JP4940530B2
JP4940530B2 JP2003028609A JP2003028609A JP4940530B2 JP 4940530 B2 JP4940530 B2 JP 4940530B2 JP 2003028609 A JP2003028609 A JP 2003028609A JP 2003028609 A JP2003028609 A JP 2003028609A JP 4940530 B2 JP4940530 B2 JP 4940530B2
Authority
JP
Japan
Prior art keywords
transition metal
lithium
composite oxide
metal composite
lithium transition
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
JP2003028609A
Other languages
Japanese (ja)
Other versions
JP2004241242A (en
Inventor
卓朗 松下
弘康 江藤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nichia Corp
Original Assignee
Nichia Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nichia Corp filed Critical Nichia Corp
Priority to JP2003028609A priority Critical patent/JP4940530B2/en
Publication of JP2004241242A publication Critical patent/JP2004241242A/en
Application granted granted Critical
Publication of JP4940530B2 publication Critical patent/JP4940530B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Links

Images

Classifications

    • YGENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02EREDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
    • Y02E60/00Enabling technologies; Technologies with a potential or indirect contribution to GHG emissions mitigation
    • Y02E60/10Energy storage using batteries

Landscapes

  • Secondary Cells (AREA)
  • Battery Electrode And Active Subsutance (AREA)

Description

【0001】
【発明の属する技術分野】
本発明は非水電解液二次電池及びその正極活物質、特にスピネル構造のリチウム遷移金属複合酸化物に関する。例えば、携帯電話、パソコン、電気自動車に使用される。
【0002】
【従来の技術】
非水電解液二次電池は、従来のニッケルカドミウム二次電池などに比べて作動電圧が高く、かつエネルギー密度が高いという特徴を有し、電子機器の電源として広く利用されている。この非水電解液二次電池の正極活物質としてはLiCoO、LiNiO、LiMnに代表されるリチウム遷移金属複合酸化物が挙げられる。
【0003】
なかでもLiMnは、構成元素であるマンガンが資源として多量に存在するため、原料が安価に入手しやすい。また環境に対する負荷も少ないという特徴がある。さらにデインターカレーション反応によって、結晶中のLiイオンが全量脱離しても、結晶構造は安定に存在する。このためLiCoO、LiNiOに比べて、LiMnを用いた二次電池は、過充電状態において発熱が少ない。
【0004】
携帯電話やノート型パソコンに代表されるモバイル電子機器において、これまではLiMnを用いた非水電解液二次電池で十分な電池特性が得られていた。
【0005】
しかしながら、現在では、携帯電話、ノート型パソコン、デジタルカメラ等のモバイル機器は、さまざまな機能が付与される等の高機能化や、高温や低温での使用等のため、使用環境がより一層厳しいものとなっている。また、電気自動車用バッテリー等の電源への応用が期待されている。このような下において、これまでのLiMnを用いた非水電解液二次電池では、十分な電池特性が得られず、更なる改良が求められている。
【0006】
【発明が解決しようとする課題】
本発明の目的は、より一層厳しい使用環境下においても優れた電池特性を有する非水電解液二次電池用正極活物質を提供することにある。すなわち極板密度が向上し、充放電時のドライアウトを防止することができる非水電解液二次電池用正極活物質を提供することにある。
【0007】
【課題を解決するための手段】
本発明に記載される非水電解液二次電池用正極活物質は、少なくともスピネル構造のリチウム遷移金属複合酸化物を有する非水電解液二次電池用正極活物質であって、前記リチウム遷移金属複合酸化物は、少なくとも第1のリチウム遷移金属複合酸化物及び第2のリチウム遷移金属複合酸化物を有すると共に、該第1のリチウム遷移金属複合酸化物は、二次粒子径を大きくする元素及び/又は化合物を含有する第2のリチウム遷移金属複合酸化物よりも小さいことを特徴とする。
