JP5049150B2 - Shrink film and shrink label - Google Patents

Shrink film and shrink label Download PDF

Info

Publication number
JP5049150B2
JP5049150B2 JP2008018660A JP2008018660A JP5049150B2 JP 5049150 B2 JP5049150 B2 JP 5049150B2 JP 2008018660 A JP2008018660 A JP 2008018660A JP 2008018660 A JP2008018660 A JP 2008018660A JP 5049150 B2 JP5049150 B2 JP 5049150B2
Authority
JP
Japan
Prior art keywords
layer
shrink
film
resin
styrene
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP2008018660A
Other languages
Japanese (ja)
Other versions
JP2009178887A (en
Inventor
泰生 大瀬
規志 安田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Fuji Seal International Inc
Original Assignee
Fuji Seal International Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Fuji Seal International Inc filed Critical Fuji Seal International Inc
Priority to JP2008018660A priority Critical patent/JP5049150B2/en
Publication of JP2009178887A publication Critical patent/JP2009178887A/en
Application granted granted Critical
Publication of JP5049150B2 publication Critical patent/JP5049150B2/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、層間剥離しない、異種積層シュリンクフィルムに関する。また、該シュリンクフィルムに印刷層を設けたシュリンクラベルに関する。   The present invention relates to a heterogeneous laminated shrink film that does not delaminate. Moreover, it is related with the shrink label which provided the printing layer in this shrink film.

現在、お茶や清涼飲料水等の飲料用容器として、PETボトル(ポリエチレンテレフタレート製ボトル)などのプラスチック製ボトルや、ボトル缶等の金属製ボトル等が広く用いられている。これらの容器には、表示や装飾性、機能性の付与のためプラスチックラベルを装着する場合が多く、近年、容器に対する追従性が良好であり、表示面積を増大できる等のメリットから、水蒸気や熱風により収縮させることにより容器に追従・装着させる熱収縮性プラスチックフィルム(シュリンクフィルム)が広く使用されている。   Currently, plastic bottles such as PET bottles (polyethylene terephthalate bottles) and metal bottles such as bottle cans are widely used as containers for beverages such as tea and soft drinks. These containers are often equipped with plastic labels for display, decoration, and functionality. In recent years, water vapor and hot air have been used because of their good trackability and increased display area. A heat-shrinkable plastic film (shrink film) that is made to follow and attach to a container by being shrunk by is widely used.

上記シュリンクフィルムの分野においては、剛性、高収縮性、収縮加工性、美麗な仕上がり、低密度などの様々な特性を両立するため、またフィルムに印刷性、耐熱性、耐摩耗性や耐薬品性などの機能を付与する目的で、異なる樹脂素材を積層した異種積層フィルムが広く用いられている。例えば、ポリエステル系樹脂とポリスチレン系樹脂を積層させたシュリンクフィルムなどが知られている(例えば、特許文献1参照)。   In the field of shrink film, in order to achieve various properties such as rigidity, high shrinkage, shrink workability, beautiful finish, low density, etc., the film has printability, heat resistance, wear resistance and chemical resistance. For the purpose of imparting functions such as these, different types of laminated films in which different resin materials are laminated are widely used. For example, a shrink film in which a polyester resin and a polystyrene resin are laminated is known (see, for example, Patent Document 1).

しかしながら、上記ポリスチレン系樹脂層、ポリエステル系樹脂層および接着層からなる積層フィルムは、センターシール工程では十分なシール強度を発揮するが、シュリンク加工(収縮加工)によりボトルに装着した場合には、センターシール部分が層間剥離する問題が生じていた。即ち、異種積層のシュリンクフィルムにおいて、実用上十分な層間強度(フィルム層間の接着強度)を有するシュリンクフィルムは得られていないのが現状である。   However, the laminated film composed of the above-mentioned polystyrene resin layer, polyester resin layer and adhesive layer exhibits sufficient sealing strength in the center sealing process, but when it is attached to the bottle by shrink processing (shrink processing), There has been a problem that the seal portion is delaminated. That is, in the present invention, a shrink film having a practically sufficient interlayer strength (adhesive strength between film layers) has not been obtained for different types of shrink films.

特開2006−15745号公報JP 2006-15745 A

本発明の目的は、ポリスチレン系樹脂とポリエステル系樹脂の異種ポリマーの積層シュリンクフィルムにおいて、層間剥離しないシュリンクフィルムを提供することにある。また、該シュリンクフィルムを用いたシュリンクラベルを提供することにある。   An object of the present invention is to provide a shrink film that does not delaminate in a laminated shrink film of different polymers of a polystyrene resin and a polyester resin. Another object of the present invention is to provide a shrink label using the shrink film.

本発明者らは、上記目的を達成するため鋭意検討した結果、非晶性の芳香族ポリエステル系樹脂および可塑剤を特定配合量で含有する表面層(A層)、および、スチレン−共役ジエン共重合体及び/又はその水添物を主成分とする中心層(B層)が、A層/B層/A層の順に積層された少なくとも3層の積層構造を有するシュリンクフィルムとすることにより、優れた層間強度を有する異種積層フィルムを得ることができることを見出し、本発明を完成した。   As a result of intensive studies to achieve the above object, the present inventors have found that a surface layer (A layer) containing an amorphous aromatic polyester resin and a plasticizer in a specific blending amount, and a styrene-conjugated diene copolymer. By making the center layer (B layer) whose main component is a polymer and / or its hydrogenated product into a shrink film having a laminated structure of at least three layers laminated in the order of A layer / B layer / A layer, The present inventors have found that a heterogeneous laminated film having excellent interlayer strength can be obtained, and the present invention has been completed.

すなわち、本発明は、非晶性芳香族ポリエステル系樹脂を主成分とし、非晶性芳香族ポリエステル系樹脂100重量部に対して可塑剤0.5〜20重量部を含有する樹脂組成物から構成される表面層(A層)、および、スチレン−共役ジエン共重合体及び/又はその水添物を主成分とする樹脂組成物から構成される中心層(B層)が、A層/B層/A層の順に積層された少なくとも3層積層構造を有することを特徴とするシュリンクフィルムを提供する。   That is, the present invention is composed of a resin composition containing an amorphous aromatic polyester resin as a main component and 0.5 to 20 parts by weight of a plasticizer with respect to 100 parts by weight of an amorphous aromatic polyester resin. And a central layer (B layer) composed of a resin composition mainly composed of a styrene-conjugated diene copolymer and / or a hydrogenated product thereof is an A layer / B layer. A shrink film having at least a three-layer laminated structure in the order of / A layers is provided.

さらに、本発明は、接着性樹脂層(C層)を有し、A層/C層/B層/C層/A層の順に積層された少なくとも5層積層構造を有する前記のシュリンクフィルムを提供する。   Furthermore, the present invention provides the above shrink film having an adhesive resin layer (C layer) and having at least a five-layer laminated structure in which A layer / C layer / B layer / C layer / A layer are laminated in this order. To do.

さらに、本発明は、前記可塑剤がフタル酸エステル、アジピン酸エステル、ポリエステル系可塑剤から選ばれた少なくとも1つである前記のシュリンクフィルムを提供する。   Furthermore, the present invention provides the shrink film, wherein the plasticizer is at least one selected from phthalic acid esters, adipic acid esters, and polyester plasticizers.

さらに、本発明は、前記C層が、極性基を有するスチレン系樹脂より構成される前記のシュリンクフィルムを提供する。   Furthermore, this invention provides the said shrink film in which the said C layer is comprised from the styrene resin which has a polar group.

さらに、本発明は、前記のシュリンクフィルムの少なくとも一方の面側に印刷層を設けたシュリンクラベルを提供する。   Furthermore, this invention provides the shrink label which provided the printing layer in the at least one surface side of the said shrink film.

本発明のシュリンクフィルムは、表面層であるポリエステル系樹脂層の収縮応力を低減し、中心層との収縮応力の差を小さくしたため、シュリンク加工を施した後にも層間剥離によるトラブルが生じない。このため、PETボトルなどの容器に装着するシュリンクラベルとして有用である。   The shrink film of the present invention reduces the shrinkage stress of the polyester-based resin layer, which is the surface layer, and reduces the difference in shrinkage stress from the center layer, so that troubles due to delamination do not occur even after shrink processing. For this reason, it is useful as a shrink label attached to a container such as a PET bottle.

以下に、本発明のシュリンクフィルムについて、さらに詳細に説明する。   Below, the shrink film of this invention is demonstrated in detail.

本発明のシュリンクフィルムは、非晶性の芳香族ポリエステル系樹脂を主成分とし、さらに可塑剤を含有する樹脂組成物から構成される表面層(以下、「A層」と称する)、スチレン−共役ジエン共重合体及び/又はその水添物を主成分とする樹脂組成物から構成される中心層(以下、「B層」と称する)を少なくとも有する。さらに、接着性樹脂層(以下、「C層」と称する)を有していてもよい。なお、本発明にいう「主成分とする」とは、特に限定がない限り、それぞれの樹脂組成物中の含有量が、樹脂組成物の総重量に対して50重量%以上であることをいい、より好ましくは60重量%以上であることをいう。   The shrink film of the present invention is a surface layer (hereinafter referred to as “A layer”) composed of a resin composition containing an amorphous aromatic polyester resin as a main component and further containing a plasticizer, styrene-conjugated. It has at least a central layer (hereinafter referred to as “B layer”) composed of a resin composition mainly composed of a diene copolymer and / or a hydrogenated product thereof. Furthermore, an adhesive resin layer (hereinafter referred to as “C layer”) may be included. The term “main component” as used in the present invention means that the content in each resin composition is 50% by weight or more based on the total weight of the resin composition unless otherwise specified. More preferably, it means 60% by weight or more.

本発明のシュリンクフィルムは、上記A、B層が、A層(表面層)/B層(中心層)/A層(表面層)の順に積層された2種3層の積層構造を少なくとも有している。なお、上記A層とB層は、他の層を介さずに積層されていてもよいし、C層(接着性樹脂層)やその他の層を介して積層されていてもよい。本発明のシュリンクフィルムがC層を含む場合には、A層/C層/B層/C層/A層の順に積層された3種5層の積層構造であることが好ましい。なお、B層の両側に設けられたA層、C層は、それぞれ同一の樹脂組成からなる層であってもよいし、異なる組成の層(例えば、A1層とA2層)であってもよい。本発明のシュリンクフィルムは、さらに上記積層フィルムの製膜工程でインラインで設けることができる層であれば、上記A〜C層以外の層を有していてもよい。このような層としては、例えば、アンカーコート層、易接着層、帯電防止剤層などのコーティング層が挙げられる。   The shrink film of the present invention has at least a two-layer / three-layer structure in which the A and B layers are laminated in the order of A layer (surface layer) / B layer (center layer) / A layer (surface layer). ing. In addition, the A layer and the B layer may be laminated without interposing other layers, or may be laminated via a C layer (adhesive resin layer) or other layers. When the shrink film of this invention contains C layer, it is preferable that it is a 3 type | mold 5 layer laminated structure laminated | stacked in order of A layer / C layer / B layer / C layer / A layer. The A layer and the C layer provided on both sides of the B layer may be layers having the same resin composition, or layers having different compositions (for example, A1 layer and A2 layer). . If the shrink film of this invention is a layer which can be further provided in-line in the film forming process of the said laminated | multilayer film, you may have layers other than said AC layer. Examples of such a layer include coating layers such as an anchor coat layer, an easy adhesion layer, and an antistatic agent layer.

[表面層(A層)]
本発明のシュリンクフィルムにおける表面層(A層)は、非晶性の芳香族ポリエステル系樹脂を主成分し、さらに可塑剤を少なくとも含有する樹脂組成物(以下、「樹脂組成物A」と称する場合がある)から構成される。
[Surface layer (A layer)]
The surface layer (A layer) in the shrink film of the present invention is a resin composition (hereinafter, referred to as “resin composition A”) containing an amorphous aromatic polyester resin as a main component and further containing at least a plasticizer. Are).

上記非晶性の芳香族ポリエステル系樹脂(以下、単に「非晶性ポリエステル系樹脂」と称する場合がある)は、実質的に非晶性であれば、特に限定されず、例えば、ジカルボン酸成分とジオール成分とで構成される種々のポリエステルが挙げられる。なお、芳香族ポリエステル系樹脂であるため、全ジカルボン酸成分中の50モル%以上(好ましくは70モル%以上)が芳香族ジカルボン酸、および/または、全ジオール成分中の50モル%以上(好ましくは70モル%以上)が芳香族ジオールである必要がある。   The amorphous aromatic polyester-based resin (hereinafter, sometimes simply referred to as “amorphous polyester-based resin”) is not particularly limited as long as it is substantially amorphous. For example, a dicarboxylic acid component And various polyesters composed of diol components. In addition, since it is an aromatic polyester-based resin, 50 mol% or more (preferably 70 mol% or more) in the total dicarboxylic acid component is 50 mol% or more (preferably in the total diol component). 70 mol% or more) must be an aromatic diol.

