JPH0625995A - Incombustible sheet - Google Patents

Incombustible sheet

Info

Publication number
JPH0625995A
JPH0625995A JP3230392A JP3230392A JPH0625995A JP H0625995 A JPH0625995 A JP H0625995A JP 3230392 A JP3230392 A JP 3230392A JP 3230392 A JP3230392 A JP 3230392A JP H0625995 A JPH0625995 A JP H0625995A
Authority
JP
Japan
Prior art keywords
binder
paper
sepiolite
sheet
fiber
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP3230392A
Other languages
Japanese (ja)
Other versions
JP2502236B2 (en
Inventor
Kenzo Hayashi
鍵三 林
Kozo Hayashi
宏三 林
Koji Tsuchiya
孝次 土屋
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tokiwa Electric Co Ltd
Original Assignee
Tokiwa Electric Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tokiwa Electric Co Ltd filed Critical Tokiwa Electric Co Ltd
Priority to JP4032303A priority Critical patent/JP2502236B2/en
Publication of JPH0625995A publication Critical patent/JPH0625995A/en
Application granted granted Critical
Publication of JP2502236B2 publication Critical patent/JP2502236B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

PURPOSE:To provide incombustibility and water resistance to a sheet and improve producibility and enable low-cost sheet making due to mass production by using sepiolite as a main raw material. CONSTITUTION:The incombustible sheet is obtained by making slurry consisting essentially of the first binder composed of sepiolite as a main material, glass fiber which is an inorganic fiber as a reinforcement and polyacrylamide which is a thermoplastic resin and the second binder composed of polyamidepolyamine epichlorohydrin which is a thermosetting resin into a sheet.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、壁装材、耐熱化粧板シ
ート等に用いられる不燃性シートに関するもので、特
に、石綿代替品として不燃性と耐熱性を有し、しかも、
生産性に優れた不燃性シートに関するものである。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a non-combustible sheet used for wall coverings, heat-resistant decorative sheet, etc., and particularly, it has non-combustibility and heat resistance as a substitute for asbestos.
The present invention relates to a nonflammable sheet having excellent productivity.

【0002】[0002]

【従来の技術】近年、火災事故の防止に係わる社会的ニ
ーズのもとに、プラスチックや衣料などとともに建築内
装材などで防炎・耐火といった問題が取上げられ、かな
り厳しく規制されるようになった。紙等のシートもその
例にもれず、壁装材を始めとして「燃えない・熱に強
い」いわゆる防炎性・不燃性シートの市場の要求は多
い。従来、汎用な燃えない紙とは、無機繊維では石綿繊
維紙が代表とされていた。この石綿繊維紙は難燃、耐
熱、高強度、易生産性、廉価等すべての面で卓越してお
り、有機繊維では困難な応用の領域をカバーし、幅広い
用途を持っていた。
2. Description of the Related Art In recent years, due to social needs related to prevention of fire accidents, problems such as fireproofing and fireproofing of interior materials such as plastics and clothing have come to be regulated considerably. . Sheets such as paper are no exception to this, and there are many market demands for so-called flameproof / noncombustible sheets, such as wall coverings, that do not burn or resist heat. Heretofore, asbestos fiber paper has been typified as the inorganic fiber as the general-purpose non-burnable paper. This asbestos fiber paper excels in all aspects such as flame retardancy, heat resistance, high strength, easy productivity, and low price. It covers a range of applications that are difficult for organic fibers and has a wide range of uses.

【0003】ここで、石綿の特性に触れると、通常の石
綿はかんらん石や輝石などの鉱石が、高圧下の地殻中で
地熱と地下水の水熱作用によって、蛇紋岩や角閃岩とな
って繊維状に晶結したものである。そのなかで、製紙原
料として用いられる品種は、蛇紋岩系のクリソタイル石
綿が多く、その化学式は、3MgO・2SiO2 ・2H
2 Oである。繊維直径は20〜40nmと極めて細く、柔
軟性である。硬度は2.5〜4.0と低く、摩耗材に使
われるのもこの点にある。また、これを抄紙する場合、
結晶水を包含しているので水とのなじみが良い。他の添
加物との混合においては、クリソタイルは水中での帯電
がカチオンであるので、吸着、補集性が良い。この物性
は紙シートにすると、強く、燃えなく、柔かく、平滑性
があって抄き易いなど無機繊維としての利点がある。
[0003] As for the characteristics of asbestos, ordinary asbestos becomes ores such as olivine and pyroxene as serpentine and amphibolite due to the geothermal and hydrothermal effects of groundwater in the crust under high pressure. It is a fibrous crystal. Among them, most of the varieties used as raw materials for papermaking are chrysotile asbestos of the serpentine series, the chemical formula of which is 3MgO · 2SiO 2 · 2H.
2 O. The fiber diameter is 20 to 40 nm, which is extremely thin and flexible. The hardness is as low as 2.5 to 4.0, which is why it is used as a wear material. Also, when making paper from this,
As it contains crystal water, it has good compatibility with water. In the case of mixing with other additives, chrysotile has good adsorption and scavenging properties because the charge in water is cation. These physical properties of a paper sheet are advantageous as an inorganic fiber such as strong, non-flammable, soft, smooth and easy to make.

【0004】ところが、最近、石綿は健康を害する作用
があるため、日本においては徐々に使えなくなった。ま
た、西欧においてもほぼ使えない状態にある。
However, recently, asbestos has a harmful effect on health, so that it has gradually become unusable in Japan. In Western Europe, it is almost unusable.

【0005】この状況から、現在、新素材の発達ととも
に、石綿に類した代替材の開発は、各所において盛んに
研究されており、高性能な無機繊維或いはウイスカーが
次々と開発されている。例えば、ピッチ系汎用炭素繊
維、チタン酸カリウム繊維、アルミナ−シリカ繊維、ガ
ラス繊維等がやや普及的に使われている。他に、石膏繊
維、塩基性硫酸マグネシウム繊維、リン酸繊維、ピロホ
ウ酸マグネシウム繊維等もある。ところが、これらの繊
維は用途、生産性、価格等において石綿の代替となる域
には達していないのが実状である。
From this situation, with the development of new materials, the development of alternative materials similar to asbestos is being actively researched in various places, and high-performance inorganic fibers or whiskers are being developed one after another. For example, pitch-based general-purpose carbon fibers, potassium titanate fibers, alumina-silica fibers, glass fibers and the like are used rather widely. In addition, gypsum fiber, basic magnesium sulfate fiber, phosphoric acid fiber, magnesium pyroborate fiber and the like are also available. However, in reality, these fibers have not reached the level of alternatives to asbestos in terms of use, productivity, price, etc.