【0008】
極板密度の向上は、電池容量の向上に大きく関係している。極板密度はプレス圧を上げることで向上させることができる。しかしプレス圧を上げればリチウム遷移金属複合酸化物の粒子が壊れ、微粉が発生し、リチウム遷移金属複合酸化物の片寄りが起こり、ドライアウトという電解液の液枯れを引き起こす。ドライアウトは電池特性の低下の最大の原因となる。このドライアウトを防止するには粒径を大きくすることが好ましいが、大粒子のリチウム遷移金属複合酸化物は極板密度が低い。したがって、極板密度の向上とドライアウトの防止はトレードオフの関係にある。
【0009】
少なくとも2種以上のリチウム遷移金属複合酸化物を有し、少なくとも第1のリチウム遷移金属複合酸化物が第2のリチウム遷移金属複合酸化物よりも小さいことで、極板に対する充填性が向上し極板密度が向上する。第2のリチウム遷移金属複合酸化物にその二次粒子径を大きくする元素及び/又は化合物を含有することで、2種以上のリチウム遷移金属複合酸化物の粒子の大きさを制御することができる。これによりプレス圧を上げて極板密度を向上させても、ドライアウトを防止することができる非水電解液二次電池用正極活物質を得ることができる。
【0010】
前記第1のリチウム遷移金属複合酸化物は、前記第2のリチウム遷移金属複合酸化物よりも少ないことが好ましい。第1のリチウム遷移金属複合酸化物が、二次粒子径を大きくする元素及び/又は化合物を含有する第2のリチウム遷移金属複合酸化物よりも少ないことで、大粒子間に存在する小粒子の割合を制御することができる。これにより、より効果的に極板密度を向上させるとともに、ドライアウトを防止することができる。
【0011】
本発明に記載される非水電解液二次電池用正極活物質は、少なくともスピネル構造のリチウム遷移金属複合酸化物を有する非水電解液二次電池用正極活物質であって、前記リチウム遷移金属複合酸化物は、第1のマンガン酸リチウム及び第2のマンガン酸リチウムを有すると共に、該第1のマンガン酸リチウムは、ホウ素を含有する第2のマンガン酸リチウムよりも小さいことを特徴とする。
【0012】
少なくとも2種のマンガン酸リチウムを有し、少なくとも第1のマンガン酸リチウムが第2のマンガン酸リチウムよりも小さいことで、極板に対する充填性が向上し極板密度が向上する。第2のマンガン酸リチウムにホウ素を含有することで、2種のマンガン酸リチウムの粒子の大きさを制御することができる。これによりプレス圧を上げて極板密度を向上させても、ドライアウトを防止することができる非水電解液二次電池用正極活物質を得ることができる。
【0013】
前記第1のマンガン酸リチウムは、第2のマンガン酸リチウムよりも少ないことが好ましい。第1のマンガン酸リチウムが、ホウ素を含有する第2のマンガン酸リチウムよりも少ないことで、大粒子間に存在する小粒子の割合を制御することができる。これにより、より効果的に極板密度を向上させるとともに、ドライアウトを防止することができる。
【0014】
本発明に記載される非水電解液二次電池用正極活物質の製造方法は、少なくともスピネル構造のリチウム遷移金属複合酸化物を有する非水電解液二次電池用正極活物質の製造方法であって、第1の粒度分布を有し一次粒子径が10μm以下の範囲にあるリチウム遷移金属複合酸化物からなる第1の粒子群を選択する工程と、第1の粒度分布よりも大きな二次粒子径となる第2の粒度分布を有し一次粒子径が8μmから150μmの範囲にあるリチウム遷移金属複合酸化物からなる第2の粒子群を選択する工程と、前記選択された第1の粒子群であるリチウム遷移金属複合酸化物と選択された第2の粒子群であるリチウム遷移金属複合酸化物とを混合する工程と、を有することを特徴とする。
【0015】
これらの工程を経ることで、大粒子間に存在する小粒子の割合を制御することができる。したがって、高い極板密度を有するとともに、ドライアウトを防止することが可能な非水電解液二次電池用正極活物質を得ることができる。
【0016】
前記第2の粒子群であるリチウム遷移金属複合酸化物は、ホウ素が含まれることが好ましい。ホウ素を含有することで、マンガン酸リチウムの粒子の大きさを制御することができる。これによりプレス圧を上げて極板密度を向上させても、ドライアウトを防止することができる非水電解液二次電池用正極活物質を得ることができる。
【0017】
前記第1の粒度分布は、その二次粒子径が1μm〜50μmの範囲に調製されていることが好ましい。サイクル充放電特性の低下やドライアウトの原因となるマンガン溶出を防ぐことができ、プレス圧を上げて極板密度を向上させても、ドライアウトを防止することができる非水電解液二次電池用正極活物質を得ることができる。
【0018】
前記第2の粒度分布は、その二次粒子径が8μm〜150μmの範囲に調製されていることが好ましい。正極合剤作製時におけるリチウム遷移金属複合酸化物の粒子の沈降を防止することができ、プレス圧を上げて極板密度を向上させても、ドライアウトを防止することができる非水電解液二次電池用正極活物質を得ることができる。
【0019】
前記リチウム遷移金属複合酸化物は、一般式がLiMn3−a4+f(aは0.8≦a≦1.2を満たす数を表し、fは−0.5≦f≦0.5を満たす数を表す。)で表されることが好ましい。携帯電話や電動工具等に用いられる優れた過充電特性、極板密度を有する非水電解液二次電池用正極活物質が得られる。さらに、電池特性を低下させる原因となる充放電時のドライアウトを防止できるため、電気自動車に用いられる優れた非水電解液二次電池用正極活物質が得られる。
【0020】