ジカルボン酸成分としては、例えば、テレフタル酸、イソフタル酸、フタル酸、5−t−ブチルイソフタル酸、4,4’−ビフェニルジカルボン酸、トランス−3,3’−スチルベンジカルボン酸、トランス−4,4’−スチルベンジカルボン酸、4,4’−ジベンジルジカルボン酸、1,4−ナフタレンジカルボン酸、1,5−ナフタレンジカルボン酸、2,3−ナフタレンジカルボン酸、2,6−ナフタレンジカルボン酸、2,7−ナフタレンジカルボン酸、2,2,6,6−テトラメチルビフェニル−4,4’−ジカルボン酸、1,1,3−トリメチル−3−フェニルインデン−4,5−ジカルボン酸、1,2−ジフェノキシエタン−4,4’−ジカルボン酸、ジフェニルエーテルジカルボン酸、及びこれらの置換体等の芳香族ジカルボン酸;シュウ酸、マロン酸、コハク酸、グルタル酸、アジピン酸、ピメリン酸、スベリン酸、アゼライン酸、セバシン酸、ウンデカン二酸、ドデカン二酸、トリデカン二酸、テトラデカン二酸、ペンタデカン二酸、ヘプタデカン二酸、オクタデカン二酸、ノナデカン二酸、イコサン二酸、ドコサン二酸、1,12−ドデカンジオン酸、及びこれらの置換体等の脂肪族ジカルボン酸;1,4−デカヒドロナフタレンジカルボン酸、1,5−デカヒドロナフタレンジカルボン酸、2,6−デカヒドロナフタレンジカルボン酸、シス−1,4−シクロヘキサンジカルボン酸、トランス−1,4−シクロヘキサンジカルボン酸、1,3−シクロヘキサンジカルボン酸、及びこれらの置換体等の脂環式ジカルボン酸などが挙げられる。これらのジカルボン酸成分は、単独で又は2種以上組み合わせて使用できる。   Examples of the dicarboxylic acid component include terephthalic acid, isophthalic acid, phthalic acid, 5-t-butylisophthalic acid, 4,4′-biphenyldicarboxylic acid, trans-3,3′-stilbene dicarboxylic acid, and trans-4,4. '-Stilbene dicarboxylic acid, 4,4'-dibenzyldicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2, 7-naphthalenedicarboxylic acid, 2,2,6,6-tetramethylbiphenyl-4,4′-dicarboxylic acid, 1,1,3-trimethyl-3-phenylindene-4,5-dicarboxylic acid, 1,2- Aromatic dicals such as diphenoxyethane-4,4′-dicarboxylic acid, diphenyl ether dicarboxylic acid, and substituted products thereof Acid; oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, Aliphatic dicarboxylic acids such as heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, icosanedioic acid, docosanedioic acid, 1,12-dodecanedioic acid, and their substitutions; 1,4-decahydronaphthalenedicarboxylic acid, 1,5-decahydronaphthalenedicarboxylic acid, 2,6-decahydronaphthalenedicarboxylic acid, cis-1,4-cyclohexanedicarboxylic acid, trans-1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and these And alicyclic dicarboxylic acids such as substitution products thereof. These dicarboxylic acid components can be used alone or in combination of two or more.

ジオール成分としては、例えば、エチレングリコール、ジエチレングリコール、1,2−プロパンジオール、1,3−プロパンジオール、1,3−ブタンジオール、1,4−ブタンジオール、1,5−ペンタンジオール、2,2−ジメチル−1,3−プロパンジオール(ネオペンチルグリコール)、1,6−ヘキサンジオール、2−エチル−2−メチル−1,3−プロパンジオール、2,2−ジエチル−1,3−プロパンジオール、1,8−オクタンジオール、2−エチル−2−ブチル−1,3−プロパンジオール、2−エチル−2,4−ジメチル−1,3−ヘキサンジオール、1,10−デカンジオール、ポリエチレングリコール、ポリプロピレングリコール等の脂肪族ジオール;1,2−シクロヘキサンジメタノール、1,3−シクロヘキサンジメタノール、1,4−シクロヘキサンジメタノール、2,2,4,4−テトラメチル−1,3−シクロブタンジオール等の脂環式ジオール;2,2−ビス(4’−β−ヒドロキシエトキシジフェニル)プロパン、ビス(4’−β−ヒドロキシエトキシフェニル)スルホン等のビスフェノール系化合物のエチレンオキシド付加物、キシリレングリコール等の芳香族ジオールなどが挙げられる。これらのジオール成分は単独で又は2種以上を組み合わせて使用できる。   Examples of the diol component include ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 2,2 -Dimethyl-1,3-propanediol (neopentyl glycol), 1,6-hexanediol, 2-ethyl-2-methyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 1,8-octanediol, 2-ethyl-2-butyl-1,3-propanediol, 2-ethyl-2,4-dimethyl-1,3-hexanediol, 1,10-decanediol, polyethylene glycol, polypropylene Aliphatic diols such as glycol; 1,2-cyclohexanedimethanol, 1,3-cyclohexane Cycloaliphatic diols such as sandimethanol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol; 2,2-bis (4′-β-hydroxyethoxydiphenyl) Examples thereof include ethylene oxide adducts of bisphenol compounds such as propane and bis (4′-β-hydroxyethoxyphenyl) sulfone, and aromatic diols such as xylylene glycol. These diol components can be used alone or in combination of two or more.

上記非晶性ポリエステル系樹脂は、上記以外にも、p−オキシ安息香酸、p−オキシエトキシ安息香酸等のオキシカルボン酸;安息香酸、ベンゾイル安息香酸等のモノカルボン酸;トリメリット酸等の多価カルボン酸;ポリアルキレングリコールモノメチルエーテル等の1価アルコール;グリセリン、ペンタエリスリトール、トリメチロールプロパン等の多価アルコールなどの構成単位を含んでいてもよい。   In addition to the above, the amorphous polyester-based resin may include oxycarboxylic acids such as p-oxybenzoic acid and p-oxyethoxybenzoic acid; monocarboxylic acids such as benzoic acid and benzoylbenzoic acid; A structural unit such as a monovalent alcohol such as a polyvalent carboxylic acid; a monohydric alcohol such as polyalkylene glycol monomethyl ether; a polyhydric alcohol such as glycerin, pentaerythritol, or trimethylolpropane may be included.

非晶性ポリエステル系樹脂としては、上記の中でも、ジカルボン酸成分としてテレフタル酸、ジオール成分としてエチレングリコール(EG)を用いたポリエチレンテレフタレート(PET)において、ジカルボン酸成分及び/又はジオール成分の一部を他のジカルボン酸成分及び/又はジオール成分に置き換えた変性PETが好ましく例示される。上記変性PETに用いられるジカルボン酸成分としては、例えば、シクロヘキサンジカルボン酸、アジピン酸、イソフタル酸などが挙げられる。また、ジオール成分としては、1,4−シクロヘキサンジメタノール(CHDM)、ネオペンチルグリコール(NPG)、ジエチレングリコールなどが挙げられる。   As an amorphous polyester resin, among the above, in polyethylene terephthalate (PET) using terephthalic acid as the dicarboxylic acid component and ethylene glycol (EG) as the diol component, a part of the dicarboxylic acid component and / or diol component is used. Preferred examples include modified PET substituted with other dicarboxylic acid components and / or diol components. Examples of the dicarboxylic acid component used in the modified PET include cyclohexane dicarboxylic acid, adipic acid, and isophthalic acid. Examples of the diol component include 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG), and diethylene glycol.

上記変性PETとしては、具体的には、ジカルボン酸成分としてテレフタル酸を用い、ジオール成分としてEGを主成分、CHDMを共重合成分として用いた共重合ポリエステル(以後、CHDM共重合PET又はCHDM変性PETという)やネオペンチルグリコール(NPG)を共重合成分として用いた共重合ポリエステル(以後、NPG共重合PET又はNPG変性PETという)が、コスト、生産性等の観点で好ましい。さらに、低温収縮性向上の観点で、ジエチレングリコールを共重合していてもよい。   Specifically, as the modified PET, terephthalic acid is used as the dicarboxylic acid component, EG as the diol component, and copolyester using CHDM as the copolymer component (hereinafter referred to as CHDM copolymerized PET or CHDM modified PET). And copolyesters using neopentyl glycol (NPG) as a copolymerization component (hereinafter referred to as NPG copolymerized PET or NPG-modified PET) are preferred from the viewpoints of cost, productivity, and the like. Furthermore, diethylene glycol may be copolymerized from the viewpoint of improving low-temperature shrinkage.

上記変性PETにおいて、変性に用いる共重合成分の共重合比率(全ジカルボン酸成分に対する共重合ジカルボン酸成分の比率、または、全ジオール酸成分に対する共重合ジオール酸成分の比率)は、層間強度を一層向上させる観点から、15モル%以上(例えば、15〜40モル%)が好ましい。中でも、例えば、CHDM共重合PETの場合、CHDMの共重合の割合は、ジオール成分中(即ち、テレフタル酸100モル%に対して)、20〜40モル%(EGが60〜80モル%)が好ましく、さらに好ましくは25〜35モル%(EGが65〜75モル%)である。また、NPG共重合PETの場合、ジオール成分中、15〜40モル%(EGが60〜85モル%)が好ましい。また、さらにEG成分の一部(好ましくは、10モル%以下)をジエチレングリコールに置き換えてもよい。   In the modified PET, the copolymerization ratio of the copolymerization component used for modification (the ratio of the copolymerized dicarboxylic acid component to the total dicarboxylic acid component or the ratio of the copolymerized diolic acid component to the total diolic acid component) further increases the interlayer strength. From the viewpoint of improvement, 15 mol% or more (for example, 15 to 40 mol%) is preferable. Among them, for example, in the case of CHDM copolymerized PET, the proportion of CHDM copolymerization is 20 to 40 mol% (EG is 60 to 80 mol%) in the diol component (that is, with respect to 100 mol% of terephthalic acid). More preferably, it is 25-35 mol% (EG is 65-75 mol%). Moreover, in the case of NPG copolymerized PET, 15-40 mol% (EG is 60-85 mol%) in a diol component is preferable. Further, a part (preferably 10 mol% or less) of the EG component may be replaced with diethylene glycol.

上述のように、ポリエステルを変性し非晶性とすることにより、A層とB層又はC層の溶融温度での流動挙動を近づけることができるため、層の成型性及び層間強度が向上する。   As described above, by modifying the polyester to be amorphous, the flow behavior at the melting temperature of the A layer and the B layer or the C layer can be made closer, so that the moldability and interlayer strength of the layer are improved.

上記非晶性ポリエステル系樹脂の、示差走査熱量測定(DSC)法(10℃/分の昇温スピードで測定)により測定した結晶化度は、15%以下が好ましく、より好ましくは10%以下である。さらに、上記DSC法による融点(融解ピーク)がほとんど見うけられないもの(すなわち、結晶化度0%)が最も好ましい。上記、結晶化度は、DSC測定より得られる結晶融解熱の値から、X線法等により固定した結晶化度の明確なサンプルを標準として、算出することができる。なお、結晶融解熱は、例えば、セイコーインスツルメンツ社製DSC(示差走査熱量測定)装置を用い、試料量10mg、昇温速度10℃/分で、窒素シールを行い、一度融点以上まで昇温し、常温まで降温した後、再度昇温したときの融解ピークの面積から求めることができる。結晶化度は、単一の樹脂から測定されることが好ましいが、混合状態で測定される場合には、混合される樹脂の融解ピークを差し引いて、対象となるポリエステル系樹脂の融解ピークを求めればよい。   The degree of crystallinity of the amorphous polyester resin measured by the differential scanning calorimetry (DSC) method (measured at a heating rate of 10 ° C./min) is preferably 15% or less, more preferably 10% or less. is there. Further, the one that hardly shows the melting point (melting peak) by the DSC method (that is, the degree of crystallinity is 0%) is most preferable. The crystallinity can be calculated from the value of heat of crystal fusion obtained by DSC measurement using a sample with a clear crystallinity fixed by the X-ray method or the like as a standard. The heat of crystal melting is, for example, using a DSC (differential scanning calorimetry) device manufactured by Seiko Instruments Inc., performing a nitrogen seal at a sample amount of 10 mg and a heating rate of 10 ° C./min. The temperature can be determined from the area of the melting peak when the temperature is lowered to room temperature and then raised again. The crystallinity is preferably measured from a single resin, but when measured in a mixed state, the melting peak of the target polyester resin can be obtained by subtracting the melting peak of the resin to be mixed. That's fine.

上記非晶性ポリエステル系樹脂の重量平均分子量は、溶融挙動を好ましい範囲に制御する観点から、50000〜90000が好ましく、より好ましくは60000〜80000である。さらに、NPG共重合PETの場合、50000〜80000が好ましく、より好ましくは60000〜70000である。   The weight average molecular weight of the amorphous polyester resin is preferably 50000 to 90000, more preferably 60000 to 80000, from the viewpoint of controlling the melting behavior within a preferable range. Furthermore, in the case of NPG copolymerized PET, it is preferably 50000 to 80000, more preferably 60000 to 70000.

