JPH064501B2 - Self-leveling floor surface forming composition - Google Patents
Self-leveling floor surface forming compositionInfo
- Publication number
- JPH064501B2 JPH064501B2 JP60109510A JP10951085A JPH064501B2 JP H064501 B2 JPH064501 B2 JP H064501B2 JP 60109510 A JP60109510 A JP 60109510A JP 10951085 A JP10951085 A JP 10951085A JP H064501 B2 JPH064501 B2 JP H064501B2
- Authority
- JP
- Japan
- Prior art keywords
- floor surface
- composition
- self
- cement
- emulsion
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Lifetime
Description
【発明の詳細な説明】 (産業上の利用分野) 本発明は、地下地上に塗布して平滑性が容易に得られ、
靭性を有した床仕上げ面となるセルフレベリング床面形
成用組成物に関する。DETAILED DESCRIPTION OF THE INVENTION (Industrial field of application) The present invention can be applied to an underground surface to easily obtain smoothness,
The present invention relates to a composition for forming a self-leveling floor surface which is a tough floor finish surface.
(従来技術) 従来、セメントモルタルにポリマーエマルジョンを混合
し、セメントモルタルのみの場合の引張り弱さ、もろさ
等の特性を改良し、靭性、接着性、防水性等の特性を向
上せしめ、セメントモルタルに多少のフレキシブル性を
与えるようにするということは知られている。斯かる如
き従来のセメントモルタルとエマルジョンとの混合物は
一般に外壁や床の下地の不陸修正材として用いられてい
たが、近時外装材、天井材、床材等に用いられるように
なってきている。これは、従来のフレキシブル材がアク
リル、ゴルラテックス等の可燃性の有機物質であったの
に対し、セメントモルタルが無機質で一種の不燃性フィ
ラーとしての役をなし、上記混合物が難燃性のフレキシ
ブル材という特性をなすからであり、又、無機質系のた
めに耐候性もよく防水特性にも優れているという理由か
らである。(Prior Art) Conventionally, by mixing a polymer emulsion with cement mortar and improving properties such as tensile weakness and brittleness in the case of only cement mortar and improving properties such as toughness, adhesiveness and waterproofness, cement mortar It is known to provide some flexibility. Such a mixture of conventional cement mortar and emulsion was generally used as a non-planar correction material for outer walls and floor substrates, but recently it has come to be used for exterior materials, ceiling materials, floor materials, etc. There is. This is because the conventional flexible materials were flammable organic substances such as acrylic and gol latex, whereas cement mortar is inorganic and acts as a kind of non-combustible filler, and the above mixture is a flame-retardant flexible material. This is because it has the property of being a material, and because it is an inorganic material, it has excellent weather resistance and excellent waterproof properties.
然るに、上記混合物にあってはエマルジョンのポリマー
のセメントに対する混合割合が通常15〜20重量%程
度を限度としており、これ以上入れた場合にはセメント
の水和反応を阻害又は遅延させてしまうという実用上の
問題があり、セメントの適度の硬化時間を確保するため
に、エマルジョンの添加量を制限せざるを得ず、その結
果十分なフレキシブル特性等が得られないという問題が
あった。However, in the above mixture, the mixing ratio of the polymer of the emulsion to the cement is usually limited to about 15 to 20% by weight, and if more than this is added, the hydration reaction of the cement will be impaired or delayed. However, there is a problem in that the amount of emulsion added must be limited in order to secure an appropriate setting time for the cement, and as a result, sufficient flexibility and the like cannot be obtained.
又、水溶性高分子を保護コロイドとしたポリマーエマル
ジョンを混入して水和反応の阻害又は遅延を比較的穏や
かにしたものが、特開昭58−55355等に開示され
ているが、これらに示されたエマルジョンを混合したセ
メントスラリーは、水溶性高分子の存在により、スラリ
ー粘度が高く、チクソトロピックな粘性を示すので、構
築物の下地処理セメントモルタルや目地セメントモルタ
ル、補修セメントモルタル、接着用セメントモルタル
等、或いは耐水性を有することから防水セメントモルタ
ル用として提供されている。Further, a polymer emulsion in which a water-soluble polymer is used as a protective colloid to make the inhibition or delay of the hydration reaction relatively mild is disclosed in JP-A-58-55355 and the like. The cement slurry mixed with the prepared emulsion has a high viscosity of slurry due to the presence of the water-soluble polymer and exhibits thixotropic viscosity. Etc., or because it has water resistance, it is provided for waterproof cement mortar.