【0006】他に、燃えにくい紙を作る方法として、防
炎化の手段がある。これは壁紙、障子紙、紙製熱交換器
等にみられる方法で、着火をしない処理方法と言える。
基材はクラフト紙等の木材パルプ紙に防炎剤を含浸また
は塗布するもので、含アンモニウム塩型水性無機塩、含
燐窒素化合物、含燐ハロゲン化合物、三酸化アンチモン
−ハロゲン化合物、ホウ素化合物、ハロゲン化合物など
が用いられる。しかし、この処理は所詮有機物が主体で
あり完全不燃とは言えない。また、高性能繊維として芳
香族ポリアミド繊維もあるが汎用的でない。
[0006] In addition, there is a flameproofing method as a method for producing a paper that is difficult to burn. This is a method found in wallpaper, shoji paper, paper heat exchangers, etc., and can be said to be a treatment method that does not ignite.
The base material is one obtained by impregnating or coating a wood pulp paper such as kraft paper with a flameproofing agent, an ammonium-containing salt type aqueous inorganic salt, a phosphorus-containing nitrogen compound, a phosphorus-containing halogen compound, an antimony trioxide-halogen compound, a boron compound, A halogen compound or the like is used. However, this treatment is mainly organic matter after all and cannot be said to be completely nonflammable. Aromatic polyamide fibers are also used as high-performance fibers, but they are not widely used.

【0007】このような状況から、石綿繊維紙が使えな
い面を他の繊維を利用して代替する開発が社会的、産業
的見地から一層強く要求されてきている。汎用的な用途
からみると、壁装材、シール材、ガスケット、パッキン
グ、アスファルトルーヒング、クッションフロアー、不
燃コアー、建材表装紙、積層紙、断熱材等あらゆる用途
でのニーズがある。
Under these circumstances, there is a strong demand from a social and industrial point of view to develop a surface that cannot use asbestos fiber paper by using another fiber. From a general-purpose application, there is a need for a wide range of applications such as wall coverings, sealing materials, gaskets, packing, asphalt roofing, cushion floors, incombustible cores, building material covering paper, laminated paper, and heat insulating materials.

【0008】こういった中で、既存の天然繊維物の中か
ら石綿代替として、セピオライトの利用可能性が着目さ
れている。そして、セピオライトを利用した不燃性シー
トの事例も多い。
[0008] Under these circumstances, the possibility of using sepiolite as an alternative to asbestos among the existing natural fiber products is drawing attention. There are also many cases of non-combustible sheets that use sepiolite.

【0009】ここで、セピオライトとは、通称、マウン
テンレザー(山皮)、マウンテンコルク、マウンテンウ
ッドと呼ばれている粘土鉱物で、日本における海泡石も
この一種である。外観はコルク状であったり、レザー状
であったり、まっ白な柔かい塊であったりするが、一般
には繊維性を持ったケイ酸マグネシウムの塊である。一
応、一次元構造粘土に分類されているものの、見方によ
ってはある方向に削れ易いレンガ積みの結晶性三次元構
造とみることもでき、ケイ素、マグネシウム、酸素、水
酸基、結晶水からなる晶形群を形成している。物性は吸
着性、揺変性、固結性の基本的な性質がある。
Here, sepiolite is a clay mineral commonly referred to as mountain leather, mountain cork, and mountain wood, and sepiolite in Japan is also a kind of this. The appearance may be cork-like, leather-like, or a pure white soft lump, but it is generally a magnesium silicate lump having fibrous properties. For the time being, although it is classified as a one-dimensional structure clay, it can be considered as a crystalline three-dimensional structure of bricks that can be easily shaved in a certain direction depending on the viewpoint, and a crystal form group consisting of silicon, magnesium, oxygen, hydroxyl group, and crystal water is Is forming. Physical properties have basic properties such as adsorption, thixotropy, and solidification.

【0010】この特性を用いた製紙の事例としては、例
えば、特開昭51−88799号公報、特開昭56−1
65097号公報、特開昭58−95636号公報、特
開昭58−144196号公報、特開昭59−2180
0号公報、特開昭61−258099号公報、特開昭6
3−235600号公報、特開昭64−61599号公
報等に掲載の技術がある。
Examples of papermaking using this characteristic include, for example, Japanese Patent Laid-Open Nos. 51-88799 and 56-1.
65097, JP-A-58-95636, JP-A-58-144196, JP-A-59-2180.
No. 0, JP 61-258099 A, JP 6
There are techniques disclosed in JP-A-3-235600, JP-A-64-61599 and the like.

【0011】[0011]

【発明が解決しようとする課題】ところで、前記不燃性
シートにおいて掲載した公報は、セラミック繊維等の無
機繊維や布、即ち、有機繊維またはこの両者からなる繊
維に吸着性、揺変性、固結性に富んだセピオライトを補
助的に用いて混合、分散させて処理し、乾燥したものが
多い。これは、セピオライトが微細繊維であるために、
紙に抄造する場合、濾水性が悪く、また、一般的に濾水
性の良い木材パルプ、合成繊維、無機繊維等からなるス
ラリーにおいて添加されている対原材料比0.01〜
0.1%の凝集剤の添加量では任意なシート形成性が困
難であるのと、引裂強度が劣るなどの原因からセピオラ
イトを主原料として抄紙することが困難なことによる。
なお、凝集剤の添加量を対原材料比0.1%以上として
も濾水性は向上しないだけでなく、過剰の添加はスラリ
ーの粘性が大きくなり、かえって抄紙性を低下させてし
まう。このようなことから、従来、実験室的な少量生産
の場合には可能としても、量産ベースに合致した工業生
産は極めて困難であり、セピオライトの持つ優れた特性
が十分に生かされていなかった。僅かに、特開昭59−
21800号公報において、セピオライト繊維単独使用
についての記載があるが、具体的な技術内容についての
記載がなく、実用性に欠けている。
DISCLOSURE OF THE INVENTION Problems to be Solved by the Invention In the publication mentioned in the non-combustible sheet, the inorganic fiber such as ceramic fiber or cloth, that is, the organic fiber or the fiber composed of both of them is adsorbable, thixotropic, and caking. In many cases, it was mixed, dispersed, treated, and dried with the help of sepiolite, which is rich in water. This is because sepiolite is a fine fiber,
In the case of papermaking, the drainage is poor, and the ratio of raw materials to raw materials added to a slurry generally composed of wood pulp, synthetic fibers, inorganic fibers, etc. having a good drainage of 0.01 to
This is because it is difficult to form an arbitrary sheet with the amount of the coagulant added of 0.1%, and it is difficult to make paper from sepiolite as a main raw material because of the poor tear strength.
Even if the amount of the aggregating agent added is 0.1% or more with respect to the raw material, not only the drainage performance is not improved, but also the excessive addition increases the viscosity of the slurry and rather deteriorates the papermaking property. For this reason, in the past, even in the case of small-scale production in a laboratory, industrial production in conformity with the mass production base was extremely difficult, and the excellent properties of sepiolite were not fully utilized. Slightly, JP-A-59-
In Japanese Patent No. 21800, there is a description of using sepiolite fiber alone, but there is no description of specific technical contents, and it is not practical.