上記非晶性ポリエステル系樹脂のIV値(固有粘度)は、層間強度の観点から、0.70(dl/g)以上が好ましく、より好ましくは0.7〜0.9(dl/g)、さらに好ましくは0.75〜0.85(dl/g)である。また、非晶性ポリエステル系樹脂のガラス転移温度(Tg)は、収縮適性の観点から、70〜100℃が好ましく、より好ましくは70〜85℃である。   The IV value (intrinsic viscosity) of the amorphous polyester resin is preferably 0.70 (dl / g) or more, more preferably 0.7 to 0.9 (dl / g), from the viewpoint of interlayer strength. More preferably, it is 0.75-0.85 (dl / g). In addition, the glass transition temperature (Tg) of the amorphous polyester resin is preferably 70 to 100 ° C, more preferably 70 to 85 ° C, from the viewpoint of shrinkage suitability.

上記の非晶性ポリエステル系樹脂としては、既存品を用いることも可能であり、例えば、Eastman Chemical社製「Eastar Copolyester」、「EMBRACE」(以上、CHDM共重合PET);ベルポリエステルプロダクツ(株)製「ベルペット」(NPG共重合PETなど)等が市場で入手できる。   As the amorphous polyester-based resin, existing products can be used. For example, “Easter Polymer”, “EMBRACE” (above, CHDM copolymerized PET) manufactured by Eastman Chemical; Bell Polyester Products Co., Ltd. “Bellepet” (NPG copolymerized PET, etc.) manufactured by the Company is available on the market.

本発明のA層を構成する樹脂組成物(樹脂組成物A)の総重量に対する上記非晶性ポリエステル系樹脂の含有量は、収縮性及び印刷適性の観点から、50〜99.5重量%が好ましく、より好ましくは80〜99.5重量%である。   The content of the amorphous polyester resin relative to the total weight of the resin composition (resin composition A) constituting the A layer of the present invention is 50 to 99.5% by weight from the viewpoint of shrinkage and printability. Preferably, it is 80 to 99.5% by weight.

上記可塑剤は、ポリエステル系樹脂に通常用いられるものを使用可能で、特に限定されないが、例えば、フタル酸エステル、アセチル化モノグリセリド、アジピン酸エステル、ポリエステル系可塑剤などが例示される。中でも、柔軟性、相溶性の観点から、好ましくはフタル酸エステル、アジピン酸エステルである。フタル酸エステルとしては、例えば、フタル酸ジオクチル(DOP)、フタル酸ジイソノニル(DINP)、フタル酸ジイソデシル(DIDP)、フタル酸ジブチル(DBP)などが挙げられる。アジピン酸エステルとしては、例えば、アジピン酸ジオクチル(DOA)、アジピン酸ジイソノニル(DINA)などが挙げられる。ポリエステル系可塑剤としては、例えば、アジピン酸成分と脂肪族ジオール成分から構成されるポリエステルなどが挙げられる。   As the plasticizer, those usually used for polyester resins can be used, and are not particularly limited. Examples thereof include phthalic acid esters, acetylated monoglycerides, adipic acid esters, and polyester plasticizers. Among these, from the viewpoints of flexibility and compatibility, phthalic acid esters and adipic acid esters are preferable. Examples of the phthalic acid ester include dioctyl phthalate (DOP), diisononyl phthalate (DINP), diisodecyl phthalate (DIDP), and dibutyl phthalate (DBP). Examples of adipic acid esters include dioctyl adipate (DOA) and diisononyl adipate (DINA). Examples of the polyester plasticizer include polyester composed of an adipic acid component and an aliphatic diol component.

A層に用いられる芳香族ポリエステル系樹脂は、B層又はC層を形成するスチレン−共役ジエン共重合体などのポリスチレン系樹脂に比べて、一般的に収縮応力が大きく、これに起因してシュリンク加工の際にA層とB層又はC層間に収縮応力の差が生じて、層間強度が低下しやすくなる。A層中に上記可塑剤を添加することにより、A層を形成する樹脂に柔軟性を付与し収縮応力を低下させることができるため、層間強度が向上する。   The aromatic polyester resin used for the A layer generally has a larger shrinkage stress than the polystyrene resin such as the styrene-conjugated diene copolymer forming the B layer or the C layer, and shrinkage is caused thereby. During processing, a difference in shrinkage stress occurs between the A layer and the B layer or the C layer, and the interlayer strength tends to decrease. By adding the plasticizer to the A layer, flexibility can be imparted to the resin forming the A layer and the shrinkage stress can be reduced, so that the interlayer strength is improved.

上記可塑剤のA層中の含有量は、A層に用いられる非晶性芳香族ポリエステル系樹脂100重量部に対して、0.5〜20重量部であり、好ましくは10〜20重量部、さらに好ましくは12〜18重量部である。含有量が0.5重量部未満の場合には層間強度向上の効果が小さく、20重量部を超えると可塑剤がフィルム表面にブリードしてブロッキングや印刷性低下を招く。   The content of the plasticizer in the A layer is 0.5 to 20 parts by weight, preferably 10 to 20 parts by weight, based on 100 parts by weight of the amorphous aromatic polyester resin used in the A layer. More preferably, it is 12-18 weight part. When the content is less than 0.5 parts by weight, the effect of improving the interlayer strength is small, and when it exceeds 20 parts by weight, the plasticizer bleeds to the film surface, leading to blocking and printability deterioration.

A層には、必要に応じてその他の添加剤、例えば、滑剤、充填剤、熱安定剤、酸化防止剤、紫外線吸収剤、帯電防止剤、難燃剤、着色剤、ピニング剤(アルカリ土類金属)等を含んでいてもよい。   For layer A, if necessary, other additives such as lubricants, fillers, heat stabilizers, antioxidants, ultraviolet absorbers, antistatic agents, flame retardants, colorants, pinning agents (alkaline earth metals) ) And the like.

[中心層(B層)]
本発明のシュリンクフィルムにおける中心層(B層)は、スチレン−共役ジエン共重合体及び/又はその水添物を主成分とする樹脂組成物(以下、「樹脂組成物B」と称する場合がある)から構成される。
[Center layer (B layer)]
The central layer (B layer) in the shrink film of the present invention may be referred to as a resin composition (hereinafter referred to as “resin composition B”) containing a styrene-conjugated diene copolymer and / or a hydrogenated product thereof as a main component. ).

上記スチレン−共役ジエン共重合体は、スチレン系単量体および共役ジエンを必須の単量体成分として構成される共重合体である。   The styrene-conjugated diene copolymer is a copolymer composed of a styrene monomer and a conjugated diene as essential monomer components.

上記スチレン系単量体としては、特に限定されないが、例えば、スチレン、α−メチルスチレン、m−メチルスチレン、p−メチルスチレン、p−エチルスチレン、p−イソブチルスチレン、p−t−ブチルスチレン、クロロメチルスチレンなどが挙げられる。中でも、強度、成型性などの物性の観点から、スチレンが特に好ましい。なお、これらスチレン系単量体は、単独で用いてもよいし、2種以上を併用してもよい。   Although it does not specifically limit as said styrene-type monomer, For example, styrene, alpha-methyl styrene, m-methyl styrene, p-methyl styrene, p-ethyl styrene, p-isobutyl styrene, pt-butyl styrene, Examples include chloromethylstyrene. Among these, styrene is particularly preferable from the viewpoint of physical properties such as strength and moldability. In addition, these styrenic monomers may be used independently and may use 2 or more types together.

上記共役ジエンとしては、特に限定されないが、例えば、1,3−ブタジエン、イソプレン(2−メチル−1,3−ブタジエン)、2,3−ジメチル−1,3−ブタジエン、1,3−ペンタジエン、1,3−ヘキサジエン、クロロプレンなどが挙げられる。中でも、脆性改良、柔軟性付与の観点から、1,3−ブタジエン、イソプレンが特に好ましい。なお、これら共役ジエンは、単独で用いてもよいし、2種以上を併用してもよい。   The conjugated diene is not particularly limited. For example, 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, Examples include 1,3-hexadiene and chloroprene. Among these, 1,3-butadiene and isoprene are particularly preferable from the viewpoints of improving brittleness and imparting flexibility. In addition, these conjugated dienes may be used independently and may use 2 or more types together.

上記スチレン−共役ジエン共重合体において、上記スチレン系単量体の含有量は、単量体成分の全重量に対して、60〜95重量%が好ましく、より好ましくは70〜85重量%である。一方、上記共役ジエンの含有量は、単量体成分の全重量に対して、5〜40重量%以上が好ましく、より好ましくは15〜30重量%である。スチレン系単量体の含有量が60重量%未満の場合(または、共役ジエンの含有量が40重量%を超える場合)には、フィルムに腰がなくなる場合や自然収縮が大きくなる場合があり、共役ジエンの含有量が5重量%未満の場合(または、スチレン系単量体の含有量が95重量%を超える場合)には、脆くなる場合や伸度が低くなる場合がある。   In the styrene-conjugated diene copolymer, the content of the styrene monomer is preferably 60 to 95% by weight, more preferably 70 to 85% by weight, based on the total weight of the monomer components. . On the other hand, the content of the conjugated diene is preferably 5 to 40% by weight or more, more preferably 15 to 30% by weight, based on the total weight of the monomer components. When the content of the styrenic monomer is less than 60% by weight (or when the content of the conjugated diene exceeds 40% by weight), the film may lose its elasticity or natural shrinkage may increase. When the content of the conjugated diene is less than 5% by weight (or when the content of the styrene monomer exceeds 95% by weight), it may become brittle or the elongation may be lowered.

上記スチレン−共役ジエン共重合体は、本発明の効果を損なわない範囲であれば、上記スチレン系単量体、共役ジエン以外の単量体成分を含有していてもよい。このような単量体成分としては、例えば、ビニル系モノマー、重合性不飽和カルボン酸エステル共重合体などが挙げられる。   The styrene-conjugated diene copolymer may contain monomer components other than the styrene monomer and conjugated diene as long as the effects of the present invention are not impaired. Examples of such monomer components include vinyl monomers and polymerizable unsaturated carboxylic acid ester copolymers.

本発明のシュリンクフィルムにおけるB層には、上記スチレン−共役ジエン共重合体とともに、または、スチレン−共役ジエン共重合体にかえて、上記スチレン−共役ジエン共重合体に水素添加した水添物を用いてもよい。   The B layer in the shrink film of the present invention contains a hydrogenated product obtained by hydrogenating the styrene-conjugated diene copolymer together with the styrene-conjugated diene copolymer or in place of the styrene-conjugated diene copolymer. It may be used.

上記スチレン−共役ジエン共重合体の共重合の形態としては、ランダム共重合体、ブロック共重合体、交互共重合体など、特に限定されないが、ブロック共重合体が好ましく、スチレンブロック(S)−共役ジエンブロック(D)型、S−D−S型、D−S−D型、S−D−S−D型等が挙げられる。また、当該共重合体の水添物であってもよい。   The form of copolymerization of the styrene-conjugated diene copolymer is not particularly limited, such as a random copolymer, a block copolymer, and an alternating copolymer, but a block copolymer is preferable, and a styrene block (S)- Examples include conjugated diene block (D) type, SDS type, DSD type, SSD type, and the like. Further, it may be a hydrogenated product of the copolymer.

上記スチレン−共役ジエン共重合体またはその水添物としては、具体的には、例えば、スチレン−ブタジエンブロック共重合体(SBS)、スチレン−イソプレンブロック共重合体(SIS)、スチレン−ブタジエン−イソプレンブロック共重合体(SBIS)、スチレン−エチレン・ブタジエンブロック共重合体(SEBS)、スチレン−エチレン・プロピレン共重合体(SEPS)などが例示される。中でも、最も好ましくは、SBS、SBISである。   Specific examples of the styrene-conjugated diene copolymer or the hydrogenated product thereof include, for example, a styrene-butadiene block copolymer (SBS), a styrene-isoprene block copolymer (SIS), and a styrene-butadiene-isoprene. Examples thereof include a block copolymer (SBIS), a styrene-ethylene / butadiene block copolymer (SEBS), and a styrene-ethylene / propylene copolymer (SEPS). Of these, SBS and SBIS are most preferable.

上記スチレン−共役ジエン共重合体またはその水添物のメルトフローレート(MFR)(JIS K 7210 :温度200℃/荷重49N)は、1〜20g/10分が好ましく、より好ましくは3〜10g/10分である。   The melt flow rate (MFR) (JIS K 7210: temperature 200 ° C./load 49 N) of the styrene-conjugated diene copolymer or its hydrogenated product is preferably 1 to 20 g / 10 minutes, more preferably 3 to 10 g / 10 minutes.

上記スチレン−共役ジエン共重合体またはその水添物としては、市販品を用いてもよく、例えば、旭化成(株)製「アサフレックス」、「タフテック」;電気化学工業(株)製「クリアレン」;クラレ(株)製「セプトン」などが挙げられる。   As the styrene-conjugated diene copolymer or hydrogenated product thereof, commercially available products may be used. For example, “Asaflex”, “Tuftec” manufactured by Asahi Kasei Co., Ltd .; “Clearene” manufactured by Denki Kagaku Kogyo Co., Ltd. ; “Kuraray Co., Ltd.” “Septon” and the like.