前記第2の粒子群であるリチウム遷移金属複合酸化物の前記第1の粒子群であるリチウム遷移金属複合酸化物と前記第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、50重量%〜90重量%であり、前記第1の粒子群であるリチウム遷移金属複合酸化物の前記第1の粒子群であるリチウム遷移金属複合酸化物と前記第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、10重量%〜50重量%であることが好ましい。このように大粒子間に存在し得る小粒子の割合を制御することで、より効果的に極板密度を向上させるとともに、ドライアウトを防止することができる非水電解液二次電池用正極活物質を得ることができる。
【0021】
【発明の実施の形態】
以下、本発明に係る非水電解液二次電池用正極活物質を、実施の形態、実施例及び図1〜図14を用いて説明する。ただし、本発明は、この実施の形態、実施例及び図1〜図14に限定されない。
【0022】
(非水電解液二次電池用正極活物質)
本発明の非水電解液二次電池用正極活物質は、少なくともスピネル構造のリチウム遷移金属複合酸化物からなる。スピネル構造とは、複酸化物でAB型の化合物(AとBは金属元素)にみられる代表的結晶構造型の一つである。リチウムは8aサイト1の四面体サイトを占有し、酸素は32eサイト2を占有し、遷移金属は16dサイト3の八面体サイトを占有する。
【0023】
スピネル構造からなるリチウム遷移金属複合酸化物としては、マンガン酸リチウム、チタン酸リチウム等が挙げられる。好ましくはマンガン酸リチウムである。マンガン酸リチウムの場合、携帯電話や電動工具等に用いられる優れた過充電特性、極板密度を有する非水電解液二次電池用正極活物質が得られる。さらに、電池特性を低下させる原因となる充放電時のドライアウトを防止できるため、電気自動車に用いられる優れた非水電解液二次電池用正極活物質が得られる。
【0024】
本発明に係るリチウム遷移金属複合酸化物は、少なくとも第1のリチウム遷移金属複合酸化物及び第2のリチウム遷移金属複合酸化物を有すると共に、該第1のリチウム遷移金属複合酸化物は、二次粒子径を大きくする元素及び/又は化合物を含有する第2のリチウム遷移金属複合酸化物よりも小さい。
【0025】
本発明に係るリチウム遷移金属複合酸化物は、少なくとも第1のリチウム遷移金属複合酸化物及び第2のリチウム遷移金属複合酸化物を有する。第1のリチウム遷移金属複合酸化物と第2のリチウム遷移金属複合酸化物は、同種でも異種でもどちらでもよい。第1のリチウム遷移金属複合酸化物がマンガン酸リチウムであり、第2のリチウム遷移金属複合酸化物がチタン酸リチウムであってもよい。第1のリチウム遷移金属複合酸化物がチタン酸リチウムであり、第2のリチウム遷移金属複合酸化物がマンガン酸リチウムであってもよい。好ましくは、第1のリチウム遷移金属複合酸化物がマンガン酸リチウムであり、第2のリチウム遷移金属複合酸化物もマンガン酸リチウムのときである。このとき、携帯電話や電動工具等に用いられる優れた過充電特性、極板密度を有する非水電解液二次電池用正極活物質が得られる。さらに、電池特性を低下させる原因となる充放電時のドライアウトを防止できるため、電気自動車に用いられる優れた非水電解液二次電池用正極活物質が得られる。
【0026】
本発明に係る第1のリチウム遷移金属複合酸化物は、二次粒子径を大きくする元素及び/又は化合物を含有する第2のリチウム遷移金属複合酸化物よりも小さい。二次粒子径を大きくする元素及び/又は化合物として、好ましくはホウ素化合物、塩素化合物およびバナジウム化合物である。これらは、フラックスとしての効果があり充放電時のドライアウトを防止することができる。より好ましくはホウ素化合物である。
【0027】
ホウ素化合物としては、特に限定されない。例えば、ホウ酸、ホウ酸リチウム、ホウ化物、酸化ホウ素、リン酸ホウ素等が用いられる。好適には、ホウ酸およびホウ酸リチウムである。塩素化合物としては、特に限定されない。例えば、塩化リチウム、塩化ナトリウム、塩化水素、塩酸、酸化塩素、フッ化酸化塩素等が用いられる。好適には、塩化リチウムおよび塩化ナトリウムである。バナジウム化合物としては、特に限定されない。例えば、酸化バナジウム、塩化バナジウム、フッ化バナジウム、水酸化バナジウム等が用いられる。好適には、酸化バナジウムである。
【0028】
小さいとは、粒子径あるいは比表面積径が小さいことを意味する。粒子径には、一次粒子径および二次粒子径が含まれる。二次粒子径には中位径が含まれる。好ましくは二次粒子径、中位径が小さいことである。より好ましくは中位径が小さいことである。一般的なリチウム遷移金属複合酸化物の粒子は、リチウム遷移金属複合酸化物の結晶形を反映して成長した一次粒子と、これが凝集または焼結等で構成された二次粒子からなる。このような一次粒子の直径を一次粒子径といい、二次粒子の直径を二次粒子という。
【0029】
比表面積径の測定方法は、特に限定されない。例えば、空気透過法によるフィッシャー・サブ・シーブ・サイザー(F.S.S.S)を用いて測定することができる。中位径とは、二次粒子の粒度分布の体積累積頻度が50%に達する粒径を意味する。中位径の測定方法は、特に限定されない。例えば、レーザー回折散乱法により粒度分布を測定し、体積基準の粒子径の対数を用いた積算分布を求め、リチウム遷移金属複合酸化物粉末全体の50%を占めるときの粒子径、即ちオーバーサイズ50%の粒径として測定することができる。一次粒子径の測定方法は、特に限定されない。例えば、画像解析法(顕微鏡法)を用いて測定することができる。
【0030】