【0012】[0012]

【課題を解決するための手段】請求項1にかかる不燃性
シートは、主材としてのセピオライトと、熱可塑性樹脂
からなる固着用の第1バインダーと、熱硬化性樹脂から
なる凝集、耐水用の第2バインダーとを必須成分とした
スラリーを抄造してなるものである。
A non-combustible sheet according to a first aspect of the present invention comprises a sepiolite as a main material, a first binder for fixing made of a thermoplastic resin, and a cohesive, water-resistant sheet made of a thermosetting resin. It is made by making a slurry containing a second binder as an essential component.

【0013】請求項2にかかる不燃性シートは、主材と
してのセピオライトと、アニオン系の熱可塑性樹脂から
なる固着用の第1バインダーと、カチオン系の熱硬化性
樹脂からなる凝集、耐水用の第2バインダーと、アニオ
ン系の熱可塑性樹脂からなる凝集用の第3バインダー
と、カチオン系の熱可塑性樹脂からなる凝集用の第4バ
インダーとを必須成分としたスラリーを抄造してなるも
のである。
A non-combustible sheet according to a second aspect of the present invention comprises sepiolite as a main material, a first binder for fixing which is an anionic thermoplastic resin, and an agglomerating and water-resistant resin made of a cationic thermosetting resin. The second binder, the third agglomerating binder made of an anionic thermoplastic resin, and the fourth agglomerating binder made of a cationic thermoplastic resin are made into papers as essential components. .

【0014】請求項3にかかる不燃性シートは、請求項
1または請求項2に記載のスラリーに、補強材としての
無機繊維を必須成分として追加したものである。
A nonflammable sheet according to a third aspect is obtained by adding the inorganic fiber as a reinforcing material as an essential component to the slurry according to the first or second aspect.

【0015】[0015]

【作用】請求項1においては、セピオライトに第1バイ
ンダー及び第2バインダーを加えて抄造したシートは、
主成分が無機繊維であるセピオライトであることによ
り、不燃性を有するとともに、廉価に製造できる。ま
た、第1バインダーの熱可塑性樹脂はセピオライトの固
着性に寄与し、シートの強度を向上する。更に、第2バ
インダーの熱硬化性樹脂であるEPAは、網目状の三次
元構造をもった高分子化合物であって原子が強い共有結
合で結ばれているので、水に対して安定で、紙に耐水性
を与えるとともに、抄造における濾水性を向上させてシ
ートの形成を容易にする。
According to the first aspect of the invention, the sheet made by adding the first binder and the second binder to sepiolite is
Since the main component is sepiolite, which is an inorganic fiber, it has noncombustibility and can be manufactured at low cost. Moreover, the thermoplastic resin of the first binder contributes to the fixing property of sepiolite and improves the strength of the sheet. Further, EPA, which is a thermosetting resin of the second binder, is a polymer compound having a network-like three-dimensional structure, and since the atoms are bound by strong covalent bonds, it is stable to water and is stable on paper. To provide water resistance to the sheet and improve drainage during papermaking to facilitate the formation of a sheet.

【0016】また、請求項2においては、第1バインダ
ー及び第2バインダーを加えた後、カチオンサイドにな
っているスラリーにアニオン系の凝集剤である第3バイ
ンダーを加えることによりフロックは粗大化する。次い
で、カチオン系の凝集剤である第4バインダーを加える
と、前記フロックは疎水化し、強固となる。これによっ
て、濾水性は更に向上する。
According to the second aspect of the present invention, after adding the first binder and the second binder, the floc is coarsened by adding the third binder which is an anionic flocculant to the cation side slurry. . Next, when a fourth binder, which is a cationic flocculant, is added, the flocs become hydrophobic and become strong. This further improves drainage.

【0017】更に、請求項3においては、請求項1また
は請求項2の作用に加えて、補強材としての無機繊維を
混ぜたことにより、更にシートの強度物性が向上する。
Further, in the third aspect, in addition to the action of the first or second aspect, the strength physical properties of the sheet are further improved by mixing the inorganic fiber as the reinforcing material.

【0018】[0018]

【実施例】以下、本発明の一実施例を図1乃至図5に基
づいて説明する。
DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will be described below with reference to FIGS.

【0019】図1は本発明の一実施例における不燃性シ
ートの製造工程の概略を示す説明図である。
FIG. 1 is an explanatory view showing an outline of a manufacturing process of a nonflammable sheet in one embodiment of the present invention.

【0020】本実施例においては、セピオライトの特性
を十分に生かすために、セピオライトを80%以上と
し、これにバインダー等を加えてスラリー化し、抄造し
た。通常、セピオライトリッチにすると、抄紙において
濾水性が悪く、任意の厚さのものが抄けない。特に、抄
紙機を用い、200g/m2 以上の秤量のものは抄紙速
度に合わない。一方、100g/m2 周辺の薄い紙は、
湿紙強度がなく、機械での搾水、搬送等連続抄紙性に問
題がある。
In this example, in order to make the best use of the characteristics of sepiolite, sepiolite was made to be 80% or more, and a binder or the like was added to this to make a slurry, and papermaking was carried out. Usually, when sepiolite rich is used, the drainage is poor in papermaking, and paper of any thickness cannot be made. In particular, using a paper machine, a machine weighing 200 g / m 2 or more does not match the paper making speed. On the other hand, the thin paper around 100 g / m 2
There is no wet paper strength, and there is a problem with continuous paper making properties such as water squeezing and conveyance by machines.

【0021】この問題を克服するために、本開発研究に
おいては、紙料調整、濾水性、改良処理、適正バインダ
ーの選択、適正装置の考案、改良等を行なった。
In order to overcome this problem, in the present development research, paper stock adjustment, drainage, improvement treatment, selection of an appropriate binder, devising of an appropriate device, improvement, etc. were carried out.

【0022】まず、本実施例における不燃性シートの製
造工程について説明する。
First, the manufacturing process of the nonflammable sheet in this embodiment will be described.