本発明のB層を構成する樹脂組成物(樹脂組成物B)の総重量に対する、上記スチレン−共役ジエン共重合体及び/又はその水添物の含有量は、50重量%以上であり、好ましくは70〜100重量%である。なお、2種以上のスチレン−共役ジエン共重合体及び/又はその水添物を用いる場合には、それらの合計量が上記の関係を満たしておればよい。   The content of the styrene-conjugated diene copolymer and / or hydrogenated product thereof with respect to the total weight of the resin composition (resin composition B) constituting the B layer of the present invention is preferably 50% by weight or more, Is 70 to 100% by weight. In addition, when using 2 or more types of styrene-conjugated diene copolymers and / or its hydrogenated material, those total amounts should just satisfy said relationship.

樹脂組成物Bには、高収縮性、腰の強さの向上と自然収縮の防止のために、石油樹脂などの粘着付与剤(タッキファイヤ)を含んでいてもよい。上記粘着付与剤としては、例えば、ロジン系樹脂(ロジン、重合ロジン、水添ロジン及びそれらの誘導体、樹脂酸ダイマーなど)、テルペン系樹脂(テルペン樹脂、芳香族変性テルペン樹脂、水添テルペン樹脂、テルペン−フェノール樹脂など)、石油樹脂(脂肪族系、芳香族系、脂環族系)などが挙げられる。中でも、石油樹脂が好ましい。粘着付与剤は単独で又は2種以上を組み合わせて使用できる。粘着付与剤を添加する場合の添加量は、樹脂組成物Bの総重量に対して、5〜30重量%が好ましく、より好ましくは10〜25重量%である。添加量が30重量%を超えると、シュリンクフィルムが脆くなる場合がある。また、5重量%未満では添加の効果が小さい場合がある。   The resin composition B may contain a tackifier (tackifier) such as petroleum resin in order to improve the high shrinkage, the strength of the waist and the prevention of natural shrinkage. Examples of the tackifier include rosin resins (rosin, polymerized rosin, hydrogenated rosin and derivatives thereof, resin acid dimers, etc.), terpene resins (terpene resins, aromatic modified terpene resins, hydrogenated terpene resins, Terpene-phenol resins, etc.), petroleum resins (aliphatic, aromatic, alicyclic) and the like. Among these, petroleum resin is preferable. A tackifier can be used individually or in combination of 2 or more types. The addition amount in the case of adding a tackifier is preferably 5 to 30% by weight, more preferably 10 to 25% by weight, based on the total weight of the resin composition B. If the amount added exceeds 30% by weight, the shrink film may become brittle. Moreover, if it is less than 5 weight%, the effect of addition may be small.

[接着性樹脂層(C層)]
本発明のシュリンクラベルにおいて、必要に応じて用いられる接着性樹脂層(C層)は、極性基を有するポリスチレン系樹脂から構成されることが好ましい。
[Adhesive resin layer (C layer)]
In the shrink label of the present invention, the adhesive resin layer (C layer) used as necessary is preferably composed of a polystyrene-based resin having a polar group.

上記極性基は、ポリエステルのエステル結合部分と反応または相互作用(水素結合など)する官能基であることが好ましく、特に限定されないが、例えば、カルボキシル基(カルボン酸無水物も含む)、水酸基、オキサゾリン基、イソシアネート基、エポキシ基などが挙げられる。中でも、層間強度向上の観点から、ジカルボン酸無水物基(無水ジカルボン酸変性)、エポキシ基(エポキシ変性)が好ましく、マレイン酸無水物基(無水マレイン酸変性)が特に好ましい。上記の極性基は、ポリスチレン系ポリマーの主鎖にグラフト化されていても良いし、共重合によりポリマー主鎖中に導入されていてもよい。上記「変性」という場合には、「反応性官能基がポリマー主鎖にグラフト化により導入されたもの」及び「共重合により導入されたもの」の両方を含むものとする。   The polar group is preferably a functional group that reacts with or interacts with the ester bond portion of the polyester (such as a hydrogen bond), and is not particularly limited. For example, a carboxyl group (including a carboxylic acid anhydride), a hydroxyl group, and an oxazoline Group, isocyanate group, epoxy group and the like. Among these, from the viewpoint of improving the interlayer strength, a dicarboxylic anhydride group (dicarboxylic anhydride modified) and an epoxy group (epoxy modified) are preferable, and a maleic anhydride group (maleic anhydride modified) is particularly preferable. The polar group may be grafted to the main chain of the polystyrene-based polymer, or may be introduced into the polymer main chain by copolymerization. The term “modified” includes both “reactive functional groups introduced by grafting into the polymer main chain” and “introduced by copolymerization”.

上記極性基を有するポリスチレン系樹脂のポリマーの主鎖骨格を構成するポリスチレン系樹脂としては、特に限定されず、スチレンの単独重合体である一般ポリスチレン(GPPS)、スチレン系単量体の単独又は共重合体、スチレン−共役ジエン共重合体、スチレン−重合性不飽和カルボン酸エステル共重合体、スチレン−共役ジエン−重合性不飽和カルボン酸エステル共重合体等が挙げられる。   The polystyrene resin constituting the main chain skeleton of the polymer of the polystyrene resin having the polar group is not particularly limited, and general polystyrene (GPPS) which is a homopolymer of styrene, styrene monomer alone or in combination. Examples thereof include a polymer, a styrene-conjugated diene copolymer, a styrene-polymerizable unsaturated carboxylic acid ester copolymer, and a styrene-conjugated diene-polymerizable unsaturated carboxylic acid ester copolymer.

中でも、スチレン系単量体および共役ジエンを必須の単量体成分として構成されるスチレン系熱可塑性エラストマーやその水添物を変性し、上記極性基を導入した変性物が好ましい。上記スチレン系単量体としては、特に限定されないが、例えば、スチレン、α−メチルスチレン、m−メチルスチレン、p−メチルスチレン、p−エチルスチレン、p−イソブチルスチレン、p−t−ブチルスチレン、クロロメチルスチレンなどが挙げられる。中でも、強度、成型性などの物性の観点から、スチレンが特に好ましい。上記共役ジエンとしては、特に限定されないが、例えば、1,3−ブタジエン、イソプレン(2−メチル−1,3−ブタジエン)、2,3−ジメチル−1,3−ブタジエン、1,3−ペンタジエン、1,3−ヘキサジエン、クロロプレンなどが挙げられる。中でも、弾性付与、極性付与の観点から、1,3−ブタジエン、イソプレンが特に好ましい。さらに、ビニル系モノマー、重合性不飽和カルボン酸エステル共重合体などの他の共重合成分を含んでいてもよい。なお、これらスチレン系単量体や共役ジエンなどの単量体成分は、単独で用いてもよいし、2種以上を併用してもよい。また、上記スチレン系熱可塑性エラストマーの共重合の形態としては、ランダム共重合体、ブロック共重合体、交互共重合体など、特に限定されないが、ブロック共重合体が好ましい。上記スチレン系熱可塑性エラストマーとしては、具体的には、例えば、スチレン−ブタジエンブロック共重合体(SBS)、スチレン−イソプレンブロック共重合体(SIS)、スチレン−ブタジエン−イソプレンブロック共重合体(SBIS)などが例示され、水添スチレン系熱可塑性エラストマーとしては、スチレン−エチレン・ブタジエンブロック共重合体(SEBS)、スチレン−エチレン・プロピレン共重合体(SEPS)などが例示される。   Among these, a modified product obtained by modifying a styrene-based thermoplastic elastomer composed of styrene-based monomer and conjugated diene as essential monomer components or a hydrogenated product thereof and introducing the above polar group is preferable. Although it does not specifically limit as said styrene-type monomer, For example, styrene, alpha-methyl styrene, m-methyl styrene, p-methyl styrene, p-ethyl styrene, p-isobutyl styrene, pt-butyl styrene, Examples include chloromethylstyrene. Among these, styrene is particularly preferable from the viewpoint of physical properties such as strength and moldability. The conjugated diene is not particularly limited. For example, 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, Examples include 1,3-hexadiene and chloroprene. Among these, 1,3-butadiene and isoprene are particularly preferable from the viewpoint of imparting elasticity and imparting polarity. Furthermore, other copolymer components such as vinyl monomers and polymerizable unsaturated carboxylic acid ester copolymers may be included. In addition, these monomer components, such as a styrene-type monomer and a conjugated diene, may be used independently and may use 2 or more types together. Further, the form of copolymerization of the styrene-based thermoplastic elastomer is not particularly limited, such as a random copolymer, a block copolymer, and an alternating copolymer, but a block copolymer is preferable. Specific examples of the styrenic thermoplastic elastomer include, for example, a styrene-butadiene block copolymer (SBS), a styrene-isoprene block copolymer (SIS), and a styrene-butadiene-isoprene block copolymer (SBIS). Examples of the hydrogenated styrene-based thermoplastic elastomer include styrene-ethylene / butadiene block copolymer (SEBS) and styrene-ethylene / propylene copolymer (SEPS).

上記スチレン系熱可塑性エラストマーにおいて、上記スチレン系単量体の含有量は、単量体成分の全重量に対して、10〜60重量%であり、好ましくは20〜50重量%、より好ましくは20〜45重量%である。一方、上記共役ジエンの含有量は、単量体成分の全重量に対して、40〜90重量%であり、好ましくは50〜80重量%、より好ましくは55〜80重量%である。   In the styrenic thermoplastic elastomer, the content of the styrenic monomer is 10 to 60% by weight, preferably 20 to 50% by weight, more preferably 20%, based on the total weight of the monomer components. ~ 45 wt%. On the other hand, content of the said conjugated diene is 40 to 90 weight% with respect to the total weight of a monomer component, Preferably it is 50 to 80 weight%, More preferably, it is 55 to 80 weight%.

上記極性基を有するポリスチレン系樹脂の重量平均分子量は、層形成時の流動性の観点から、10万〜50万が好ましく、より好ましくは20万〜40万である。   The weight-average molecular weight of the polystyrene-based resin having a polar group is preferably 100,000 to 500,000, more preferably 200,000 to 400,000, from the viewpoint of fluidity during layer formation.

上記極性基を有するポリスチレン系樹脂としては、具体的には、無水マレイン酸変性SEBS、無水マレイン酸変性SEPS、エポキシ変性SEBS、エポキシ変性SEPSなどが好ましく例示される。これらは、市販品を用いてもよく、例えば、旭化成(株)製「タフテックM」、クレイトン(株)製「クレイトンFG」などが挙げられる。   Specific examples of the polystyrene resin having a polar group include maleic anhydride-modified SEBS, maleic anhydride-modified SEPS, epoxy-modified SEBS, and epoxy-modified SEPS. Commercially available products may be used, and examples thereof include “Tuftec M” manufactured by Asahi Kasei Corporation, “Clayton FG” manufactured by Clayton Co., Ltd., and the like.

本発明のC層を構成する樹脂組成物(樹脂組成物C)の総重量に対する上記極性基を有するポリスチレン系樹脂の含有量は、5〜100重量%であり、接着性(層間強度)の観点から、好ましくは20〜100重量%である。上記含有量が5重量%未満の場合には、接着強度が不足し、デラミ(層間剥離)が生じる場合がある。   Content of the polystyrene-type resin which has the said polar group with respect to the total weight of the resin composition (resin composition C) which comprises C layer of this invention is 5 to 100 weight%, and is a viewpoint of adhesiveness (interlayer strength). Therefore, it is preferably 20 to 100% by weight. When the content is less than 5% by weight, the adhesive strength is insufficient and delamination (delamination) may occur.

樹脂組成物Cには、耐熱性向上のために、石油樹脂などの粘着付与剤(タッキファイヤ)を含んでいてもよい。上記粘着付与剤としては、例えば、ロジン系樹脂(ロジン、重合ロジン、水添ロジン及びそれらの誘導体、樹脂酸ダイマーなど)、テルペン系樹脂(テルペン樹脂、芳香族変性テルペン樹脂、水添テルペン樹脂、テルペン−フェノール樹脂など)、石油樹脂(脂肪族系、芳香族系、脂環族系)などが挙げられる。中でも、石油樹脂が好ましい。粘着付与剤は単独で又は2種以上を組み合わせて使用できる。粘着付与剤を添加する場合の添加量は、樹脂組成物Cの総重量に対して、5〜30重量%が好ましく、より好ましくは10〜25重量%である。   The resin composition C may contain a tackifier such as petroleum resin in order to improve heat resistance. Examples of the tackifier include rosin resins (rosin, polymerized rosin, hydrogenated rosin and derivatives thereof, resin acid dimers, etc.), terpene resins (terpene resins, aromatic modified terpene resins, hydrogenated terpene resins, Terpene-phenol resins, etc.), petroleum resins (aliphatic, aromatic, alicyclic) and the like. Among these, petroleum resin is preferable. A tackifier can be used individually or in combination of 2 or more types. The addition amount in the case of adding a tackifier is preferably 5 to 30% by weight, more preferably 10 to 25% by weight, based on the total weight of the resin composition C.