本発明に係るリチウム遷移金属複合酸化物は、少なくとも第1のリチウム遷移金属複合酸化物及び第2のリチウム遷移金属複合酸化物を有すると共に、該第1のリチウム遷移金属複合酸化物は、二次粒子径を大きくする元素及び/又は化合物を含有する第2のリチウム遷移金属複合酸化物よりも中位径が小さいことにより、極板密度が向上するとともに、ドライアウトを防止することができ、さらに過充電特性も向上した非水電解液二次電池用正極活物質を得ることができる。
【0031】
本発明に係る前記第1のリチウム遷移金属複合酸化物は、好適には前記第2のリチウム遷移金属複合酸化物よりも少ない。少ないとは、第1のリチウム遷移金属複合酸化物の第1のリチウム遷移金属複合酸化物と第2のリチウム遷移金属複合酸化物の合計に対する混合割合が、第2のリチウム遷移金属複合酸化物の第1のリチウム遷移金属複合酸化物と第2のリチウム遷移金属複合酸化物の合計に対する混合割合よりも少ないことをいう。また、第1のリチウム遷移金属複合酸化物の重量が、第2のリチウム遷移金属複合酸化物の重量よりも少なくてもよい。
【0032】
本発明に係るリチウム遷移金属複合酸化物は、第1のマンガン酸リチウム及び第2のマンガン酸リチウムを有すると共に、該第1のマンガン酸リチウムは、ホウ素を含有する第2のマンガン酸リチウムよりも小さい。
【0033】
本発明において、ホウ素は第2のマンガン酸リチウムに固溶していても、マンガン酸リチウムの粒子の表面にホウ素を有していてもよい。好ましくは、第1のマンガン酸リチウム及び第2のマンガン酸リチウムを有すると共に、該第1のマンガン酸リチウムは、粒子の表面にホウ素を有する第2のマンガン酸リチウムよりも小さいことを特徴とする非水電解液二次電池用正極活物質である。このとき、ホウ素はマンガン酸リチウムにおける電子の通りやすさを向上させるため、サイクル充放電特性、熱安定性が向上する。マンガン酸リチウムの粒子は一次粒子であっても、二次粒子であってもよい。
【0034】
ホウ素に代えてホウ素化合物であってもよい。ホウ素化合物としては、特に限定されない。例えば、ホウ酸、ホウ酸リチウム、ホウ化物、酸化ホウ素、リン酸ホウ素等が用いられる。好適には、ホウ酸およびホウ酸リチウムである。
【0035】
本発明において、ホウ素化合物は第2のマンガン酸リチウムに固溶していても、マンガン酸リチウムの粒子の表面にホウ素化合物を有していてもよい。好ましくは、第1のマンガン酸リチウム及び第2のマンガン酸リチウムを有すると共に、該第1のマンガン酸リチウムは、粒子の表面にホウ酸リチウムを有する第2のマンガン酸リチウムよりも小さいことを特徴とする非水電解液二次電池用正極活物質である。このとき、ホウ酸リチウムはマンガン酸リチウムにおける電子の通りやすさを向上させるため、サイクル充放電特性、熱安定性が向上する。マンガン酸リチウムの粒子は一次粒子であっても、二次粒子であってもよい。
【0036】
ホウ素及び/又はホウ酸リチウムはマンガン酸リチウムの粒子の表面にどのような形で存在していても本発明の効果を発揮する。例えば、ホウ素及び/又はホウ酸リチウムがマンガン酸リチウムの粒子の表面の全体に被膜されている場合であっても、ホウ素及び/又はホウ酸リチウムがマンガン酸リチウムの粒子の表面の一部に被覆されている場合であっても、サイクル充放電特性、熱安定性が向上する。
【0037】
より好ましくは、ホウ素及び/又はホウ酸リチウムがマンガン酸リチウムの粒子の表面の全体に被膜されている場合である。この場合、サイクル充放電特性、熱安定性だけでなく、保存特性も向上した非水電解液二次電池用正極活物質を得ることができる。
また、ホウ素及び/又はホウ酸リチウムは、少なくとも粒子の表面に存在していればよい。したがって、ホウ素及び/又はホウ酸リチウムが粒子の内部に存在していてもよい。
【0038】
ホウ酸及び/又はホウ酸リチウムがマンガン酸リチウムの粒子の表面に存在しているかどうかは、種々の方法によって解析できる。例えば、オージェ電子分光法(AES)、X線光電子分光法(XPS)で解析することができる。
【0039】
第2のマンガン酸リチウムに含有されるホウ素の量は、第2のマンガン酸リチウムに対して50ppm〜500ppmであることが好ましい。このとき本発明の効果が明確に表れる。好ましくは100ppm〜400ppmであり、より好ましくは150ppm〜350ppmである。このとき過充電特性を低下させることなく、極板密度が向上し、ドライアウトを防止することができる。
【0040】
小さいとは、粒子径あるいは比表面積径が小さいことを意味する。粒子径には、一次粒子径および二次粒子径が含まれる。二次粒子径には中位径が含まれる。好ましくは二次粒子径、中位径が小さいことである。より好ましくは中位径が小さいことである。一般的なマンガン酸リチウムの粒子は、マンガン酸リチウムの結晶形を反映して成長した一次粒子と、これが凝集または焼結等で構成された二次粒子からなる。このような一次粒子の直径を一次粒子径といい、二次粒子の直径を二次粒子という。
【0041】
本発明に係る前記第1のマンガン酸リチウムは、好適には前記第2のマンガン酸リチウムよりも少ない。少ないとは、第1のマンガン酸リチウムの第1のマンガン酸リチウムと第2のマンガン酸リチウムの合計に対する混合割合が、第2のマンガン酸リチウムの第1のマンガン酸リチウムと第2のマンガン酸リチウムの合計に対する混合割合よりも少ないことをいう。また、第1のマンガン酸リチウムの重量が、第2のマンガン酸リチウムの重量よりも少なくてもよい。
【0042】