【0023】図において、解繊工程Aでは主原料である
セピオライトと、補強材としてのガラス繊維と補強繊維
の木材パルプと合成繊維とを解繊機に入れて、撹拌によ
って解繊し、繊維の分散を良くする。なお、この実施例
において、木材パルプ量は、5重量%以上とすると、不
燃性に支障をきたすこととなるので、5重量%以下に抑
えている。
In the figure, in the defibration step A, sepiolite as a main raw material, glass fiber as a reinforcing material, wood pulp as a reinforcing fiber, and synthetic fiber are put into a defibrating machine and defibrated by stirring to disperse the fibers. Improve In this example, if the amount of wood pulp is 5% by weight or more, nonflammability will be impaired, so the amount is limited to 5% by weight or less.

【0024】次に、原料混合工程Bでは解繊されたセピ
オライト、第1バインダー、第2バインダー、軟化剤、
安定剤等を混合タンクに入れて混合し、スラリーを作製
する。ここで使用する第1バインダーは、紙力を増加す
るため、熱可塑性樹脂である分子量80万〜100万の
PAA(ポリアクリルアミド)を使用し、第2バインダ
ーは、凝集性、耐水性を付与するため、網目状の三次元
構造を持った熱硬化性樹脂を用い、このうちEPA(ポ
リアミドポリアミンエピクロルヒドリン)を使用した。
Next, in the raw material mixing step B, the disentangled sepiolite, the first binder, the second binder, the softening agent,
Stabilizers are put in a mixing tank and mixed to prepare a slurry. The first binder used here is PAA (polyacrylamide) having a molecular weight of 800,000 to 1,000,000, which is a thermoplastic resin, in order to increase the paper strength, and the second binder imparts cohesiveness and water resistance. Therefore, a thermosetting resin having a three-dimensional network structure was used, and EPA (polyamide polyamine epichlorohydrin) was used among them.

【0025】なお、ここで、各バインダーを加える順序
としては、先に第1バインダーを添加し、その後、第2
バインダーを加えるのが望ましいが、必ずしもこれに限
定されるものではなく、先に第2バインダーを、後に第
1バインダーを混合しても抄紙可能である。
Here, the order of adding the respective binders is that the first binder is added first, and then the second binder is added.
It is desirable to add a binder, but the binder is not necessarily limited to this, and it is possible to make paper by mixing the second binder first and the first binder later.

【0026】原料混合工程Bで混合されたスラリーは、
処理工程Cで紙料集束化反応装置により集束化を行な
う。集束化においては、前記第1バインダー及び第2バ
インダーのスラリーへの定着を促進し、併せて、抄紙時
の濾水性を改良するために、分子量800万〜1000
万のアニオン系のPAAを加えた。
The slurry mixed in the raw material mixing step B is
In the processing step C, the paper stock is made into a bundle by a bundle focusing reaction device. In the bundling, in order to promote the fixing of the first binder and the second binder to the slurry and to improve the drainage property at the time of papermaking, the molecular weight is 8,000,000 to 1,000.
Tens of thousands of anionic PAAs were added.

【0027】処理工程Cで紙料化調製されたスラリー
は、ストックタンクに送出され、沈降分離または調製紙
料の崩壊等が生じないように、混合状態が常に均一化さ
れるように維持する蓄積工程Dに入る。
The slurry prepared as a stock in the processing step C is sent to a stock tank and accumulated so that the mixed state is always made uniform so that sedimentation separation or disintegration of the prepared stock does not occur. Enter the process D.

【0028】そして、蓄積工程Dで均一に維持されたス
ラリーは定量ホッパーに定量ポンプでポンプアップし、
定量ホッパーで計量されたスラリーは抄造工程Eに導か
れる。
Then, the slurry uniformly maintained in the accumulation step D is pumped up by a metering pump into a metering hopper,
The slurry measured by the quantitative hopper is guided to the papermaking process E.

【0029】本実施例の抄造工程Eでは、短網式抄紙機
を用いて抄造した。このときのスラリー濃度は0.5〜
1.0%であり、短網式抄紙機は60〜80メッシュの
抄網を使用した。この抄造工程Eにおいて、凝集フロッ
クが形成された前記分散水溶液を約80メッシュの網を
張った抄具に上方から流入すると、前記凝集フロックを
通して水が速やかに網から流下して紙層が形成される。
In the papermaking process E of this example, papermaking was performed using a short-net paper machine. The slurry concentration at this time is 0.5 to
1.0%, and the short-net paper machine used a 60-80 mesh net. In this papermaking step E, when the dispersed aqueous solution in which flocs are formed is flown into a papermaking machine having a mesh of about 80 mesh from above, water quickly flows down from the nets through the flocs to form a paper layer. It

【0030】この後、この紙層を、乾燥工程Fで、プレ
スをかけて脱水し、約120℃の雰囲気温度で所定時間
乾燥することにより、紙層は内部の水分が蒸発し、バイ
ンダーの凝縮が促進して乾燥固化される。そして、乾燥
された成形体はスチーム回転ドライヤーのドライヤー面
から剥離されて巻取紙に形成される。
Then, in the drying step F, the paper layer is dehydrated by pressing and dried at an ambient temperature of about 120 ° C. for a predetermined time, whereby the water content in the paper layer is evaporated and the binder is condensed. Is accelerated and dried and solidified. Then, the dried molded body is peeled off from the dryer surface of the steam rotary dryer to form a roll paper.

【0031】以上により、板厚が0.1〜1.0mmの不
燃性シートが完成する。この不燃シート性は高い耐熱性
を有し、火を接近させても僅かな発煙と黒色化するだけ
で、所定の形状を維持できる。
As described above, a nonflammable sheet having a plate thickness of 0.1 to 1.0 mm is completed. This non-combustible sheet has high heat resistance, and even if a fire is approached, only a slight amount of smoke and blackening can be maintained and a predetermined shape can be maintained.

【0032】次に、濾水性の改良を図るために行なうス
ラリーの集束化について説明する。凝集剤としては、セ
ピオライトの組成中の金属イオンであるカルシウムイオ
ンやマグネシウムイオンまたはカチオン物質と結合して
繊維と凝集結束する前述のアニオン系であるPAAを選
定した。セピオライトとPAAとの結合は、セピオライ
トのマグネシウムイオンとPAAのアミド基とが反発し
て直鎖状に伸びた橋架け構造も形成されていると考えら
れる。
Next, the bundling of the slurry to improve drainage will be described. As the aggregating agent, the above-mentioned anionic PAA that aggregates and binds with the fibers by binding with calcium ions or magnesium ions which are metal ions in the composition of sepiolite or a cation substance was selected. It is considered that the bond between sepiolite and PAA is such that a magnesium ion of sepiolite and the amide group of PAA repel each other to form a linear bridge structure.