[シュリンクフィルム]
本発明のシュリンクフィルムは、前述のとおり、A層(表面層)/B層(中心層)/A層の順に、A層およびB層が積層された2種3層の積層構造を少なくとも含んだ積層構成である。好ましくは、A層/C層(接着性樹脂層)/B層/C層/A層の3種5層の積層構成である。
[Shrink film]
As described above, the shrink film of the present invention includes at least a two-layer / three-layer structure in which the A layer and the B layer are stacked in the order of A layer (surface layer) / B layer (center layer) / A layer. It is a laminated structure. Preferably, it is a laminated structure of 3 types and 5 layers of A layer / C layer (adhesive resin layer) / B layer / C layer / A layer.

上記積層構造は共押出により形成される。上記共押出の一般的方法(A層/C層/B層/C層/A層の3種5層積層の場合を例に説明する)は、それぞれ所定の温度に設定した複数の押出機に樹脂組成物A〜Cをそれぞれ投入し、Tダイ、サーキュラーダイなどから共押出する方法である。この際、マニホールドや合流ブロックを用いて、所定の積層構成とすることが好ましい。また必要に応じて、ギアポンプを用いて供給量を調節してもよく、さらにフィルターを用いて、異物を除去するとフィルム破れが低減できるため好ましい。なお、押出温度は、用いる樹脂組成物A〜Cの種類によっても異なり、特に限定されないが、各樹脂組成物の成型温度領域が近接していることが好ましい。具体的には、樹脂組成物A(A層)の押出温度は210〜250℃が好ましく、樹脂組成物B(B層)は180〜220℃、樹脂組成物C(C層)は190〜220℃が好ましい。上記共押出したポリマーを、冷却ドラムなどを用いて急冷することにより、未延伸積層フィルム(シート)を得ることができる。   The laminated structure is formed by coextrusion. The above general method of coextrusion (explained by taking the case of three layers of five layers of A layer / C layer / B layer / C layer / A layer as an example) is applied to a plurality of extruders each set at a predetermined temperature. In this method, resin compositions A to C are respectively charged and coextruded from a T die, a circular die or the like. At this time, it is preferable to use a manifold or a merging block to form a predetermined laminated structure. Further, if necessary, the supply amount may be adjusted using a gear pump, and it is preferable to remove foreign substances using a filter because film tearing can be reduced. The extrusion temperature varies depending on the types of the resin compositions A to C to be used, and is not particularly limited. However, it is preferable that the molding temperature regions of the resin compositions are close to each other. Specifically, the extrusion temperature of the resin composition A (A layer) is preferably 210 to 250 ° C, the resin composition B (B layer) is 180 to 220 ° C, and the resin composition C (C layer) is 190 to 220 ° C. ° C is preferred. An unstretched laminated film (sheet) can be obtained by quenching the coextruded polymer using a cooling drum or the like.

本発明のシュリンクフィルムは、収縮特性の観点から、1軸又は2軸に配向したフィルムである。シュリンクフィルムがA層、B層からなる2種3層構成の場合には、A層、B層のいずれもが、また、A〜C層からなる3種5層構成の場合には、A〜Cの全ての層(5層)が配向している必要がある。全ての層が配向していない場合には、良好な収縮性を得ることができない。配向は1軸配向、2軸配向など特に限定されないが、フィルム幅方向(ラベルを筒状にした場合に周方向となる方向)に強く配向した、実質的に幅方向の1軸配向が好ましい。また、フィルムの長手方向(幅方向と直交する方向)に強く配向した実質的に長手方向の1軸配向フィルムであってもよい。   The shrink film of the present invention is a film oriented uniaxially or biaxially from the viewpoint of shrinkage characteristics. In the case where the shrink film has a two-kind three-layer structure composed of an A layer and a B layer, both of the A layer and the B layer, and in the case of a three-kind five-layer structure composed of A to C layers, A to All layers (5 layers) of C need to be oriented. When all the layers are not oriented, good shrinkage cannot be obtained. The orientation is not particularly limited, such as uniaxial orientation or biaxial orientation, but substantially uniaxial orientation in the width direction, which is strongly oriented in the film width direction (direction that becomes the circumferential direction when the label is formed into a cylinder) is preferable. Further, it may be a substantially uniaxially oriented film in the longitudinal direction that is strongly oriented in the longitudinal direction (direction perpendicular to the width direction) of the film.

上記1軸配向、2軸配向などの配向フィルムは、未延伸積層フィルムを延伸することにより作製できる。延伸としては、所望の配向に応じて選択でき、長手方向(縦方向;MD方向)および幅方向(横方向;TD方向)の2軸延伸でもよいし、長手、または、幅方向の1軸延伸でもよい。また、延伸方式は、ロール方式、テンター方式、チューブ方式の何れの方式を用いてもよい。延伸条件としては、用いる樹脂組成物A〜Cの種類によっても異なり、特に限定されないが、一般的には70〜110℃の範囲で、長手、幅の各方向に1.01〜8倍程度の倍率で行うことが好ましい。例えば、長手方向に1.01〜1.5倍(好ましくは1.05〜1.3倍)程度に延伸した後、幅方向に2〜8倍(好ましくは3〜6倍)程度延伸することが好ましい。   An oriented film such as the uniaxial orientation or the biaxial orientation can be produced by stretching an unstretched laminated film. Stretching can be selected according to the desired orientation, and may be biaxial stretching in the longitudinal direction (longitudinal direction; MD direction) and width direction (transverse direction; TD direction), or uniaxial stretching in the longitudinal direction or width direction. But you can. The stretching method may be any of a roll method, a tenter method, and a tube method. The stretching conditions vary depending on the types of resin compositions A to C used, and are not particularly limited, but are generally in the range of 70 to 110 ° C. and about 1.01 to 8 times in the longitudinal and width directions. It is preferable to carry out at a magnification. For example, the film is stretched about 1.01 to 1.5 times (preferably 1.05 to 1.3 times) in the longitudinal direction and then stretched about 2 to 8 times (preferably 3 to 6 times) in the width direction. Is preferred.

本発明のシュリンクフィルムにおいて、A層の厚み(1層分)は、特に限定されないが、2〜10μmが好ましく、より好ましくは3〜5μmである。A層厚みが10μmを超えるとA層の収縮応力が大きくなり、層間剥離しやすくなる場合があり、2μm未満では耐溶剤性が低下する場合がある。   In the shrink film of the present invention, the thickness of the A layer (one layer) is not particularly limited, but is preferably 2 to 10 μm, more preferably 3 to 5 μm. When the thickness of the A layer exceeds 10 μm, the shrinkage stress of the A layer increases, and the delamination may easily occur. When the thickness is less than 2 μm, the solvent resistance may decrease.

本発明のシュリンクフィルムにおいて、B層の厚み(1層分)は、特に限定されないが、10〜40μmが好ましく、より好ましくは20〜30μmである。B層厚みが40μmを超えるとA層の収縮に追従しにくくなる場合があり、10μm未満ではB層とA層の収縮応力が極端に異なるため、層間剥離しやすくなる場合がある。   In the shrink film of the present invention, the thickness of B layer (one layer) is not particularly limited, but is preferably 10 to 40 μm, more preferably 20 to 30 μm. If the thickness of the B layer exceeds 40 μm, it may be difficult to follow the shrinkage of the A layer. If the thickness is less than 10 μm, the shrinkage stress between the B layer and the A layer may be extremely different, and thus delamination may be likely.

本発明のシュリンクフィルムにおいて、C層を設ける場合のC層の厚み(1層分)は、特に限定されないが、2〜10μmが好ましく、より好ましくは3〜5μmである。C層厚みが10μmを超えると収縮が不均一となる場合があり、2μm未満では接着機能を発揮できない場合がある。   In the shrink film of the present invention, the thickness (one layer) of the C layer when the C layer is provided is not particularly limited, but is preferably 2 to 10 μm, more preferably 3 to 5 μm. If the thickness of the C layer exceeds 10 μm, the shrinkage may be nonuniform, and if it is less than 2 μm, the adhesion function may not be exhibited.

本発明のシュリンクフィルムの厚みは、特に限定されないが、20〜60μmが好ましく、より好ましくは35〜55μm、さらに好ましくは30〜50μmである。   Although the thickness of the shrink film of this invention is not specifically limited, 20-60 micrometers is preferable, More preferably, it is 35-55 micrometers, More preferably, it is 30-50 micrometers.

本発明のシュリンクフィルムにおいて、全体厚みを100%とした場合、A層の厚み比(全A層の合計)は5〜40%、B層の厚み比(全B層の合計)は50〜90%、C層の厚み比(全C層の合計)は5〜40%が好ましい。各層厚みを上記範囲に制御することにより、各層の収縮量、収縮応力のバランスを調整し、層間剥離を防止できるため好ましい。   In the shrink film of the present invention, when the total thickness is 100%, the thickness ratio of the A layer (total of all A layers) is 5 to 40%, and the thickness ratio of the B layer (total of all B layers) is 50 to 90. %, C layer thickness ratio (total of all C layers) is preferably 5 to 40%. Controlling the thickness of each layer within the above range is preferable because the balance between the shrinkage and shrinkage stress of each layer can be adjusted and delamination can be prevented.

本発明のシュリンクフィルムにおいて、表面層(A層)は、ポリエステル系樹脂を主成分とするため、高収縮性であり、また表面に耐摩耗性、耐薬品性を付与することができる。これに対して中心層(B層)に用いられるスチレン−共役ジエン共重合体またはその水添物はラベルの急激な収縮を抑え収縮挙動を緩やかにすることができる。また、必要に応じて設けられる接着性樹脂層(C層)は、A層及びB層の両層と密着性が高く、層間強度をより一層向上させる役割を担う。   In the shrink film of the present invention, the surface layer (A layer) has a polyester resin as a main component, and therefore has high shrinkability, and can impart wear resistance and chemical resistance to the surface. On the other hand, the styrene-conjugated diene copolymer or hydrogenated product used for the central layer (B layer) can suppress the rapid shrinkage of the label and can moderate the shrinkage behavior. Moreover, the adhesive resin layer (C layer) provided as needed has high adhesiveness with both the A layer and the B layer and plays a role of further improving the interlayer strength.

しかしながら、上記のような異種素材を積層した積層フィルムでは、接着層を設けることなどにより、シュリンクフィルム製造工程、センターシール工程などでは十分な層間強度を発揮させることができるものの、センターシールを施しシュリンク加工(収縮加工)によりボトルに装着した後には、センターシール部分で層間剥離が生じるという問題が生じていた。上記問題は、ポリエステル系樹脂層とスチレン−共役ジエン共重合体などのポリスチレン系樹脂は加熱した場合の収縮応力が異なるため、シュリンク加工(加熱)を施した場合には、各フィルム層間に収縮応力の差が生じ、それによって層間剥離が発生すると推定される。特にセンターシール部分は、フィルムの一方の面側がシールにより固定されているため、上記フィルム層間の収縮応力の差が顕著にあらわれると推定される。   However, in the laminated film in which different kinds of materials are laminated as described above, it is possible to exert a sufficient interlayer strength in the shrink film manufacturing process, the center seal process, etc. by providing an adhesive layer, etc. After being attached to the bottle by processing (shrink processing), there was a problem that delamination occurred at the center seal portion. The above problem is that when a polyester resin layer and a polystyrene resin such as a styrene-conjugated diene copolymer have different shrinkage stress when heated, the shrinkage stress between each film layer when shrink processing (heating) is applied. It is estimated that delamination occurs, thereby causing delamination. In particular, in the center seal portion, since one surface side of the film is fixed by the seal, it is estimated that the difference in shrinkage stress between the film layers appears remarkably.

これに対して、本発明のシュリンクフィルムにおいては、B層やC層の樹脂に比べて、収縮応力の大きいA層のポリエステル系樹脂に可塑剤を特定量添加することによって、A層の収縮応力を低減することにより、層間に生じる収縮応力差を低減し、層間剥離の発生を抑止している。また、各層を共押出により積層させることにより、フィルム層同士の密着を向上させて層間強度を高めている。さらに、各層の厚み、厚み比を上記の範囲に制御することにより、収縮応力差をより一層低減して層間剥離を抑制することができる。なお、延伸配向を低くすることにより収縮応力差を低減することもできるが、その場合には収縮特性(収縮率など)も低下するため好ましくない。   On the other hand, in the shrink film of the present invention, by adding a specific amount of plasticizer to the polyester resin of the A layer having a larger shrinkage stress than the resin of the B layer or the C layer, the shrinkage stress of the A layer is obtained. Is reduced, the shrinkage stress difference generated between the layers is reduced, and the occurrence of delamination is suppressed. Further, by laminating each layer by coextrusion, the adhesion between the film layers is improved to increase the interlayer strength. Furthermore, by controlling the thickness and thickness ratio of each layer within the above ranges, the shrinkage stress difference can be further reduced and delamination can be suppressed. Although the shrinkage stress difference can be reduced by lowering the stretch orientation, in that case, the shrinkage characteristics (shrinkage rate, etc.) are also lowered, which is not preferable.