本発明に係るマンガン酸リチウムは、好適には一般式がLiMn3−a4+f(aは0.8≦a≦1.2を満たす数を表し、fは−0.5≦f≦0.5を満たす数を表す。)で表される。一般式がLiMn3−a4+f(aは0.8≦a≦1.2を満たす数を表し、fは−0.5≦f≦0.5を満たす数を表す。)で表されるマンガン酸リチウムであることにより、携帯電話や電動工具等に用いられる優れた過充電特性、極板密度を有する非水電解液二次電池用正極活物質が得られる。さらに、電池特性を低下させる原因となる充放電時のドライアウトを防止できるため、電気自動車に用いられる優れた非水電解液二次電池用正極活物質が得られる。
【0043】
(非水電解液二次電池用正極活物質の製造方法)
本発明に係る非水電解液二次電池用正極活物質の製造方法は、第1の粒度分布を有し一次粒子径が10μm以下の範囲にあるリチウム遷移金属複合酸化物からなる第1の粒子群を選択する工程と、第1の粒度分布よりも大きな二次粒子径となる第2の粒度分布を有し一次粒子径が8μmから150μmの範囲にあるリチウム遷移金属複合酸化物からなる第2の粒子群を選択する工程と、前記選択された第1の粒子群であるリチウム遷移金属複合酸化物と選択された第2の粒子群であるリチウム遷移金属複合酸化物とを混合する工程とを有する。
【0044】
以下、本発明に係る非水電解液二次電池用正極活物質(Li1.072Mn1.914Mg0.010.0035)の製造方法を説明するが、上記工程以外は本製造方法に限定されない。
【0045】
所定の組成比のマンガンイオンとマグネシウムイオンを含む水溶液中に炭酸水素ナトリウム水溶液を加え、マンガンとマグネシウムを共沈させ、共沈物を得る。
【0046】
マンガン源は特に限定されない。基本的には水溶液を作りうる塩であればいずれも使用可能である。例えば塩化マンガン、ヨウ化マンガン、硫酸マンガン、硝酸マンガン等が用いられる。好適には、MnSO、MnCl等が用いられる。
【0047】
マグネシウム源は特に限定されない。基本的には水溶液を作りうる塩であればいずれも使用可能である。例えば塩化マグネシウム、ヨウ化マグネシウム、過塩素酸マグネシウム、硫酸マグネシウム、硝酸マグネシウム等が用いられる。好適には、MgSO、Mg(NO等が用いられる。
【0048】
また、炭酸水素ナトリウム水溶液を加えているが、これに限られるわけではなく、水酸化ナトリウム水溶液、水酸化カリウム水溶液、水酸化リチウム水溶液等のアルカリ溶液であればよい。
【0049】
次に、得られる共沈物を濾過、水洗後、乾燥したのち、第1の共沈物はそのままにし、第2の共沈物にはオルトホウ酸を所定量混合する。第1の共沈物は、炭酸リチウムを所定の組成比となるように混合し、空気中または弱酸化雰囲気にて、800℃〜1000℃の温度で5時間〜15時間焼成を行う。第2の共沈物は、炭酸リチウムを所定の組成比となるように混合し、空気中または弱酸化雰囲気にて、800℃〜1000℃の温度で5時間〜15時間焼成を行う。こうして第1の粒度分布を有し一次粒子径が10μm以下の範囲にあるリチウム遷移金属複合酸化物と、第2の粒度分布を有し一次粒子径が8μmから150μmの範囲にあるリチウム遷移金属複合酸化物を得る。図3から図6において、本発明における第1の粒度分布21と第2の粒度分布22を示す。
【0050】
第1の粒度分布を有し一次粒子が10μmを越えると小粒子と大粒子との差異が小さくなり好ましくない。好ましくは、第1の粒度分布を有し一次粒子径が2μmから8μmである。第2の粒度分布を有し一次粒子径が8μmより小さい、あるいは150μmより大きいと小粒子と大粒子のバランスを保つことが難しくなり、正極合剤作製時におけるリチウム遷移金属複合酸化物の粒子の沈降が生じるため好ましくない。好ましくは、第2の粒度分布を有し一次粒子径が10μmから80μmの範囲にあるリチウム遷移金属複合酸化物である。
【0051】
共沈物と混合するものは炭酸リチウムに限定されない。基本的にはリチウム化合物であればいずれも使用可能である。例えばフッ化リチウム、塩化リチウム、臭化リチウム、ヨウ化リチウム、酸化リチウム、過酸化リチウム、水酸化リチウム等が用いられる。好適にはLiCO、LiOH、LiOH・HO、LiO、LiCl、LiNO、LiSO、LiHCO、Li(CHCOO)等が用いられる。
【0052】
共沈物、リチウム化合物とともに、硫黄含有化合物、ハロゲン元素を含む化合物、等を混合してもよい。
【0053】
硫黄含有化合物は特に限定されない。例えば硫化物、ヨウ化硫黄、硫化水素、硫酸とその塩、硫化窒素等が用いられる。好適にはLiSO、MnSO、(NHSO、Al(SO、MgSO等が用いられる。
【0054】
ハロゲン元素を含む化合物は特に限定されない。例えば、フッ化水素、フッ化酸素、フッ化水素酸、塩化水素、塩酸、酸化塩素、フッ化酸化塩素、酸化臭素、フルオロ硫酸臭素、ヨウ化水素、酸化ヨウ素、過ヨウ素酸等が用いられる。好適には、NHF、NHCl、NHBr、NHI、LiF、LiCl、LiBr、LiI、MnF、MnCl、MnBr、MnI等が用いられる。
【0055】
焼成の温度は、好適には850℃〜950℃であり、また焼成の時間は8〜14時間が好ましい。焼成温度が800℃よりも低い場合、未反応の原料が非水電解液二次電池用正極活物質中に残留し、本発明の目的を達成できる十分な特性が得られない場合がある。また、1000℃よりも高い温度で焼成した場合、副生成物が生成しやすくなり、単位重量当たりの放電容量の低下、サイクル充放電特性の低下、動作電圧の低下を招く。焼成の時間は、5時間未満では原料混合物の粒子間の拡散反応が進行せず、目的とする非水電解液二次電池用正極活物質が得られない。また15時間より長く焼成を行うと焼結による粗大粒子が形成され、好ましくない。
【0056】
第1の粒度分布を有し一次粒子径が10μm以下の範囲にあるリチウム遷移金属複合酸化物からなる第1の粒子群を選択し、第1の粒度分布よりも大きな二次粒子径となる第2の粒度分布を有し一次粒子径が8μmから150μmの範囲にあるリチウム遷移金属複合酸化物からなる第2の粒子群からなる第2の粒子群を選択し、選択された第1の粒子群と第2の粒子群を混合する。