【0033】本開発研究では、まず、このPAAの配合
割合について検討を行なった。
In the present development study, first, the blending ratio of PAA was examined.

【0034】処理条件としては、抄具150×150mm
判、抄網80メッシュを用い、原料はセピオライト85
重量%に補強材としてガラス繊維を15重量%加え、こ
の2.5gを100mlの水に解繊分散させた。これにカ
チオン系のEPA(ポリアミドポリアミンエピクロヒド
リン)を固定条件として各試料に固形分換算で2.0重
量%加え、PAAの配合量を図2の如く変えた。そし
て、抄紙濃度として2.5g/1000ml(0.25
%)に稀釈した後、この稀釈液1000mlの濾水時間を
測定することによって濾水性を判断した。
The processing conditions are as follows: paper making tool 150 × 150 mm
Size, 80 mesh, and raw material is Sepiolite 85
15% by weight of glass fiber was added to the weight% as a reinforcing material, and 2.5 g of this was disintegrated and dispersed in 100 ml of water. To this, cationic EPA (polyamide polyamine epichlorohydrin) was added as a fixed condition to each sample in an amount of 2.0% by weight in terms of solid content, and the compounding amount of PAA was changed as shown in FIG. The papermaking concentration is 2.5 g / 1000 ml (0.25
%), And then the freeness was judged by measuring the freezing time of 1000 ml of this diluted solution.

【0035】結果は、図2の本発明の一実施例における
不燃性シートのPAAによる変化を示す表図の通りで、
PAAを0.3重量%加えたものは濾水性は良いが、集
束塊が大きすぎて、紙の地合が悪い。したがって、0.
2重量%周辺が良い。
The results are shown in the table of FIG. 2, which shows the change due to PAA of the non-combustible sheet in one embodiment of the present invention.
Draft with 0.3% by weight of PAA has good drainage, but the bundles are too large and the texture of paper is poor. Therefore, 0.
Around 2% by weight is good.

【0036】次に、紙力増強剤の添加と濾水性について
述べる。
Next, the addition of the paper strengthening agent and the drainage will be described.

【0037】紙力増強剤として前述のごとく第1バイン
ダーのアニオンである分子量80万〜100万のPAA
(ポリアクリルアミド)を選定した。
PAA having a molecular weight of 800,000 to 1,000,000 which is an anion of the first binder as a paper-strengthening agent as described above.
(Polyacrylamide) was selected.

【0038】固定条件として、凝集用のPAAは前記の
試験によって濾水性の良い0.2重量%に、また、EP
Aは前記と同じく2.0重量%にした。処理条件は前記
に準じた。
As fixing conditions, PAA for flocculation was 0.2 wt% with good drainage by the above test, and EP
A was 2.0% by weight as above. The processing conditions were the same as above.

【0039】結果を図3に示す。図3は本発明の一実施
例における不燃性シートの紙力増強剤の添加と濾水性に
よる変化を示す表図である。
The results are shown in FIG. FIG. 3 is a table showing the change of the non-combustible sheet in one embodiment of the present invention due to the addition of the paper strength enhancer and the drainage.

【0040】供試した紙力増強用のPAAは高粘度であ
り、No. 4以上になると、凝集体がゲル化し、濾水性が
良くないので、1.0〜2.0重量%が好ましい。
The tested paper strength increasing PAA has a high viscosity, and when it is No. 4 or more, the aggregate is gelled and the drainage is not good, so 1.0 to 2.0% by weight is preferable.

【0041】次に、EPA(熱硬化性樹脂)の増減によ
る物性の傾向を調べた。
Next, the tendency of physical properties due to increase and decrease of EPA (thermosetting resin) was examined.

【0042】固定条件として、PAA(凝集用)は0.
2重量%に、PAA(紙力増強用)は2.0重量%にし
た。処理条件は前記に準じた。
As a fixed condition, PAA (for aggregation) was 0.
2% by weight, and PAA (for strengthening paper strength) was 2.0% by weight. The processing conditions were the same as above.

【0043】結果を図4に示す。図4は本発明の一実施
例における不燃性シートのEPAの増減による物性傾向
を示す表図である。
The results are shown in FIG. FIG. 4 is a table showing the physical property tendency of the non-combustible sheet according to one embodiment of the present invention as the EPA increases and decreases.

【0044】No. 5が最も湿潤引張強さが高く、EPA
としては、2.0重量%が好ましい。なお、2.0重量
%を越えると有機成分が多くなって不燃の意図から外れ
てくるので、2.0重量%を上限とした。
No. 5 has the highest wet tensile strength and is EPA
Is preferably 2.0% by weight. It should be noted that when the content exceeds 2.0% by weight, the amount of organic components increases and it deviates from the intent of non-combustion, so 2.0% by weight was set as the upper limit.

【0045】ところで、本試験においては、紙力強度を
より向上させるために、補強材であるガラス繊維を加え
ている。
By the way, in this test, in order to further improve the paper strength, glass fiber as a reinforcing material is added.

【0046】このガラス繊維について、セピオライトに
対する混合割合と繊維長を変え、強度及び濾水性を調べ
た。具体的には、繊維長として3、6、13mmを設定
し、それぞれについて混合割合を5、10、15、20
重量%と変えた。
With respect to this glass fiber, the mixing ratio to sepiolite and the fiber length were changed, and the strength and drainage were examined. Specifically, the fiber length is set to 3, 6, 13 mm, and the mixing ratio is 5, 10, 15, 20 for each.
Changed to% by weight.

【0047】その結果、繊維長は13mm、混合割合は1
5〜20重量%のものが強度及び濾水性を総合的に比較
して最も良かった。ガラス繊維はフィラーとして凝集を
促進する作用もあると考えられる。
As a result, the fiber length was 13 mm and the mixing ratio was 1.
Those having 5 to 20% by weight were the best in comprehensively comparing strength and drainage. It is considered that glass fiber also has a function of promoting aggregation as a filler.

【0048】耐水性について本発明の実施例の図4No.
4の試料と市販の試料(木材パルプと水酸化アルミ粉か
らなる水酸化アルミ紙)とを比較した事例を図5に示
す。
Regarding the water resistance, FIG. 4 No. of the embodiment of the present invention.
FIG. 5 shows an example in which the sample of No. 4 and a commercially available sample (aluminum hydroxide paper made of wood pulp and aluminum hydroxide powder) are compared.

【0049】図5は本発明の一実施例における不燃性シ
ートとの水中伸度を比較した表図である。
FIG. 5 is a table comparing the elongation in water with the noncombustible sheet in one example of the present invention.