本発明のシュリンクフィルムにおけるA層(単層)の収縮応力(85℃、主配向方向)は、3〜10MPaが好ましく、より好ましくは4〜6MPaである。A層の収縮応力が10MPaを超える場合にはB層、C層との収縮応力の差が大きくなり層間剥離を生じやすくなる。3MPa未満ではラベル収縮(シュリンク加工時)に容器形状に追従できなくなる場合がある。B層(単層)の収縮応力(85℃、主配向方向)は、2〜10MPaが好ましく、より好ましくは3〜5MPaである。B層の収縮応力が10MPaを超える場合にはC層との収縮差が大きくなり剥離しやすくなる。2MPa未満ではA層との収縮応力の差が大きくなり層間剥離を生じやすくなる。C層(単層)の収縮応力(85℃、主配向方向)は、2〜8MPaが好ましく、より好ましくは3〜4MPaである。B層の収縮応力が8MPaを超える場合には接着特性が低下する。2MPa未満ではA層との収縮応力の差が大きくなり層間剥離を生じやすくなる。上記「主配向方向」とは、「主に延伸処理を施した方向」のことをいう。1軸延伸フィルムであれば延伸方向、2軸延伸フィルムであれば、配向のより大きな延伸方向をいう。筒状シュリンクラベル用のシュリンクフィルムの場合は、一般的に、装着される際に容器の周方向となる方向(フィルムの幅方向)が主配向方向であることが多い。   The shrinkage stress (85 ° C., main orientation direction) of the A layer (single layer) in the shrink film of the present invention is preferably 3 to 10 MPa, more preferably 4 to 6 MPa. When the shrinkage stress of the A layer exceeds 10 MPa, the difference in shrinkage stress between the B layer and the C layer becomes large and delamination tends to occur. If it is less than 3 MPa, label shrinkage (during shrink processing) may not be able to follow the container shape. The shrinkage stress (85 ° C., main orientation direction) of the B layer (single layer) is preferably 2 to 10 MPa, more preferably 3 to 5 MPa. When the shrinkage stress of the B layer exceeds 10 MPa, the shrinkage difference from the C layer becomes large and the film is easily peeled off. If it is less than 2 MPa, the difference in shrinkage stress with the A layer becomes large and delamination tends to occur. The shrinkage stress (85 ° C., main orientation direction) of the C layer (single layer) is preferably 2 to 8 MPa, more preferably 3 to 4 MPa. When the shrinkage stress of the B layer exceeds 8 MPa, the adhesive properties are deteriorated. If it is less than 2 MPa, the difference in shrinkage stress with the A layer becomes large and delamination tends to occur. The “main orientation direction” means “a direction in which a stretching process is mainly performed”. In the case of a uniaxially stretched film, it refers to the stretched direction, and in the case of a biaxially stretched film, it refers to a stretched direction having a larger orientation. In the case of a shrink film for a cylindrical shrink label, generally, the direction (the width direction of the film) that becomes the circumferential direction of the container when mounted is often the main orientation direction.

なお、上記の各層(単層)の収縮応力は、各層樹脂からなる、TD方向に幅15mm、長さ100mmの試験片を作製し、チャック間50mmにて、85℃の湯浴に10秒間浸漬し応力を測定することにより求める。上記収縮応力はシュリンク加工を行う前の各層の収縮応力を表す値である。   The shrinkage stress of each layer (single layer) was prepared by preparing a test piece made of each layer resin and having a width of 15 mm and a length of 100 mm in the TD direction, and immersed in a 85 ° C. hot water bath for 10 seconds at 50 mm between chucks. It is obtained by measuring the stress. The shrinkage stress is a value representing the shrinkage stress of each layer before shrink processing.

A層とB層の収縮応力差(絶対値)、B層とC層の収縮応力差(絶対値)、C層とA層の収縮応力差(絶対値)は、層間剥離抑制の観点から、3MPa未満が好ましく、より好ましくは2MPa未満である。   The shrinkage stress difference between the A layer and the B layer (absolute value), the shrinkage stress difference between the B layer and the C layer (absolute value), and the shrinkage stress difference between the C layer and the A layer (absolute value) are as follows. The pressure is preferably less than 3 MPa, more preferably less than 2 MPa.

本発明のシュリンクフィルムの収縮応力(85℃)は、2〜13MPaが好ましく、より好ましくは2〜8MPa、さらに好ましくは2〜5MPaである。収縮応力が2MPa未満の場合には、印刷層のシュリンク加工追従性が低下し、仕上がりが低下する場合がある。13MPaを超えると容器の変形を引き起こしたり、開封時に内容物があふれたりするおそれがある。   The shrinkage stress (85 ° C.) of the shrink film of the present invention is preferably 2 to 13 MPa, more preferably 2 to 8 MPa, and still more preferably 2 to 5 MPa. When the shrinkage stress is less than 2 MPa, the shrinkage followability of the printed layer is lowered, and the finish may be lowered. If it exceeds 13 MPa, the container may be deformed or the contents may overflow when opened.

本発明のシュリンクフィルムは優れた層間強度を有する。層間強度(延伸配向後のシュリンクフィルム(シュリンク加工前)の層間強度)は、1N/15mm以上が好ましく、より好ましくは2N/15mm以上である。層間強度(延伸配向後のシュリンクフィルム(シュリンク加工後)の層間強度)は、1N/15mm以上が好ましく、より好ましくは2N/15mm以上である。層間強度が上記範囲未満の場合には、加工工程や製品化した後に、フィルム層同士がはがれて、生産性を低下させたり、品質上の問題となる場合がある。   The shrink film of the present invention has excellent interlayer strength. The interlayer strength (the interlayer strength of the shrink film after stretch orientation (before shrink processing)) is preferably 1 N / 15 mm or more, more preferably 2 N / 15 mm or more. The interlayer strength (the interlayer strength of the shrink film after stretch orientation (after shrink processing)) is preferably 1 N / 15 mm or more, more preferably 2 N / 15 mm or more. If the interlaminar strength is less than the above range, the film layers may be peeled off after processing or commercialization, resulting in reduced productivity or quality problems.

本発明のシュリンクフィルム(シュリンク加工前)の90℃10秒(温水処理)における主配向方向(主に延伸処理を施した方向)の熱収縮率は、15%以上が好ましく、より好ましくは25〜80%、さらに好ましくは30〜70%である。熱収縮率が15%未満の場合には、ラベルを容器に熱で密着させる工程において、収縮が十分でないため、容器の形に追従困難となり、特に複雑な形状の容器に対して仕上がりが悪くなることがある。   The shrinkage ratio in the main orientation direction (mainly in the direction subjected to the stretching treatment) at 90 ° C. for 10 seconds (warm water treatment) of the shrink film (before shrink processing) of the present invention is preferably 15% or more, more preferably 25 to 25%. 80%, more preferably 30 to 70%. When the heat shrinkage rate is less than 15%, the shrinkage is not sufficient in the process of closely attaching the label to the container with heat, making it difficult to follow the shape of the container, and the finish is particularly poor for a complex shaped container. Sometimes.

なお、本発明のシュリンクフィルム(シュリンク加工前)の90℃10秒(温水処理)における上記主配向方向と直交する方向の熱収縮率は、−5〜15%が好ましい。   In addition, as for the thermal contraction rate of the direction orthogonal to the said main orientation direction in 90 degreeC 10 second (warm water process) of the shrink film (before shrink process) of this invention, -5-15% is preferable.

本発明のシュリンクフィルム(シュリンク加工前)の圧縮強度(厚み40μm:JIS P 8126)は、2N以上が好ましく、より好ましくは3.5N以上、さらに好ましくは5N以上である。なお、圧縮強度が2N未満の場合には、ラベルの腰が弱くなり、円筒状にしたシュリンクラベルを、容器に装着する工程でラベルが挫屈しやすくなる。   The compressive strength (thickness 40 μm: JIS P 8126) of the shrink film (before shrink processing) of the present invention is preferably 2N or more, more preferably 3.5N or more, and further preferably 5N or more. In addition, when the compressive strength is less than 2N, the waist of the label becomes weak, and the label tends to be bent in the process of mounting the cylindrical shrink label on the container.

本発明のシュリンクフィルムの透明度(透明性)(ヘイズ値:JIS K 7105、厚み40μm換算)(単位:%)は、10未満が好ましく、より好ましくは5.0未満、さらに好ましくは2.0未満である。ヘイズ値が10以上の場合には、シュリンクフィルムの内側(ラベルを容器に装着した時に容器側になる面側)に印刷を施し、フィルムを通して印刷を見せるシュリンクラベルの場合、製品とした際に、印刷が曇り、装飾性が低下することがある。ただし、ヘイズが10以上の場合であっても、フィルムを通して印刷を見せる上記用途以外の用途においては十分に使用可能である。   The transparency (transparency) (haze value: JIS K 7105, converted to 40 μm thickness) (unit:%) of the shrink film of the present invention is preferably less than 10, more preferably less than 5.0, and still more preferably less than 2.0. It is. When the haze value is 10 or more, the inside of the shrink film (the side that becomes the container side when the label is attached to the container) is printed, and in the case of a shrink label that shows printing through the film, Printing may be cloudy and decorative properties may be reduced. However, even if the haze is 10 or more, it can be sufficiently used in applications other than the above-mentioned applications that show printing through a film.

[シュリンクラベル]
本発明のシュリンクフィルムを基材として、その少なくとも一方の面側に印刷層を設けることによりシュリンクラベルとして好ましく用いることができる。また、上記シュリンクラベルとしては、印刷層の他にも、保護層、アンカーコート層、プライマーコート層、接着剤層(感圧性、感熱性など)などの樹脂層、コーティング層を設けてもよく、さらに、不織布、紙等の層を設けてもよい。本発明のシュリンクラベルの具体的構成としは、例えば、印刷層/A/B/A、印刷層/A/B/A/印刷層、印刷層/A/C/B/C/A、印刷層/A/C/B/C/A/印刷層などの層構成が好ましく例示される。なお、本発明のシュリンクフィルムは、印刷層を設けない場合にも、それ自体でシュリンクラベル用途として用いることも可能である。
[Shrink label]
By using the shrink film of the present invention as a base material and providing a printing layer on at least one side thereof, it can be preferably used as a shrink label. In addition to the printed layer, the shrink label may be provided with a protective layer, an anchor coat layer, a primer coat layer, a resin layer such as an adhesive layer (pressure sensitive, heat sensitive, etc.), a coating layer, Furthermore, you may provide layers, such as a nonwoven fabric and paper. Specific examples of the shrink label of the present invention include, for example, printing layer / A / B / A, printing layer / A / B / A / printing layer, printing layer / A / C / B / C / A, and printing layer. A layer structure such as / A / C / B / C / A / print layer is preferably exemplified. In addition, the shrink film of this invention can also be used for shrink label use by itself, even when a printing layer is not provided.

本発明のシュリンクラベルは、少なくとも一方の表面に印刷層(例えば、商品名やイラスト、取り扱い注意事項等を表示した層)を有する。上記印刷層は、印刷インキを塗布することにより形成する。塗布の方法は、生産性、加工性などの観点から、フィルム製膜後に公知慣用の印刷手法などを用いて塗布を行うオフラインコートによって設けることが好ましい。印刷手法としては、慣用の方法を用いることができるが、グラビア印刷またはフレキソ印刷が最も好ましい。印刷層の形成に用いられる印刷インキは、例えば顔料、バインダー樹脂、溶剤、その他の添加剤等からなる。上記バインダー樹脂としては、特に限定されないが、例えば、アクリル系、ウレタン系、ポリアミド系、塩化ビニル−酢酸ビニル共重合系、セルロース系、ニトロセルロース系などの樹脂を単独あるいは併用して使用できる。上記顔料としては、酸化チタン(二酸化チタン)等の白顔料、銅フタロシアニンブルー等の藍顔料、カーボンブラック、アルミフレーク、雲母(マイカ)、その他着色顔料等が用途に合わせて選択、使用できる。また、顔料として、その他にも、光沢調製などの目的で、アルミナ、炭酸カルシウム、硫酸バリウム、シリカ、アクリルビーズ等の体質顔料も使用できる。上記溶剤としては、例えば、トルエン、キシレン、メチルエチルケトン、酢酸エチル、メチルアルコール、エチルアルコール、イソプロピルアルコールなどの有機溶媒や水など通常用いられるものを使用できる。   The shrink label of the present invention has a printed layer (for example, a layer displaying a product name, an illustration, handling precautions, etc.) on at least one surface. The printing layer is formed by applying printing ink. From the viewpoint of productivity, workability, and the like, the coating method is preferably provided by off-line coating in which coating is performed using a known and commonly used printing method after film formation. As a printing method, a conventional method can be used, but gravure printing or flexographic printing is most preferable. The printing ink used for forming the printing layer is made of, for example, a pigment, a binder resin, a solvent, and other additives. Although it does not specifically limit as said binder resin, For example, resin, such as an acrylic type, a urethane type, a polyamide type, a vinyl chloride-vinyl acetate copolymer type, a cellulose type, a nitrocellulose type, can be used individually or in combination. As the pigment, white pigments such as titanium oxide (titanium dioxide), indigo pigments such as copper phthalocyanine blue, carbon black, aluminum flakes, mica (mica), and other colored pigments can be selected and used in accordance with the application. In addition, extender pigments such as alumina, calcium carbonate, barium sulfate, silica, and acrylic beads can also be used as pigments for the purpose of adjusting gloss. Examples of the solvent include organic solvents such as toluene, xylene, methyl ethyl ketone, ethyl acetate, methyl alcohol, ethyl alcohol, and isopropyl alcohol, and commonly used solvents such as water.