【0057】
第2の粒子群であるリチウム遷移金属複合酸化物は、ホウ素が含まれることが好ましい。本発明において、ホウ素は第2の粒子群であるリチウム遷移金属複合酸化物に固溶していても、リチウム遷移金属複合酸化物の粒子の表面にホウ素を有していてもよい。第2の粒子群であるリチウム遷移金属複合酸化物の粒子の表面にホウ素を有していれば、ホウ素はリチウム遷移金属複合酸化物における電子の通りやすさを向上させるため、サイクル充放電特性、高負荷特性が向上する。リチウム遷移金属複合酸化物の粒子は一次粒子であっても、二次粒子であってもよい。
【0058】
ホウ素に代えてホウ素化合物であってもよい。ホウ素化合物としては、特に限定されない。例えば、ホウ酸、ホウ酸リチウム、ホウ化物、酸化ホウ素、リン酸ホウ素等が用いられる。好適には、ホウ酸およびホウ酸リチウムである。
【0059】
本発明において、ホウ素化合物は第2の粒子群であるリチウム遷移金属複合酸化物に固溶していても、リチウム遷移金属複合酸化物の粒子の表面にホウ素化合物を有していてもよい。第2の粒子群であるリチウム遷移金属複合酸化物の粒子の表面にホウ酸リチウムを有していることが好ましい。このとき、ホウ酸リチウムはリチウム遷移金属複合酸化物における電子の通りやすさを向上させるため、サイクル充放電特性、高負荷特性が向上する。リチウム遷移金属複合酸化物の粒子は一次粒子であっても、二次粒子であってもよい。
【0060】
ホウ素及び/又はホウ酸リチウムはリチウム遷移金属複合酸化物の粒子の表面にどのような形で存在していても本発明の効果を発揮する。例えば、ホウ素及び/又はホウ酸リチウムがリチウム遷移金属複合酸化物の粒子の表面の全体に被膜されている場合であっても、ホウ素及び/又はホウ酸リチウムがリチウム遷移金属複合酸化物の粒子の表面の一部に被覆されている場合であっても、サイクル充放電特性、熱安定性が向上する。
【0061】
より好ましくは、ホウ素及び/又はホウ酸リチウムがリチウム遷移金属複合酸化物の粒子の表面の全体に被膜されている場合である。この場合、サイクル充放電特性、熱安定性だけでなく、保存特性も向上した非水電解液二次電池用正極活物質を得ることができる。
また、ホウ素及び/又はホウ酸リチウムは、少なくとも粒子の表面に存在していればよい。したがって、ホウ素及び/又はホウ酸リチウムが粒子の内部に存在していてもよい。
【0062】
ホウ酸及び/又はホウ酸リチウムがリチウム遷移金属複合酸化物の粒子の表面に存在しているかどうかは、種々の方法によって解析できる。例えば、オージェ電子分光法(AES)、X線光電子分光法(XPS)で解析することができる。
【0063】
第2の粒子群であるリチウム遷移金属複合酸化物に含有されるホウ素の量は、第2の粒子群であるリチウム遷移金属複合酸化物に対して50ppm〜500ppmであることが好ましい。このとき本発明の効果が明確に表れる。好ましくは100ppm〜400ppmであり、より好ましくは150ppm〜350ppmである。このとき過充電特性を低下させることなく、極板密度が向上し、ドライアウトを防止することができる。
【0064】
第1の粒度分布は、その二次粒子径が1μm〜50μmの範囲に調製されていることが好ましい。二次粒子径が1μmより小さければリチウム遷移金属複合酸化物の比表面積が増大し、サイクル充放電特性の低下やドライアウトの原因となるマンガン溶出が生じる。二次粒子径が50μmより大きければ小粒子として大粒子との混合に寄与することができなくなり、本発明の目的を達成するのに効果的でない。より好ましくは第1の粒度分布の二次粒子径が1μm〜30μmの範囲に調製されていることである。
【0065】
第2の粒度分布は、その二次粒子径が8μm〜150μmの範囲に調製されていることが好ましい。二次粒子径が8μmより小さければ大粒子として小粒子との混合に寄与することができなくなり、本発明の目的を達成するのに効果的でない。二次粒子径が150μmより大きければ正極合剤作製時におけるリチウム遷移金属複合酸化物の粒子の沈降が生じ好ましくない。より好ましくは第2の粒度分布の二次粒子径が10μm〜50μmの範囲に調製されていることである。
【0066】
リチウム遷移金属複合酸化物は、一般式がLiMn3−a−b4+f(Mはアルミニウム及び/又はマグネシウム、Aはチタン、ジルコニウムおよびハフニウムからなる群から選ばれる少なくとも1種を表し、Xはフッ素、塩素、臭素およびヨウ素からなる群から選ばれる少なくとも1種を表し、Bはホウ素を表し、Sは硫黄を表し、Dはナトリウム及び/又はカルシウムを表し、aは0.8≦a≦1.2を満たす数を表し、bは0≦b≦0.2を満たす数を表し、cは0≦c≦0.05を満たす数を表し、dは0≦d≦0.02を満たす数を表し、eは0≦e≦0.1を満たす数を表し、fは−0.5≦f≦0.5を満たす数を表し、gは0≦g≦0.1を満たす数を表し、hは0≦h≦0.015を満たす数を表す。)で表されることが好ましい。
【0067】
第2の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、50重量%〜90重量%であり、第1の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、10重量%〜50重量%であることが好ましい。混合割合がこの範囲でなければ、効率的に極板密度の上昇が望めない。また小粒子の混合割合が多い場合には、極板作製時のプレスによって極板表面がつぶれてしまい電解液の出入りが困難となり、ドライアウトが生じる。より好ましくは、第2の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、55重量%〜75重量%であり、第1の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、25重量%〜45重量%である。