(発明が解決しようとする問題点) ところで、仕上り上平滑性を必要とする床面は、セルフ
レベリング性と同時に施工作業性のよい硬化性を必要と
するもので、このような床面を形成するポリマーセメン
トスラリーが望まれるが、この用途への水溶性高分子ポ
リマーエマルジョンの応用は未開発であった。(Problems to be solved by the invention) By the way, a floor surface requiring finish smoothness requires self-leveling property and at the same time hardenability for good construction workability. Polymer cement slurries are desired, but the application of water-soluble polymer emulsions for this purpose has not been developed.
しかしながら、ポリマーセメント本来の靭性、接着性、
防水性等は床面としても有用であり、種々の加工上の問
題点を同時に解決して、上記未開発のセルフレベリング
床面形成用組成物を提供出来ることが好ましい。However, the toughness, adhesion, and
Water resistance and the like are also useful as a floor surface, and it is preferable to be able to simultaneously solve various processing problems and provide the above-mentioned undeveloped composition for forming a self-leveling floor surface.
本発明は、斯くの如き着眼に立ち種々な問題点を同時に
解決するため鋭意研究を重ねた結果、特定の組成を有す
るポリマーエマルジョンを混合することによって、セル
フレベリング床面形成用組成物となし得ることを見出し
た。As a result of earnest studies to solve various problems at the same time, the present invention can be made into a self-leveling floor surface-forming composition by mixing a polymer emulsion having a specific composition. I found that.
(問題点を解決するための手段及び作用効果) 即ち、上記目的を達成した床面形成用組成物を得る混和
用エマルジョンとは、実質的にアニオン性界面活性剤を
含まず且つ分子中に水酸基を持ったノニオン性水溶液性
高分子の存在下で乳化重合して得られる合成樹脂エルジ
ョンである。(Means and Actions for Solving Problems) That is, an admixture for obtaining a composition for forming a floor surface which achieves the above-mentioned object is a mixture containing substantially no anionic surfactant and a hydroxyl group in the molecule. A synthetic resin eljon obtained by emulsion polymerization in the presence of a nonionic aqueous polymer.
アニオン性界面活性剤を使用して乳化重合したものは、
セメント等水硬性組成物と混和したとき配合物ペースト
粘度が不安定になり易く、又、各種粘度安定剤を添加し
た場合は水硬性組成物の硬化を阻害、遅延するので不適
当である。又、分子中に水酸基を持ったノニオン性の水
溶性高分子を使用して乳化重合したものが床材としての
各性能を満たし得る。該水溶性高分子を例示すると、各
種ヒドロキシエチルセルロース誘導体、各種ポリビニル
アルコール誘導体、各種ポリエチレンオキサイド誘導
体、各種デンプン誘導体等である。What was emulsion polymerized using an anionic surfactant,
Mixing with a hydraulic composition such as cement tends to make the viscosity of the paste paste unstable, and the addition of various viscosity stabilizers is not suitable because it inhibits or delays the hardening of the hydraulic composition. Also, emulsion polymerization using a nonionic water-soluble polymer having a hydroxyl group in the molecule can satisfy each performance as a flooring material. Examples of the water-soluble polymer include various hydroxyethyl cellulose derivatives, various polyvinyl alcohol derivatives, various polyethylene oxide derivatives, various starch derivatives and the like.
但し上記においては必要に応じて、セメント水和反応の
阻害及び配合物ペーストの流動性低下等の弊害が生じな
い範囲内でのみ他のイオン性界面活性剤を併用してもよ
い。However, in the above case, other ionic surfactants may be used together, if necessary, within a range that does not cause adverse effects such as inhibition of cement hydration reaction and deterioration of fluidity of the compound paste.
エマルジョン中に分散しているポリマーは、各種水硬性
組成物と混和して床面としての性能を満たすものであれ
ば限定されないが、一般的には常温で造膜する必要があ
り、例えば、アクリル酸エステル、スチレン、酢酸ビニ
ル、ベオバ、エチレン、塩化ビニル、ジエン系各モノマ
ーの単独又は共重合ポリマー等である。The polymer dispersed in the emulsion is not limited as long as it is mixed with various hydraulic compositions to satisfy the performance as a floor surface, but generally it is necessary to form a film at room temperature, for example, acrylic. Examples thereof include acid ester, styrene, vinyl acetate, veova, ethylene, vinyl chloride, and diene-based monomers which are homopolymers or copolymers.
上記乳化重合して得られたエマルジョンの水硬性組成物
に対する混合割合は、樹脂固形分として50乃至100
重量%が好ましく、80重量%前後が最も好ましい。約
50重量%以下であると硬化後にひび割を生じる危険性
があり、100重量%以上となると経済性の点で負担が
大きい。The mixing ratio of the emulsion obtained by emulsion polymerization to the hydraulic composition is 50 to 100 as resin solid content.