上記印刷層は、特に限定されないが、可視光、紫外線、電子線などの活性エネルギー線硬化性の樹脂層であってもよい。過剰の熱によるフィルムの変形を防ぐ場合などに有効である。例えば、紫外線による硬化の場合、紫外線(UV)ランプ、紫外線LEDや紫外線レーザーなどを用い、波長300〜460nmの紫外線(又は近紫外線)で、照射強度150〜1000mJ/cm2、照射時間0.1〜3秒程度の条件で行うことができる。活性エネルギー線硬化性の印刷層である場合には、印刷インキには、上記の他に、光ラジカル重合開始剤及び光カチオン重合開始剤などの光重合開始剤を添加することが好ましい。光ラジカル重合開始剤としては、例えば、ベンゾフェノン系、チオキサントン系、アセトフェノン系、アシルフォスフィン系重合開始剤等が挙げられ、光カチオン重合開始剤としては、例えば、ジアゾニウム塩、ジアリールヨードニウム塩、トリアリールスルホニウム塩、シラノール/アルミニウム錯体、スルホン酸エステル、イミドスルホネートなどが挙げられる。これら光重合開始剤の含有量は、特に限定されないが、印刷インキ全体に対して、0.5〜7重量%が好ましく、より好ましくは1〜5重量%である。さらに、印刷インキには、生産効率を高める観点から、必要に応じて、増感剤を添加してもよい。その場合の増感剤は、例えば、脂肪族、芳香族アミン、ピペリジンなど窒素を環に含むアミンなどのアミン系増感剤;アリル系、o−トリルチオ尿素などの尿素系増感剤;ナトリウムジエチルジチオホスフェートなどのイオウ化合物系増感剤;アントラセン系増感剤;N,N−ジ置換−p−アミノベンゾニトリル系化合物などのニトリル系増感剤;トリ−n−ブチルホスフィンなどのリン化合物系増感剤;N−ニトロソヒドロキシルアミン誘導体、オキサゾリジン化合物などの窒素化合物系増感剤;四塩化炭素などの塩素化合物系増感剤などが挙げられる。増感剤の含有量としては、特に限定されないが、印刷インキ全体に対して、0.1〜5重量%が好ましく、特に好ましくは0.3〜3重量%である。 Although the said printing layer is not specifically limited, Active energy ray-curable resin layers, such as visible light, an ultraviolet-ray, and an electron beam, may be sufficient. This is effective for preventing deformation of the film due to excessive heat. For example, in the case of curing by ultraviolet rays, an ultraviolet (UV) lamp, such as using an ultraviolet LED or an ultraviolet laser, ultraviolet ray having a wavelength 300~460Nm (or near UV), irradiation intensity 150~1000mJ / cm 2, irradiation time 0.1 It can be performed under about 3 seconds. In the case of an active energy ray-curable printing layer, it is preferable to add a photopolymerization initiator such as a photoradical polymerization initiator and a photocationic polymerization initiator to the printing ink in addition to the above. Examples of the photo radical polymerization initiator include benzophenone, thioxanthone, acetophenone, and acylphosphine polymerization initiators. Examples of the photo cationic polymerization initiator include diazonium salts, diaryl iodonium salts, and triaryls. Examples include sulfonium salts, silanol / aluminum complexes, sulfonate esters, and imide sulfonates. Although content of these photoinitiators is not specifically limited, 0.5-7 weight% is preferable with respect to the whole printing ink, More preferably, it is 1-5 weight%. Furthermore, you may add a sensitizer to printing ink as needed from a viewpoint of improving production efficiency. In this case, the sensitizer is, for example, an amine-based sensitizer such as an aliphatic, aromatic amine, piperidine, or other amine containing a nitrogen in the ring; an allyl-based or o-tolylthiourea-based urea-based sensitizer; sodium diethyl Sulfur compound sensitizers such as dithiophosphate; Anthracene sensitizers; Nitrile sensitizers such as N, N-disubstituted p-aminobenzonitrile compounds; Phosphorus compound systems such as tri-n-butylphosphine Sensitizers; nitrogen compound sensitizers such as N-nitrosohydroxylamine derivatives and oxazolidine compounds; chlorine compound sensitizers such as carbon tetrachloride. Although it does not specifically limit as content of a sensitizer, 0.1 to 5 weight% is preferable with respect to the whole printing ink, Most preferably, it is 0.3 to 3 weight%.

上記印刷層の厚みは、特に限定されないが、例えば0.1〜10μm程度である。厚みが0.1μm未満である場合には、印刷層を均一に設けることが困難である場合があり、部分的な「かすれ」が起こったりして、装飾性が損なわれたり、デザイン通りの印刷が困難となる場合がある。また、厚みが10μmを超える場合には、印刷インキを多量に消費するため、コストが高くなったり、均一に塗布することが困難となったり、印刷層がもろくなって、剥離しやすくなったりする。また、印刷層の剛性が高くなり、シュリンク加工時にフィルムの収縮に追従しにくくなる場合がある。   Although the thickness of the said printing layer is not specifically limited, For example, it is about 0.1-10 micrometers. If the thickness is less than 0.1 μm, it may be difficult to provide a uniform printing layer, and partial “blur” may occur, resulting in a loss of decorativeness or printing as designed. May be difficult. In addition, when the thickness exceeds 10 μm, a large amount of printing ink is consumed, which increases the cost, makes it difficult to apply uniformly, makes the printed layer brittle and easily peels off. . Moreover, the rigidity of a printing layer becomes high and it may become difficult to follow the shrinkage | contraction of a film at the time of shrink processing.

[加工]
本発明のシュリンクラベルは、例えば、ラベル両端を溶剤や接着剤でシールし筒状にして容器に装着されるタイプの筒状ラベルや、ラベルの一端を容器に貼り付け、ラベルを巻き回した後、他端を一端に重ね合わせて筒状にする巻き付け方式のラベルとして好適に用いることができる。中でも、筒状シュリンクラベルとして好ましく用いられる。この筒状ラベルのセンターシール強度は、2N/15mm以上が好ましい。シール強度が2N/15mm未満の場合には、加工工程や製品化した後に、シール部分がはがれて、生産性を低下させたり、ラベル脱落の原因となる場合がある。
[processing]
The shrink label of the present invention is, for example, a cylindrical label of a type in which both ends of the label are sealed with a solvent or an adhesive and attached to the container, or one end of the label is attached to the container and the label is wound The other end can be suitably used as a winding-type label that overlaps with one end to form a cylinder. Especially, it is preferably used as a cylindrical shrink label. The center seal strength of this cylindrical label is preferably 2 N / 15 mm or more. When the seal strength is less than 2N / 15 mm, the seal portion may be peeled off after processing or product production, which may reduce the productivity or cause the label to drop off.

上記筒状ラベルの製造方法は、特に限定されないが、例えば下記の通りである。本発明のシュリンクラベルは、長尺状のシュリンクフィルムに印刷した後、所定の幅にスリットして、ロール状に巻回し、ラベルが長尺方向に複数個連なったロール状物とされた後、加工に用いられる。これらロール状物のひとつを繰り出しながら、フィルムの主延伸方向(例えば幅方向)が円周方向となるように円筒状に成形する。具体的には、長尺状のシュリンクラベルを筒状に形成し、ラベルの一方の側縁部に、長手方向に帯状に約2〜4mm幅で、テトラヒドロフラン(THF)などの溶剤や接着剤(以下溶剤等)を内面に塗布し、筒状に丸めて、該溶剤等塗布部を、他方の側縁部から5〜10mmの位置に重ね合わせて、他方の側縁部外面に接着(センターシール)し、長尺筒状のラベル連続体(長尺筒状シュリンクラベル)を得る。なお、ラベル切除用のミシン目を設ける場合は、所定の長さ及びピッチのミシン目を長手方向に形成する。ミシン目は慣用の方法(例えば、周囲に切断部と非切断部とが繰り返し形成された円板状の刃物を押し当てる方法やレーザーを用いる方法等)により施すことができる。ミシン目を施す工程段階は、印刷工程の後や、筒状加工工程の前後など、適宜選択することができる。   Although the manufacturing method of the said cylindrical label is not specifically limited, For example, it is as follows. After the shrink label of the present invention is printed on a long shrink film, it is slit into a predetermined width, wound into a roll, and after the roll is formed into a plurality of continuous labels in the long direction, Used for processing. While feeding one of these rolls, the film is formed into a cylindrical shape so that the main stretching direction (for example, the width direction) of the film is in the circumferential direction. Specifically, a long shrink label is formed into a cylindrical shape, and a solvent or adhesive (such as tetrahydrofuran (THF)) having a width of about 2 to 4 mm in the longitudinal direction on one side edge of the label. (Solvent, etc.) is applied to the inner surface, rounded into a cylindrical shape, and the coated portion of the solvent, etc. is superposed at a position of 5 to 10 mm from the other side edge and bonded to the outer surface of the other side edge (center seal) ) To obtain a long cylindrical label continuous body (long cylindrical shrink label). In the case where a perforation for label excision is provided, a perforation having a predetermined length and pitch is formed in the longitudinal direction. The perforation can be applied by a conventional method (for example, a method of pressing a disk-shaped blade having a cut portion and a non-cut portion repeatedly formed around it, a method using a laser, or the like). The process stage for perforating can be appropriately selected after the printing process and before and after the cylindrical processing process.

本発明のシュリンクラベルは、容器に装着し、ラベル付き容器として用いられる。このような容器には、例えば、PETボトルなどのソフトドリンク用ボトル、宅配用牛乳瓶、調味料などの食品用容器、アルコール飲料用ボトル、医薬品容器、洗剤、スプレーなどの化学製品の容器、カップ麺容器などが含まれる。容器の形状としても、円筒状、角形のボトルや、カップタイプなど様々な形状が含まれる。また、容器の材質としても、PETなどのプラスチック製、ガラス製、金属製などが含まれる。   The shrink label of the present invention is attached to a container and used as a labeled container. Such containers include, for example, soft drink bottles such as PET bottles, milk bottles for home delivery, food containers such as seasonings, alcoholic beverage bottles, pharmaceutical containers, containers for chemical products such as detergents and sprays, cups, etc. This includes noodle containers. The shape of the container includes various shapes such as a cylindrical shape, a square bottle, and a cup type. Further, the material of the container includes plastic such as PET, glass, metal and the like.

上記ラベル付き容器は、長尺筒状シュリンクラベルを切断後、所定の容器に装着し、加熱処理によって、ラベルを収縮、容器に追従密着させることによって作製できる。具体的には、ロール状にされた上記長尺筒状シュリンクラベルを、自動ラベル装着装置(シュリンクラベラー)に供給し、必要な長さに切断し、筒状シュリンクラベルとした後、該筒状シュリンクラベルを内容物を充填した容器に外嵌し、所定温度の熱風トンネルやスチームトンネルを通過させたり、赤外線等の輻射熱で加熱して熱収縮させ、容器に密着させて、ラベル付き容器を得る。上記加熱処理としては、例えば、80〜100℃のスチームで処理する(スチームおよび湯気が充満した加熱トンネルを通過させる)ことなどが例示される。   The above-mentioned container with a label can be produced by cutting a long cylindrical shrink label, mounting it on a predetermined container, shrinking the label by heat treatment, and closely contacting the container. Specifically, the above-described long cylindrical shrink label in a roll shape is supplied to an automatic label mounting device (shrink labeler), cut into a required length, and formed into a cylindrical shrink label. A shrink label is externally fitted to a container filled with the contents, and is passed through a hot air tunnel or steam tunnel at a predetermined temperature, or is heat-shrinked by radiant heat such as infrared rays, and is brought into close contact with the container to obtain a labeled container. . Examples of the heat treatment include treatment with steam at 80 to 100 ° C. (passing through a heating tunnel filled with steam and steam).