【0068】
上記焼成により得られるリチウム遷移金属複合酸化物を乳鉢やボールミル、振動ミル、ピンミル等により粉砕しても構わない。上記方法によって比表面積が0.2m/g〜1.2m/gである本発明の非水電解液二次電池用正極活物質を得ることができる。
【0069】
以上の製造方法を使用することにより、目的とする非水電解液二次電池用正極活物質を得ることが可能である。
【0070】
なお、炭酸塩によるマンガンとマグネシウムの共沈により、Li1.072Mn1.914Mg0.010.0035を製造したが、マンガン化合物、マグネシウム化合物を所定の組成比となるように混合し、焼成して製造してもよい。
【0071】
(非水電解液二次電池)
本発明に係る非水電解液二次電池用正極活物質は、リチウムイオン二次電池、リチウムイオンポリマー二次電池等の非水電解液二次電池に好適に用いられる。
【0072】
非水電解液二次電池は、従来公知の非水電解液二次電池において、正極活物質を本発明の正極活物質とすればよく、他の構成は特に限定されない。本発明に係るリチウム遷移金属複合酸化物を主成分とする正極活物質層を備えた非水電解液二次電池であればよい。
【0073】
正極活物質として本発明の正極活物質とともにコバルト酸リチウム及び/又はニッケル酸リチウムを用いることにより過充電特性、熱安定性、安全性だけでなく、放電容量、負荷特性、出力特性にも優れた非水電解液二次電池を得ることができる。
【0074】
一般式がLi1+xCoO(xは−0.5≦x≦0.5を満たす数を表す。)で表されるコバルト酸リチウムが好ましい。前記コバルト酸リチウムは、その一部がマグネシウム、アルミニウム、カルシウム、バナジウム、チタン、クロム、マンガン、鉄、コバルト、ニッケル、銅、亜鉛、ストロンチウム、ジルコニウム、ニオブ、モリブデンおよびスズからなる群から選ばれる少なくとも1種で置換されていてもよい。
【0075】
一般式がLi1+xNiO(xは−0.5≦x≦0.5を満たす数を表す。)で表されるニッケル酸リチウムが好ましい。前記ニッケル酸リチウムは、その一部がマグネシウム、アルミニウム、カルシウム、バナジウム、チタン、クロム、マンガン、鉄、コバルト、ニッケル、銅、亜鉛、ストロンチウム、ジルコニウム、ニオブ、モリブデンおよびスズからなる群から選ばれる少なくとも1種で置換されていてもよい。
【0076】
本発明に係るリチウム遷移金属複合酸化物を主成分とする正極活物質を使用する正極は、好ましくは次のように製造される。本発明に係るリチウム遷移金属複合酸化物の粉末に、アセチレンブラック、黒鉛等のカーボン系導電剤、結着剤及び結着剤の溶媒または分散媒とを混合することにより正極合剤が形成される。前記正極合剤をスラリーまたは混練物とし、アルミニウム箔等の集電体12に塗布又は担持し、プレス圧延して正極活物質層を集電体12に形成する。
【0077】
結着剤にはポリフッ化ビニリデン、ポリテトラフルオロエチレン、ポリアミドアクリル樹脂等が使用できる。
【0078】
本発明に係るリチウム遷移金属複合酸化物は、導電剤粉末との混合性が良く、電池の内部抵抗は減少すると考えられる。このため充放電特性、特に放電容量が向上する。また結着剤と混練するときも、本発明のリチウム遷移金属複合酸化物は、流動性に優れ、また結着剤の高分子と絡まりやすく、優れた結着性を有する。さらに粗大粒子を含まず、球状であるため、作製した正極13の塗膜面の表面は平滑性に優れる。このため正極板の塗膜面は結着性に優れ剥がれにくく、また表面が平滑で充放電に伴う塗膜面表面のリチウムイオンの出入りが均一に行われるため、サイクル充放電特性において顕著な改善が得られる。
【0079】
例えば、負極活物質には金属リチウム、リチウム合金、又はリチウムイオンを吸蔵放出可能な化合物が使用できる。リチウム合金としては例えばLiAl合金,LiSn合金,LiPb合金などが使用できる。リチウムイオンを吸蔵放出可能な化合物としては例えばグラファイト,黒鉛などの炭素材料が使用できる。また酸化スズ、酸化チタン等のリチウムイオンを挿入・脱離することができる酸化物を用いてもよい。
【0080】
電解液としては作動電圧で変質、分解しない化合物であれば特に限定されず使用できる。溶媒として例えばジメトキシエタン,ジエトキシエタン,エチレンカーボネート,プロピレンカーボネート,ジメチルカーボネート,ジエチルカーボネート,エチルメチルカーボネート,メチルホルメート,γ−ブチロラクトン,2−メチルテトラヒドロフラン,ジメチルスルホキシド,スルホランなどの有機溶媒が使用でき、また前記した有機溶媒群から選ばれた2種類以上を混合して使用しても構わない。
【0081】
電解質としては例えば過塩素酸リチウム,四フッ化ホウ酸リチウム,四フッ化リン酸リチウム,トリフルオロメタン酸リチウムなどのリチウム塩などが使用できる。上記した溶媒と電解質とを混合して電解液として使用する。ここでゲル化剤などを添加し、ゲル状として使用してもよく、また吸湿性ポリマーに吸収させて使用しても構わない。更に無機系又は有機系のリチウムイオンの導電性を有する固体電解質を使用しても構わない。
【0082】
更にセパレーター14としてポリエチレン製、ポリプロピレン製等の多孔性膜等が使用できる。本発明に係る非水電解液二次電池用正極活物質、上記した負極活物質、電解液、セパレーターを用いて定法に従い非水電解液二次電池とする。これにより従来達成できなかった優れた電池特性が実現できる。