【0050】縦方向については、1時間浸漬後と24時
間浸漬後のいずれにおいても本発明の実施例の試料と市
販の試料とで差はないが、横方向については本発明の実
施例の試料の伸びは明らかに少なく、総合的に本発明の
実施例の試料は優れた耐水性を示している。
Regarding the longitudinal direction, there is no difference between the sample of the example of the present invention and the commercially available sample after both 1-hour immersion and 24-hour immersion, but in the horizontal direction, the sample of the example of the present invention. The elongation of the samples is obviously small, and the samples of the examples of the present invention show excellent water resistance.

【0051】なお、市販の試料において縦と横の伸びが
著しく異なるのは、抄紙のときに、木材パルプの繊維配
向が縦に並び易く、繊維の絡み度合が大きくなって伸び
が小さくなるのて対し、横は繊維の絡み度合が小さいた
めに伸びは大きくなるためと考えられる。
In the commercially available sample, the longitudinal and lateral elongations are remarkably different from each other because the fiber orientation of wood pulp is easily aligned in the longitudinal direction during papermaking, and the degree of entanglement of fibers increases and the elongation decreases. On the other hand, it is considered that the elongation is large in the horizontal direction because the degree of entanglement of fibers is small.

【0052】一方、本発明の実施例の試料は、木材パル
プを使っておらず、セピオライトが主材で相対的に繊維
長が短いために、繊維方向性が小さく、かつ、微細なガ
ラス繊維が一体となった集束繊維を形成しているので、
縦と横の差が小さくなっていると考えられる。
On the other hand, the samples of the examples of the present invention did not use wood pulp, and since sepiolite was the main material and the fiber length was relatively short, the fiber orientation was small and fine glass fibers were formed. Since it forms an integrated bundle of fibers,
It is considered that the difference between the vertical and horizontal directions has become smaller.

【0053】このように、上記実施例の不燃性シート
は、主材としてのセピオライトと、補強材としての無機
繊維であるガラス繊維と、熱可塑性樹脂であるPAA
(ポリアクリルアミド)からなる第1バインダーと、熱
硬化性樹脂であるEPA(ポリアミドポリアミンエピク
ロルヒドリン)からなる第2バインダーとを必須成分と
したスラリーを抄造してなるものである。
As described above, the non-combustible sheet of the above-described embodiment has sepiolite as the main material, glass fiber as the inorganic fiber as the reinforcing material, and PAA as the thermoplastic resin.
It is made by making a slurry containing a first binder made of (polyacrylamide) and a second binder made of EPA (polyamide polyamine epichlorohydrin) which is a thermosetting resin as essential components.

【0054】したがって、上記実施例によれば、セピオ
ライトに第1バインダー及び第2バインダーを加えて抄
造した紙は、主成分が無機繊維であるセピオライトであ
ることにより、不燃性を有する。また、第1バインダー
のPAAはセピオライトの固着性に寄与し、紙の強度を
向上させることができる。
Therefore, according to the above embodiment, the paper made by adding the first binder and the second binder to sepiolite has nonflammability because the main component is sepiolite, which is the inorganic fiber. Further, PAA of the first binder contributes to the fixing property of sepiolite and can improve the strength of the paper.

【0055】更に、第2バインダーの熱硬化性樹脂であ
るEPAは、網目状の三次元構造をもった高分子化合物
であって原子が強い共有結合で結ばれているので、水に
対して安定で、紙に耐水性を与えるとともに、抄造にお
ける濾水性を向上させてシートの形成を容易にする。
Further, EPA, which is the thermosetting resin of the second binder, is a polymer compound having a network-like three-dimensional structure, and the atoms are bound by strong covalent bonds, so that it is stable to water. In addition, it imparts water resistance to the paper and improves drainage in papermaking to facilitate sheet formation.

【0056】また、補強材としてガラス繊維を混ぜたこ
とにより、更に強度物性を向上させることができる。
By mixing glass fiber as a reinforcing material, the strength and physical properties can be further improved.

【0057】そして、原料、バインダーとして、普及さ
れた材料を使用しているので、廉価に製造することがで
きる。
Since the widely used materials are used as the raw material and the binder, it can be manufactured at low cost.

【0058】なお、この実施例は請求項1及び請求項3
の態様に相当するものである。
In this embodiment, claims 1 and 3 are provided.
It corresponds to the embodiment of.

【0059】次に、別の実施例を説明する。Next, another embodiment will be described.

【0060】この別の実施例では、前記実施例の第1バ
インダー、第2バインダー及びアニオン系の熱可塑性樹
脂である凝集用のPAAにカチオン系の熱可塑性樹脂を
加え、前記凝集用のPAA(分子量800万〜1000
万)を第3バインダーとし、前記カチオン系の熱可塑性
樹脂を第4バインダーとしたものである。
In this another embodiment, a cationic thermoplastic resin is added to the aggregating PAA which is the first binder, the second binder and the anionic thermoplastic resin of the above embodiment, and the aggregating PAA ( Molecular weight 8 million to 1000
10,000) as the third binder and the cationic thermoplastic resin as the fourth binder.

【0061】これらの第3バインダー及び第4バインダ
ーは凝集剤として作用し、前記実施例で述べた第1バイ
ンダーと第2バインダーを加えて定着及び凝集したもの
に対して、更に、フロックを粗大化させて抄紙性を向上
させることができる。即ち、原料混合工程Bにおいて、
第1バインダー及び第2バインダーを前記実施例と同様
に加えた後、カチオンサイドになっているスラリーにア
ニオン系の熱可塑性樹脂である第3バインダーを混合し
てフロックを粗大化させ、次いで、カチオン系の凝集剤
である第4バインダーを加えて疎水性フロックとするこ
とにより、強固なフロックを形成させることができる。
The third binder and the fourth binder act as an aggregating agent, and the flocs are further coarsened with respect to those obtained by fixing and aggregating by adding the first binder and the second binder described in the above embodiment. It is possible to improve the papermaking property. That is, in the raw material mixing step B,
After adding the first binder and the second binder in the same manner as in the above example, the third binder, which is an anionic thermoplastic resin, is mixed with the slurry which is the cation side to coarsen the flocs, and then the cation. A strong floc can be formed by adding a fourth binder, which is a coagulant of the system, into a hydrophobic floc.

【0062】ここで、第3バインダーとしては、前述の
凝集用のPAAの他に、例えば、AA(アクリルアミド
アクリル酸共重合体)を、また、第4バインダーとして
は、例えば、DMAEM(ジメチルアミノエチルメタク
リレート)を挙げることができる。
The third binder may be, for example, AA (acrylamide / acrylic acid copolymer) in addition to the above-mentioned flocculating PAA, and the fourth binder may be, for example, DMAEM (dimethylaminoethyl). Methacrylate) can be mentioned.