[物性の測定方法ならびに効果の評価方法]
(1)層間強度(シュリンク加工前)
シュリンクフィルムを用いて評価を行う。
長手方向(シュリンクフィルムの製膜方向)に15mmの幅で、幅方向(長手方向と直交方向)に長い短冊状のサンプル(200mm(シュリンクフィルム幅方向)×15mm(シュリンクフィルム長手方向))を採取した。以下で、サンプル幅方向とはシュリンクフィルムの長手方向をさす。
サンプルの長辺方向(シュリンクフィルムの幅方向)を測定方向として、下記の条件でT型剥離試験(JIS K 6854−3に準拠)を行い、層間の剥離荷重を測定する。
剥離荷重の平均値をもって層間強度(N/15mm)とし、以下の基準で評価する。
1N/15mm以上 : ○(良好な層間強度)
1N/15mm未満 : ×(層間強度が劣る)
(測定条件)
測定装置 : 島津製作所(株)製オートグラフ(AG−IS:ロードセルタイプ500N)
温湿度 : 温度23±2℃、湿度50±5%RH(JIS K 7000標準温度状態2級)
初期チャック間隔 : 40mm
サンプル幅 : 15mm
試験回数 : 3回
引張速度 : 200mm/分
前半削除範囲 : 50mm
感度 : 1
なお、上記層間強度は、積層構造の中で最も層間強度の弱い層間について評価するものとする。
[Methods for measuring physical properties and methods for evaluating effects]
(1) Interlaminar strength (before shrink processing)
Evaluation is performed using a shrink film.
A strip-shaped sample (200 mm (shrink film width direction) × 15 mm (shrink film length direction)) having a width of 15 mm in the length direction (shrink film forming direction) and long in the width direction (direction perpendicular to the length direction) is collected. did. Hereinafter, the sample width direction refers to the longitudinal direction of the shrink film.
Using the long side direction of the sample (the width direction of the shrink film) as the measurement direction, a T-type peel test (based on JIS K 6854-3) is performed under the following conditions to measure the peeling load between layers.
The average value of the peeling load is defined as the interlayer strength (N / 15 mm), and evaluated according to the following criteria.
1N / 15mm or more: ○ (good interlayer strength)
Less than 1 N / 15 mm: × (interlayer strength is inferior)
(Measurement condition)
Measuring device: Autograph manufactured by Shimadzu Corporation (AG-IS: load cell type 500N)
Temperature and humidity: Temperature 23 ± 2 ° C, humidity 50 ± 5% RH (JIS K 7000 standard temperature state 2nd grade)
Initial chuck interval: 40 mm
Sample width: 15mm
Number of tests: 3 times Tensile speed: 200 mm / min First half deleted range: 50 mm
Sensitivity: 1
The interlayer strength is evaluated for the interlayer having the weakest interlayer strength in the laminated structure.

(2)層間強度(シュリンク加工後)
得られたシュリンクフィルムを、治具を用いて、85℃にて30%フィルムを収縮させた後に評価に用いる。
上記サンプルを用いて、上記(1)の評価と同様の評価方法で層間強度を測定し、同様の基準で評価する。
(2) Interlaminar strength (after shrink processing)
The obtained shrink film is used for evaluation after shrinking the film by 30% at 85 ° C. using a jig.
Using the sample, the interlayer strength is measured by the same evaluation method as the evaluation of (1) above, and evaluated by the same standard.

(3)熱収縮率(90℃10秒)
シュリンクフィルム(シュリンク加工前)から、測定方向(主配向方向:基材フィルムの長手方向または幅方向)に長さ120mm(標線間隔100mm)、サンプルの幅5mmの長方形のサンプル片を作製する。
サンプル片を90℃の温水中で、10秒熱処理(無荷重下)し、熱処理前後の標線間隔の差を読み取り、以下の計算式で熱収縮率を算出する。
収縮率(%) = (L0−L1)/L0×100
0 : 熱処理前のサンプルの寸法(主配向方向:長手方向又は幅方向)
1 : 熱処理後のサンプルの寸法(L0と同じ方向)
(3) Thermal shrinkage (90 ° C for 10 seconds)
From the shrink film (before shrink processing), a rectangular sample piece having a length of 120 mm in the measurement direction (main orientation direction: longitudinal direction or width direction of the base film) and a sample width of 5 mm is prepared.
The sample piece is heat-treated in warm water at 90 ° C. for 10 seconds (under no load), the difference between the marked lines before and after the heat treatment is read, and the thermal contraction rate is calculated by the following formula.
Shrinkage rate (%) = (L 0 −L 1 ) / L 0 × 100
L 0 : Size of sample before heat treatment (main orientation direction: longitudinal direction or width direction)
L 1 : Sample dimensions after heat treatment (same direction as L 0 )

(4)圧縮強度(リングクラッシュ法)
シュリンクフィルム(シュリンク加工前)を用いて評価を行う。
JIS P 8126に準拠して、シュリンクラベルの圧縮強度を、以下の条件で、測定する。測定方向は長手方向である。
測定装置 : 島津製作所(株)製オートグラフ(AGS−50G:ロードセルタイプ500N)
サンプルサイズ : 15mm(長手方向)×152.4mm(幅方向)
試験回数: 5回
(4) Compressive strength (ring crush method)
Evaluation is performed using a shrink film (before shrink processing).
In accordance with JIS P 8126, the compressive strength of the shrink label is measured under the following conditions. The measurement direction is the longitudinal direction.
Measuring device: Shimadzu Corporation autograph (AGS-50G: load cell type 500N)
Sample size: 15 mm (longitudinal direction) x 152.4 mm (width direction)
Number of tests: 5

(5)透明度(ヘイズ値)
シュリンクフィルム(厚み40μm)を用いて、JIS K 7105に準じて測定を行う。なお、厚みが異なるフィルムの場合には40μm厚みに換算すればよい。
(5) Transparency (haze value)
Measurement is performed according to JIS K 7105 using a shrink film (thickness 40 μm). In the case of films having different thicknesses, the thickness may be converted to 40 μm.

以下に、実施例に基づいて、本発明をより詳細に説明するが、本発明はこれらの実施例により限定されるものではない。   EXAMPLES Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.

実施例1
樹脂組成物Aとして、非晶性芳香族ポリエステル樹脂(Eastman Chemical社製、商品名「Embrace」)100重量部と、可塑剤としてフタル酸ジオクチル(DOP)20重量部の混合樹脂を用いた。
また、樹脂組成物Bとして、SBS(旭化成(株)製、商品名「アサフレックス 830」)60重量部と、SBIS(旭化成(株)製、商品名「アサフレックス i−100」)40重量部の混合樹脂を用いた。
さらに、樹脂組成物Cとして、無水マレイン酸変性した水添スチレン系熱可塑性エラストマー(旭化成(株)製、商品名「タフテック M」)100重量部を用いた。
210℃に加熱した押出機aに上記樹脂組成物A、210℃に加熱した押出機bに上記樹脂組成物B、210℃に加熱した押出機cには上記樹脂組成物Cを投入した。上記3台の押出機を用いて、溶融押出を行った。押出機bから押出される樹脂が中心層、押出機cから押出される樹脂が中心層の両側となり、押出機aから押出される樹脂がさらにその両側となるように合流ブロックを用いて合流させ、Tダイ(スリット間隔0.7mm)より押出した後、25℃に冷却したキャスティングドラム上で急冷して、3種5層積層未延伸フィルムを得た。
次に、厚みを調整した未延伸フィルムを、幅方向に90℃で5.6倍延伸することにより、主に1軸方向に収縮する2軸延伸フィルムを得た。製膜速度を調節して、フィルムの総厚みが50μm(層厚み比:(2/1/8/1/2)のシュリンクフィルムを得た。
また、得られたシュリンクフィルムに、大日本インキ工業(株)製「ファインラップNTV」をグラビア印刷し、5μmの厚みで印刷層を形成し、シュリンクラベルを得た。
得られたシュリンクフィルムおよびシュリンクラベルは、90℃の熱水中に10秒浸漬して熱収縮させて層間剥離の有無を確認した。フィルム及びラベルは共に、層間剥離のない層間密着性に優れたものであった。
Example 1
As the resin composition A, a mixed resin of 100 parts by weight of an amorphous aromatic polyester resin (manufactured by Eastman Chemical, trade name “Embrac”) and 20 parts by weight of dioctyl phthalate (DOP) as a plasticizer was used.
As resin composition B, 60 parts by weight of SBS (manufactured by Asahi Kasei Co., Ltd., trade name “Asaflex 830”) and 40 parts by weight of SBIS (manufactured by Asahi Kasei Co., Ltd., trade name “Asaflex i-100”) The mixed resin was used.
Further, 100 parts by weight of maleic anhydride-modified hydrogenated styrene thermoplastic elastomer (manufactured by Asahi Kasei Co., Ltd., trade name “Tuftec M”) was used as the resin composition C.
The resin composition A was charged in the extruder a heated to 210 ° C., the resin composition B in the extruder b heated to 210 ° C., and the resin composition C in the extruder c heated to 210 ° C. Melt extrusion was performed using the above three extruders. The resin extruded from the extruder b is the center layer, the resin extruded from the extruder c is on both sides of the center layer, and the resin extruded from the extruder a is further joined on both sides using a merge block. After extruding from a T-die (slit interval 0.7 mm), it was rapidly cooled on a casting drum cooled to 25 ° C. to obtain a three-kind five-layer laminated unstretched film.
Next, the unstretched film whose thickness was adjusted was stretched 5.6 times at 90 ° C. in the width direction to obtain a biaxially stretched film that contracts mainly in the uniaxial direction. By adjusting the film forming speed, a shrink film having a total thickness of 50 μm (layer thickness ratio: (2/1/8/1/2)) was obtained.
Moreover, Dainippon Ink Industries Co., Ltd. "fine wrap NTV" was gravure-printed on the obtained shrink film, the printing layer was formed in thickness of 5 micrometers, and the shrink label was obtained.
The obtained shrink film and shrink label were immersed in hot water at 90 ° C. for 10 seconds and thermally contracted to confirm the presence or absence of delamination. Both the film and the label were excellent in interlayer adhesion without delamination.

実施例2
A層に用いる可塑剤をアジピン酸ジオクチル(DOA)に変更した以外は、実施例1と全く同様にして、シュリンクフィルムおよびシュリンクラベルを得た。
得られたシュリンクフィルムおよびシュリンクラベルは、90℃の熱水中に10秒浸漬して熱収縮させて層間剥離の有無を確認した。フィルム及びラベルは共に、層間剥離のない層間密着性に優れたものであった。
Example 2
A shrink film and a shrink label were obtained in exactly the same manner as in Example 1 except that the plasticizer used for the A layer was changed to dioctyl adipate (DOA).
The obtained shrink film and shrink label were immersed in hot water at 90 ° C. for 10 seconds and thermally contracted to confirm the presence or absence of delamination. Both the film and the label were excellent in interlayer adhesion without delamination.

比較例1
A層に可塑剤を用いなかった以外は、実施例1と全く同様にして、シュリンクフィルムおよびシュリンクラベルを得た。
得られたシュリンクフィルムおよびシュリンクラベルは、90℃の熱水中に10秒浸漬して熱収縮させて層間剥離の有無を確認した。フィルム及びラベルは共に、層間剥離があり層間密着性の劣るものであった。
Comparative Example 1
A shrink film and a shrink label were obtained in the same manner as in Example 1 except that no plasticizer was used for the A layer.
The obtained shrink film and shrink label were immersed in hot water at 90 ° C. for 10 seconds and thermally contracted to confirm the presence or absence of delamination. Both the film and the label had delamination and poor interlayer adhesion.

Claims (5)

非晶性芳香族ポリエステル系樹脂を主成分とし、非晶性芳香族ポリエステル系樹脂100重量部に対して可塑剤0.5〜20重量部を含有する樹脂組成物から構成される表面層(A層)、および、スチレン−共役ジエン共重合体及び/又はその水添物を主成分とする樹脂組成物から構成される中心層(B層)が、A層/B層/A層の順に積層された少なくとも3層積層構造を有することを特徴とするシュリンクフィルム。   A surface layer composed of a resin composition containing an amorphous aromatic polyester-based resin as a main component and containing 0.5 to 20 parts by weight of a plasticizer with respect to 100 parts by weight of the amorphous aromatic polyester-based resin (A Layer) and a central layer (B layer) composed of a resin composition mainly composed of a styrene-conjugated diene copolymer and / or a hydrogenated product thereof, is laminated in the order of A layer / B layer / A layer. A shrink film having a laminated structure of at least three layers. さらに、接着性樹脂層(C層)を有し、A層/C層/B層/C層/A層の順に積層された少なくとも5層積層構造を有する請求項1に記載のシュリンクフィルム。   Furthermore, the shrink film of Claim 1 which has an adhesive resin layer (C layer) and has at least 5 layer laminated structure laminated | stacked in order of A layer / C layer / B layer / C layer / A layer. 前記可塑剤がフタル酸エステル、アジピン酸エステル、ポリエステル系可塑剤から選ばれた少なくとも1つである請求項1または2に記載のシュリンクフィルム。   The shrink film according to claim 1, wherein the plasticizer is at least one selected from a phthalate ester, an adipate ester, and a polyester plasticizer. 前記C層が、極性基を有するスチレン系樹脂より構成される請求項1〜3のいずれかの項に記載のシュリンクフィルム。   The shrink film according to any one of claims 1 to 3, wherein the C layer is composed of a styrene resin having a polar group. 請求項1〜4のいずれかの項に記載のシュリンクフィルムの少なくとも一方の面側に印刷層を設けたシュリンクラベル。   The shrink label which provided the printing layer in the at least one surface side of the shrink film in any one of Claims 1-4.
JP2008018660A 2008-01-30 2008-01-30 Shrink film and shrink label Expired - Fee Related JP5049150B2 (en)