン誘導体か
らなる群より選択される少なくとも一種の化合物からな
る発泡剤、ポリオール、ポリイソシアネート、ウレタン
反応触媒および整泡剤を含む樹脂原料組成物を混合する
ことにより発泡、成形することを特徴とする断熱性樹脂
発泡体の製造方法。12. A foaming agent, a polyol, a polyisocyanate, a urethane reaction catalyst and a foam stabilizer, which comprises at least one compound selected from the group consisting of fluorinated iodohydrocarbons, perfluoroalkenes and hydrogen-containing fluorinated morpholine derivatives. A method for producing a heat insulating resin foam, which comprises foaming and molding by mixing a resin raw material composition containing an agent.
素、およびパーフルオロアルケンと水素含有フッ化モル
フォリン誘導体のいずれかである請求項12に記載の断
熱性樹脂発泡体の製造方法。13. The method for producing a heat insulating resin foam according to claim 12, wherein the foaming agent is a fluorinated iodohydrocarbon, or a perfluoroalkene and a hydrogen-containing fluorinated morpholine derivative.
12または13に記載の断熱性樹脂発泡体の製造方法。14. The method for producing a heat insulating resin foam according to claim 12, further comprising water as a foaming agent.
℃以上のカーボネート化合物、エステルおよびエポキシ
ドのうち少なくとも一種を含む請求項12に記載の断熱
性樹脂発泡体の製造方法。15. A boiling point of 100 in the raw material of the resin composition.
The method for producing a heat insulating resin foam according to claim 12, which contains at least one of a carbonate compound, an ester, and an epoxide at a temperature of not less than 0 ° C.
活性剤とともにポリイソシアネ−ト組成物中に分散させ
てなるポリイソシアネートエマルジョンと、ポリオ−ル
とを混合して形成される請求項12または13記載の断
熱性樹脂発泡体の製造方法。16. The resin raw material composition is formed by mixing a polyisocyanate emulsion obtained by dispersing a reducing agent together with a surfactant in a polyisocyanate composition with a polyol. 13. The method for producing a heat insulating resin foam according to 13.
化炭化水素を含み、前記ポリオールが、少なくとも30
wt%の非アミン系ポリオールを含有する請求項12ま
たは13に記載の断熱性樹脂発泡体の製造方法。17. The blowing agent comprises at least a fluorinated iodohydrocarbon, and the polyol comprises at least 30.
The method for producing a heat insulating resin foam according to claim 12 or 13, which contains wt% of a non-amine-based polyol.
て、炭素数3以下の第一級アルコールまたは第二級アル
コールに溶解する塩を含む請求項12または13に記載
の断熱性樹脂発泡体の製造方法。18. The heat insulating resin foam according to claim 12, wherein the resin raw material composition contains, as a foaming nucleus, a salt soluble in a primary alcohol or a secondary alcohol having 3 or less carbon atoms. Production method.
合を有するアミン、アンモニウム塩または四級アンモニ
ウム塩との錯化合物、ポリオール、およびポリイソシア
ネートを含む樹脂組成物原料を混合することにより、発
泡、成形することを特徴とする断熱性樹脂発泡体の製造
方法。19. Foaming by mixing a resin composition raw material containing a complex compound of a fluorinated iodohydrocarbon and an amine having a non-conjugated bond, an ammonium salt or a quaternary ammonium salt, a polyol, and a polyisocyanate. A method for producing a heat insulating resin foam, which comprises molding.
との反応熱によって、前記錯化合物からフッ素化ヨウ化
炭化水素が分離し、そのフッ素化ヨウ化炭化水素が発泡
剤として働く請求項19記載の断熱性樹脂発泡体の製造
方法。20. The heat insulating resin according to claim 19, wherein fluorinated iodohydrocarbon is separated from the complex compound by the heat of reaction between the polyol and polyisocyanate, and the fluorinated iodohydrocarbon acts as a foaming agent. Method for producing foam.
ズ化合物、有機酸の金属塩、芳香族アミン、および有機
リン化合物からなる群より選択される少なくとも一種の
ウレタン反応触媒を含む請求項19記載の断熱性樹脂発
泡体の製造方法。21. The resin composition raw material further contains at least one urethane reaction catalyst selected from the group consisting of an organic tin compound, a metal salt of an organic acid, an aromatic amine, and an organic phosphorus compound. A method for producing a heat insulating resin foam.
化合物と等モル量までの範囲で、かつ前記ポリオール成
分100重量部に対して10重量部以下の水を含む請求
項19に記載の断熱性樹脂発泡体の製造方法。22. The heat insulation according to claim 19, wherein the resin composition raw material further contains water in an amount up to an equimolar amount with the complex compound and not more than 10 parts by weight with respect to 100 parts by weight of the polyol component. For producing a flexible resin foam.
二酸化炭素固定化触媒を含み、発泡工程中に生成する二
酸化炭素が前記エポキシドと反応してカーボネート化合
物を形成することにより、生成する発泡体の気泡内が減
圧化される工程を有する請求項12、13または19に
記載の断熱性樹脂発泡体の製造方法。23. A foam produced by the resin raw material composition containing an epoxide and a carbon dioxide-immobilized catalyst, wherein carbon dioxide produced during the foaming step reacts with the epoxide to form a carbonate compound. The method for producing a heat-insulating resin foam according to claim 12, 13 or 19, which has a step of reducing the pressure inside the bubbles.
化炭化水素および前記二酸化炭素固定化触媒を混合した
ポリイソシアネート組成物と、ポリオール、ウレタン反
応触媒、前記エポキシド、および整泡剤を含むプレミッ
クスとの混合により形成される請求項23に記載の断熱
性樹脂発泡体の製造方法。24. The resin raw material composition comprises a polyisocyanate composition in which a fluorinated iodohydrocarbon and the carbon dioxide-immobilized catalyst are mixed, a polyol, a urethane reaction catalyst, the epoxide, and a foam stabilizer. The method for producing a heat insulating resin foam according to claim 23, which is formed by mixing with a mix.
素固定化触媒とフッ素化ヨウ化炭化水素との錯化合物を
含み、ポリオールとポリイソシアネートとの反応熱によ
って、前記錯化合物が分解してフッ素化ヨウ化炭化水素
と二酸化炭素固定化触媒を生成する工程を含み、生成し
た二酸化炭素固定化触媒が、エポキシドと発泡工程中に
生成した二酸化炭素との反応に作用する請求項23に記
載の断熱性樹脂発泡体の製造方法。25. The resin raw material composition contains a complex compound of the carbon dioxide-immobilized catalyst and a fluorinated iodohydrocarbon, and the complex compound is decomposed by the heat of reaction between the polyol and the polyisocyanate to produce fluorine. 24. The heat insulation according to claim 23, comprising a step of producing a fluorinated iodohydrocarbon and a carbon dioxide-immobilized catalyst, wherein the produced carbon dioxide-immobilized catalyst acts on the reaction between the epoxide and the carbon dioxide produced during the foaming step. For producing a flexible resin foam.
ソペンタンおよびシクロペンタンからなる群より選択さ
れる少なくとも一種の炭化水素を含む請求項12、13
または19に記載の断熱性樹脂発泡体の製造方法。26. The foaming agent further comprises at least one hydrocarbon selected from the group consisting of pentane, isopentane and cyclopentane.
Alternatively, the method for producing a heat insulating resin foam according to Item 19.
ル%である請求項26に記載の断熱性樹脂発泡体の製造
方法。27. The method for producing a heat insulating resin foam according to claim 26, wherein the content of the hydrocarbon is 45 to 96 mol%.