【0063】各バインダーの配合量は、第1バインダー
が固形分換算で2重量%以下、第2バインダーが2重量
%以下、第3バインダー及び第4バインダーは原材料固
形分で合計0.2〜1.0重量%で、かつ、第3バイン
ダー及び第4バインダー中の第3バインダーの比率が2
5〜75%としたものが好ましい。
The blending amount of each binder is such that the first binder is 2% by weight or less in terms of solid content, the second binder is 2% by weight or less, and the third binder and the fourth binder are 0.2 to 1 in total in solid content of raw materials. 0.0% by weight, and the ratio of the third binder in the third binder and the fourth binder is 2
It is preferably 5 to 75%.

【0064】なお、この実施例においても、第1バイン
ダーと第2バインダーの添加順序は、第1バインダーが
先、第2バインダーは後が好ましいが、この逆であって
もよく、また、第3バインダーと第4バインダーとの間
の添加順序においても、第3バインダーが先が望ましい
が、その逆であっても抄紙可能である。
Also in this embodiment, the addition order of the first binder and the second binder is preferably such that the first binder is first and the second binder is second, but the order may be reversed, and the third binder may be added. Also in the order of addition between the binder and the fourth binder, the third binder is desirable first, but the reverse is also possible for papermaking.

【0065】この別の実施例は請求項2の態様に相当す
るものであるが、請求項3の態様に相当するとすること
もできる。
Although this another embodiment corresponds to the aspect of claim 2, it can also be considered to correspond to the aspect of claim 3.

【0066】ところで、上記実施例では、熱可塑性樹脂
からなる第1バインダーはPAAを、熱硬化性樹脂から
なる第2バインダーはEPAを、熱可塑性樹脂からなる
第3バインダーはAAを、熱可塑性樹脂からなる第4バ
インダーはDMAEMをそれぞれ使用しているが、本発
明を実施する場合には、これに限定されるものではな
く、それぞれ他の合成高分子、天然高分子を使用するこ
ともできる。そして、各熱可塑性樹脂及び熱硬化性樹脂
に用いる樹脂はそれぞれ1種類でもよく、或いは2種類
以上混合してもよい。
By the way, in the above embodiment, the first binder made of the thermoplastic resin is PAA, the second binder made of the thermosetting resin is EPA, the third binder made of the thermoplastic resin is AA, and the thermoplastic resin is the thermoplastic resin. DMAEM is used as each of the fourth binders consisting of, but the present invention is not limited to this, and other synthetic polymers and natural polymers can also be used. And the resin used for each thermoplastic resin and thermosetting resin may be one kind respectively, or two or more kinds may be mixed.

【0067】また、上記実施例におけるセピオライト、
凝集剤、補強材、補強繊維等の混合比率は、実施例に示
した比率に限定されるものではなく、物性、濾水性、製
法、用途等に応じて最適なものを選定すればよい。
Further, the sepiolite in the above embodiment,
The mixing ratio of the aggregating agent, the reinforcing material, the reinforcing fiber, etc. is not limited to the ratio shown in the examples, and an optimum one may be selected depending on the physical properties, drainage, manufacturing method, application and the like.

【0068】更に、上記実施例の不燃性シートは、補強
材としてガラス繊維を混ぜているが、本発明を実施する
場合には、これに限定されるものではなく、ロックウー
ル繊維、ステンレス繊維、ウィスカー等各種の補強材の
使用が可能である。但し、材料コスト、凝集効果等の点
からガラス繊維が最適である。なお、使用用途によって
は、補強材を必ずしも混ぜる必要はない。この種の発明
の実施例では、補強材の混合工程を省略でき、作業を簡
略化することができる。また、ガラス繊維を混入して固
い感じのする不燃性シートに対して、滑らかな風合を与
えることができる。同様に、補強繊維としての木材パル
プ、合成繊維についても必ずしも混ぜる必要はなく、抄
紙性、使用用途等を考慮して適宜使用すればよい。
Further, the non-combustible sheet of the above-mentioned embodiment is mixed with glass fiber as a reinforcing material. However, the present invention is not limited to this, and rock wool fiber, stainless fiber, Various reinforcing materials such as whiskers can be used. However, glass fiber is most suitable in terms of material cost, aggregation effect, and the like. Depending on the intended use, it is not always necessary to mix the reinforcing material. In this embodiment of the invention, the step of mixing the reinforcing material can be omitted and the work can be simplified. In addition, it is possible to give a smooth texture to a non-combustible sheet that is hard by mixing glass fibers. Similarly, it is not always necessary to mix the wood pulp as the reinforcing fiber and the synthetic fiber, and they may be appropriately used in consideration of paper-making properties, intended use and the like.

【0069】なお、本実施例の不燃性シートは、壁装
材、シール材、建築表装紙等への使用が可能であるが、
他にも、断熱材の両面に貼着することによって、断熱材
の繊維のケバ立ちや剥れ落ちを防止するような使い方も
できる。或いは、絶縁材として使用することもできる。
The non-combustible sheet of this embodiment can be used as a wall covering material, a sealing material, a building surface covering paper, etc.
In addition, it can be used by preventing the fibers of the heat insulating material from fluffing or peeling off by sticking it to both sides of the heat insulating material. Alternatively, it can be used as an insulating material.

【0070】また、不燃性シートの厚さは10mm程度に
抄造することもでき、更に、凹凸状に抄造することも可
能であるから、立体的な形状の不燃材としての使用も可
能である。
Further, since the nonflammable sheet can be made into a paper having a thickness of about 10 mm and further can be made into a concavo-convex shape, it can be used as a three-dimensionally shaped nonflammable material.