Weight% is preferable, and about 80 weight% is the most preferable. If it is about 50% by weight or less, there is a risk of cracking after curing, and if it is 100% by weight or more, the cost is heavy in terms of economy.
上記エマルジョンをセメントの如き水硬性組成物と混合
し塗布せしめると、一般的に分散媒にある水の基材への
吸収と塗面よりの蒸散によるエマルジョンの硬化、及び
水硬性組成物の吸水硬化による脱水作用ということに加
え、乳化剤が、上記の如く水硬性組成物の硬化阻害因子
を排除せしめる配合となっているので、水硬性組成物に
対するポリマー比を1対1程度としても、水硬性組成物
の水和反応は阻害されることがなく、従って、斯かる混
合組成物の硬化反応を速めることができ、厚塗した場合
でも内部を容易に硬化せしめることができる。このこと
はポルトランド、白セメントアルミナを用いた場合は勿
論、アルミナ、早強セメント等の水硬性組成物を用いた
場合でも同様に行われる。しかもこの場合所要量のエマ
ルジョンが混和されていることにより、それによる靭
性、接着性、防水性等の特性が十分に生かされるので、
硬化後も該組成物のフレキシブル性は適正に確保され
る。更にペーストのレベルリング性が良いために平滑面
が形成でき、仕上げに関する作業を省略することができ
る。When the above emulsion is mixed with a hydraulic composition such as cement and applied, the emulsion is generally hardened by absorption of water in the dispersion medium to the substrate and evaporation from the coated surface, and water absorption hardening of the hydraulic composition. In addition to the dehydration effect by the above, since the emulsifier has a composition that eliminates the curing inhibitor of the hydraulic composition as described above, even if the polymer ratio to the hydraulic composition is about 1 to 1, The hydration reaction of the product is not hindered, and therefore, the curing reaction of such a mixed composition can be accelerated, and the inside can be easily cured even when it is applied thickly. This applies not only when Portland or white cement alumina is used, but also when a hydraulic composition such as alumina or early cement is used. Moreover, in this case, since the required amount of emulsion is mixed, the characteristics such as toughness, adhesiveness, and waterproofness can be fully utilized.
Even after curing, the flexibility of the composition is properly ensured. Further, since the leveling property of the paste is good, a smooth surface can be formed, and the work for finishing can be omitted.
上述の如くしてなる本発明に係る混合組成物は、適宜骨
材、顔料、添加剤等を加え、単頭乃至は多頭のガン吹き
工法によって施工することができる。例えば、単頭ガン
によりアクリル樹脂顔料の青色により地を形成し、次い
で白色によって模様吹きを行い、さらに地色と同様の青
色で戻し吹きを行う等のことをすれば、流動特性とも相
俟って色の重なりが適宜になじみ、複雑でしかもマイル
ドな感じの光沢を有した、色彩感にすぐれた模様面の床
を現出せしめることができる。多頭ガンによれば、良好
な流動性によって、各ガン頭から異色の組成物を同時吹
き付けすることができ、独自の色混合床を容易に施工す
ることできる。The mixed composition according to the present invention as described above can be applied by a single-head or multi-head gun blowing method by appropriately adding aggregates, pigments, additives and the like. For example, if the background is formed with the blue color of the acrylic resin pigment with a single-headed gun, then the pattern is blown with white, and then the back-blowing is performed with the same blue color as the background color, the flow characteristics are also combined. It is possible to bring out a floor with a patterned surface that has an excellent color sense and has a complex and mild luster that blends colors appropriately. According to the multi-headed gun, the composition of different color can be simultaneously sprayed from the heads of each gun due to the good fluidity, and the unique color mixing bed can be easily constructed.
本発明によれば、上記の如く、無機質系でありながら極
めて良好なフレキシブル性を有した床面形成材で、弾性
床を形成することができ、硬化速度が速くセルフレベリ
ング性にすぐれた施工性が極めてよいセルフレベリング
床面形成用組成物を提供できる。According to the present invention, as described above, it is possible to form an elastic floor with a floor surface forming material that is an inorganic material and has very good flexibility, and the curing rate is fast and the self-leveling property is excellent. It is possible to provide a composition for forming a self-leveling floor surface which is extremely excellent.
(実施例) ・第1表について 本発明に係る乳化重合して得られたエマルジョンを配合
してなるポリマーセメントスラリーの実施例1〜3、及
びこれらと対比すべく本発明とは異なる乳化剤によるエ
マルジョンを配合したポリマーセメントスラリーによる
対比例1,2のそれぞれのスラリー性状、セメント硬化
時間、塗膜表面性を調べた。その結果が第1表である。(Examples) Table 1 Examples 1 to 3 of polymer cement slurries obtained by blending emulsions obtained by emulsion polymerization according to the present invention, and emulsions with emulsifiers different from the present invention to compare with these. The slurry properties, the cement hardening time, and the coating surface properties of the polymer cement slurries in which the ratios of 1 and 2 were compared were examined. The results are shown in Table 1.