【0071】[0071]

【発明の効果】以上のように、請求項1の発明の不燃性
シートは、主材としてのセピオライトと、熱可塑性樹脂
からなる固着用の第1バインダーと、熱硬化性樹脂から
なる凝集、耐水用の第2バインダーとを必須成分とした
スラリーを抄造してなるものである。したがって、セピ
オライトに第1バインダー及び第2バインダーを加えて
抄造したシートは、主成分が無機繊維であるセピオライ
トであることにより、不燃性を有するとともに、廉価に
製造できる。また、第1バインダーの熱可塑性樹脂はセ
ピオライトの固着性に寄与し、シートの強度を向上す
る。更に、第2バインダーの熱硬化性樹脂であるEPA
は、網目状の三次元構造をもった高分子化合物であって
原子が強い共有結合で結ばれているので、水に対して安
定で、紙に耐水性を与えるとともに、抄造における濾水
性を向上させてシートの形成を容易にする。
As described above, the non-combustible sheet of the first aspect of the present invention comprises sepiolite as a main material, a first binder for fixing made of a thermoplastic resin, and an agglomerate, water resistant material made of a thermosetting resin. A second binder for use is made into paper by making a slurry containing the essential component. Therefore, the sheet produced by adding the first binder and the second binder to sepiolite has the non-flammability and can be manufactured at a low price because the main component is sepiolite. Moreover, the thermoplastic resin of the first binder contributes to the fixing property of sepiolite and improves the strength of the sheet. Furthermore, EPA, which is a thermosetting resin for the second binder
Is a polymer compound with a three-dimensional network structure and its atoms are bound by strong covalent bonds, so it is stable to water, imparts water resistance to paper, and improves drainage in papermaking. To facilitate the formation of the sheet.

【0072】また、請求項2の発明の不燃性シートは、
主材としてのセピオライトと、アニオン系の熱可塑性樹
脂からなる固着用の第1バインダーと、カチオン系の熱
硬化性樹脂からなる凝集、耐水用の第2バインダーと、
アニオン系の熱可塑性樹脂からなる凝集用の第3バイン
ダーと、カチオン系の熱可塑性樹脂からなる凝集用の第
4バインダーとを必須成分としたスラリーを抄造してな
るものである。したがって、第1バインダー及び第2バ
インダーを加えた後、カチオンサイドになっているスラ
リーにアニオン系の凝集剤である第3バインダーを加え
ると、フロックは粗大化し、次いで、カチオン系の凝集
剤である第4バインダーを加えると、前記フロックは疎
水化し、強固となる。これによって、濾水性は更に向上
する。
Further, the nonflammable sheet according to the invention of claim 2 is
Sepiolite as a main material, a first binder for fixation composed of an anionic thermoplastic resin, a second binder for aggregation and water resistance composed of a cation thermosetting resin,
This is made by paper-making a slurry containing a third aggregating binder made of an anionic thermoplastic resin and a fourth agglomerating binder made of a cationic thermoplastic resin as essential components. Therefore, when the third binder, which is an anionic flocculant, is added to the slurry that is the cation side after adding the first binder and the second binder, the flocs become coarse, and then the flocculant is a cationic flocculant. When the fourth binder is added, the flocs become hydrophobic and become strong. This further improves drainage.

【0073】更に、請求項3の発明の不燃性シートは、
請求項1または請求項2のスラリーに、補強材としての
無機繊維を必須成分として追加したものである。したが
って、更にシートの強度物性を向上することができる。
Further, the nonflammable sheet of the invention of claim 3 is
An inorganic fiber as a reinforcing material is added as an essential component to the slurry according to claim 1 or 2. Therefore, the strength and physical properties of the sheet can be further improved.

【図面の簡単な説明】[Brief description of drawings]

【図1】図1は本発明の一実施例における不燃性シート
の製造工程の概略を示す説明図である。
FIG. 1 is an explanatory view showing an outline of a manufacturing process of a non-combustible sheet according to an embodiment of the present invention.

【図2】図2は本発明の一実施例における不燃性シート
のPAAによる変化を示す表図である。
FIG. 2 is a table showing changes due to PAA of a nonflammable sheet in an example of the present invention.

【図3】図3は本発明の一実施例における不燃性シート
の紙力増強剤の添加と濾水性による変化を示す表図であ
る。
FIG. 3 is a table showing changes due to addition of a paper strength enhancer and drainage of a non-combustible sheet in one example of the present invention.

【図4】図4は本発明の一実施例における不燃性シート
のEPAの増減による物性傾向を示す表図である。
FIG. 4 is a table showing physical property trends due to increase / decrease in EPA of a nonflammable sheet in an example of the present invention.

【図5】図5は本発明の一実施例における不燃性シート
と市販の不燃性シートとの水中伸度を比較した表図であ
る。
FIG. 5 is a table comparing the underwater elongations of a non-combustible sheet and a commercially available non-combustible sheet in one example of the present invention.

【符号の説明】[Explanation of symbols]

A 解繊工程 B 原料混合工程 C 処理工程 D 蓄積工程 E 抄造工程 F 乾燥工程 A defibration process B raw material mixing process C treatment process D accumulation process E papermaking process F drying process

【手続補正書】[Procedure amendment]

【提出日】平成5年6月24日[Submission date] June 24, 1993

【手続補正1】[Procedure Amendment 1]

【補正対象書類名】図面[Document name to be corrected] Drawing

【補正対象項目名】図5[Name of item to be corrected] Figure 5

【補正方法】変更[Correction method] Change

【補正内容】[Correction content]

【図5】 [Figure 5]

Claims (3)

【特許請求の範囲】[Claims] 【請求項1】 主材としてのセピオライトと、熱可塑性
樹脂からなる固着用の第1バインダーと、熱硬化性樹脂
からなる凝集、耐水用の第2バインダーとを必須成分と
したスラリーを抄造してなることを特徴とする不燃性シ
ート。
1. A slurry containing, as essential components, sepiolite as a main material, a first binder for fixation made of a thermoplastic resin, and a second binder for aggregation and water resistance made of a thermosetting resin is made into paper. Non-combustible sheet characterized by being.
【請求項2】 主材としてのセピオライトと、アニオン
系の熱可塑性樹脂からなる固着用の第1バインダーと、
カチオン系の熱硬化性樹脂からなる凝集、耐水用の第2
バインダーと、アニオン系の熱可塑性樹脂からなる凝集
用の第3バインダーと、カチオン系の熱可塑性樹脂から
なる凝集用の第4バインダーとを必須成分としたスラリ
ーを抄造してなることを特徴とする不燃性シート。
2. Sepiolite as a main material, and a first binder for fixing which is made of an anionic thermoplastic resin,
The second for aggregation and water resistance, which consists of a cationic thermosetting resin
It is characterized in that a slurry is made into paper by using a binder, a third binder for aggregation made of an anionic thermoplastic resin, and a fourth binder for aggregation made of a cationic thermoplastic resin as essential components. Non-combustible sheet.
【請求項3】 前記スラリーに、補強材としての無機繊
維を必須成分として追加したことを特徴とする請求項1
または請求項2に記載の不燃性シート。
3. The inorganic fiber as a reinforcing material is added to the slurry as an essential component to the slurry.
Alternatively, the nonflammable sheet according to claim 2.
JP4032303A 1992-02-19 1992-02-19 Non-combustible sheet Expired - Lifetime JP2502236B2 (en)