試験方法は、必要に応じて水で吹付け適正粘度に調整
し、粘度,チクソトロピー指数はB型回転粘度計3号ロ
ーターを用いて測定し、フロー値は、ガラス板上に置い
た内径50mm、高さ50mmの塩ビパイプに試料を満たし
た後、直ちにパイプを抜取って広がりを直径で測定し
た。塗膜表面性は目視判定し、○は良好、△はやや良、
×は不良であった。The test method was adjusted by spraying with water to an appropriate viscosity, and the viscosity and thixotropy index were measured using a B-type rotational viscometer No. 3 rotor, and the flow value was an inner diameter of 50 mm placed on a glass plate, After filling a 50 mm high PVC pipe with the sample, the pipe was immediately withdrawn and the spread was measured by the diameter. The surface property of the coating film is visually evaluated, and ○ is good, Δ is slightly good,
X was bad.
この結果、綜合判定として床面形成用組成物として十分
な適性、即ち適度な燃性を有し、セルフレベリング性に
よって平滑性が得られ、かつ硬化時間が適切なものは、
本発明に係る実施例1,2,3のものであった。比較例
1,2はいずれも実用に供し得ないものであった。尚、
比較例2は約10分でペースト粘度が上昇してしまった。As a result, a composition having sufficient suitability as a floor surface-forming composition as a comprehensive judgment, that is, having suitable flammability, having smoothness by self-leveling property, and having an appropriate curing time,
It was one of Examples 1, 2, and 3 according to the present invention. Comparative Examples 1 and 2 could not be put to practical use. still,
In Comparative Example 2, the paste viscosity increased in about 10 minutes.
・第2表について 上記本発明に係る実施例3のエマルジョンを用い、ポリ
マーセメントの配合比を変えて、夫々のスラリー性状、
セメント硬化時間、塗膜表面性を調べた結果が第2表で
ある。-About Table 2 Using the emulsion of Example 3 according to the present invention, changing the compounding ratio of the polymer cement, the respective slurry properties,
Table 2 shows the results of examining the cement hardening time and the coating film surface property.
この結果、ポリマーセメント比即ちP/Cは、50重量
%前後より明確に少ないとクラックが発生してしまうの
で、50〜100重量%前後が好ましいことが確認され
た。床としての硬度も十分であった。なお、フィラー量
が多すぎるとクラックが生じ、P/Cが高い試料4は樹
脂分が多く床として弾性感があった。As a result, it was confirmed that the polymer cement ratio, that is, P / C, is preferably 50 to 100% by weight, because cracks occur when the amount is clearly less than around 50% by weight. The hardness as a floor was also sufficient. It should be noted that when the amount of the filler was too large, cracks occurred, and Sample 4 having a high P / C had a large amount of resin and had an elastic feeling as a floor.
───────────────────────────────────────────────────── フロントページの続き (51)Int.Cl.5 識別記号 庁内整理番号 FI 技術表示箇所 C04B 24:38 Z 2102−4G 24:26 F 2102−4G G 2102−4G C 2102−4G A 2102−4G ) Z 2102−4G (56)参考文献 特開 昭57−71842(JP,A) 特開 昭59−146960(JP,A) 特開 昭59−203742(JP,A) 特開 昭58−138764(JP,A)─────────────────────────────────────────────────── ─── Continuation of the front page (51) Int.Cl. 5 Identification code Internal reference number FI technical display location C04B 24:38 Z 2102-4G 24:26 F 2102-4G G 2102-4G C 2102-4G A 2102 -4G) Z 2102-4G (56) Reference JP-A-57-71842 (JP, A) JP-A-59-146960 (JP, A) JP-A-59-203742 (JP, A) JP-A-58- 138764 (JP, A)
Claims (1)
つ分子中に水酸基を持ったノニオン性水溶性高分子の存
在下で乳化重合して得られる合成樹脂エマルジョンを、
無機質の水硬性組成物に対して樹脂固形分として50乃
至100重量%の割合で混合してなるセルフレベリング
床面形成用組成物。1. A synthetic resin emulsion obtained by emulsion polymerization in the presence of a nonionic water-soluble polymer having substantially no anionic surfactant and having a hydroxyl group in the molecule,
A composition for forming a self-leveling floor surface, which is obtained by mixing an inorganic hydraulic composition at a resin solid content of 50 to 100% by weight.