【0083】
また、本発明に係る非水電解液二次電池用正極活物質を正極活物質として用いた正極活物質層を帯状正極集電体の両面にそれぞれ形成することにより構成した帯状正極と、上記の負極活物質層の負極活物質層を帯状負極集電体の両面にそれぞれ形成することにより構成した帯状負極とをそれぞれ具備し、帯状正極と帯状負極とを帯状セパレータを介して積層した状態で多数回巻回することにより帯状正極と帯状負極との間に帯状セパレータが介在している渦巻型の巻回体を構成して非水電解液二次電池とすることができる。このように構成することで、製造工程が簡単であるとともに、正極活物質層および負極活物質層の割れや帯状セパレータからの剥離を生じ難く、電池容量を大きく、エネルギー密度を高くすることができる。特に本発明に係る非水電解液二次電池用正極活物質は、極板密度が高く充填性に優れ、かつ結合材となじみやすい。そのため高い充放電容量を有し、かつ結着性、表面の平滑性に優れた正極になるため、さらに正極活物質層の割れや剥がれを防ぐことができる。
【0084】
非水電解液二次電池の形状としては、円筒型でも、コイン型でも、角型等でもよい。
【0085】
(非水電解液二次電池の用途)
本発明に係る非水電解液二次電池用正極活物質を用いた非水電解液二次電池の用途は特に限定されない。例えばノートパソコン、ペン入力パソコン、ポケットパソコン、ノート型ワープロ、ポケットワープロ、電子ブックプレーヤ、携帯電話、コードレスフォン子機、電子手帳、電卓、液晶テレビ、電気シェーバ、電動工具、電子翻訳機、自動車電話、携帯プリンタ、トランシーバ、ページャ、ハンディターミナル、携帯コピー、音声入力機器、メモリカード、バックアップ電源、テープレコーダ、ラジオ、ヘッドホンステレオ、ハンディクリーナ、ポータブルCD、ビデオムービ、ナビゲーションシステムなどの機器用の電源に用いることができる。また照明機器、エアコン、テレビ、ステレオ、温水器、冷蔵庫、オーブン電子レンジ、食器洗い器、洗濯機、乾燥器、ゲーム機器、玩具、ロードコンディショナ、医療機器、自動車、電気自動車、ゴルフカート、電動カート、電力貯蔵システムなどの電源として使用することができる。また、民生用の他、軍需用、宇宙用としても使用することができる。
【0086】
以下、本発明に係る非水電解液二次電池用正極活物質について実施例を挙げて説明するが、この実施例に限定されるものではない。
【0087】
【実施例】
〔実施例1〕
所定の組成比のマンガンイオンとマグネシウムイオンを含む水溶液中に炭酸水素ナトリウム水溶液を加え、マンガンとマグネシウムを共沈させ、共沈物を得た。
得られた共沈物を濾過、水洗後、乾燥したのち、第1の共沈物はそのままにし、第2の共沈物にはオルトホウ酸を300ppm混合した。第1の共沈物は、炭酸リチウムを所定の組成比となるように混合し、大気雰囲気中にて、930℃の温度で12時間焼成を行った。第2の共沈物は、炭酸リチウムを所定の組成比となるように混合し、大気雰囲気中にて、930℃の温度で12時間焼成を行った。こうして第1の粒度分布を有し一次粒子径が4μmのリチウム遷移金属複合酸化物と、第2の粒度分布を有し一次粒子径が20μmの範囲にあるリチウム遷移金属複合酸化物を得た。
第1の粒度分布を有し一次粒子径が4μmのリチウム遷移金属複合酸化物からなる第1の粒子群を選択し、第2の粒度分布を有し一次粒子径が20μmの範囲にあるリチウム遷移金属複合酸化物からなる第2の粒子群からなる第2の粒子群を選択し、選択された第1の粒子群と第2の粒子群を混合した。第2の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、70重量%とし、第1の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、30重量%とした。こうしてLi1.072Mn1.914Mg0.010.0035が得られた。
【0088】
(非水電解液二次電池用正極活物質の評価)
本発明に係る非水電解液二次電池用正極活物質は、以下の方法により組成分析、比表面積、粒度分布の測定を行う。また試験電池を作製し、各評価を行う。
【0089】
(組成分析)
所定量の非水電解液二次電池用正極活物質を硝酸に溶解し、プラズマ発光分光(ICP)分析法により、ハロゲン元素、酸素以外の各構成元素の含有量の定量を行う。また所定量の非水電解液二次電池用正極活物質を純水に投入して撹拌し、上澄み水溶液を得る。アニオン選択性電極を指示電極に用いたイオンメーターにより、上澄み水溶液中のハロゲン元素を定量する。
【0090】
(粉末の評価)
非水電解液二次電池用正極活物質の比表面積は、窒素ガスを用いた定圧式BET吸着法により測定する。中位径は、レーザー回折散乱法により粒度分布を測定し、体積基準の粒子径の対数を用いた積算分布を求め、リチウム遷移金属複合酸化物粉末全体の50%を占めるときの粒子径、即ちオーバーサイズ50%の粒径として測定する。一次粒子径の測定は、画像解析法(顕微鏡法)を用いて測定する。
【0091】
(結晶子径の測定)
理学電気(株)社製のRINT2500Vを用いて測定する。X線源にはCuKα1を用い、管電流100mA、管電圧40kVにてX線回折パターンを測定する。(400)面に起因する回折ピークより以下の式で表されるシェラーの式によって算出される。
【0092】
【数1】

Figure 0004940530
【0093】
なお式中のDは結晶子の大きさ(Å)、Kはシェラー定数(βを積分幅より算出した場合はK=1.05)、λはX線源の波長(CuKα1=1.540562Å)、βは結晶子の大きさによる回折線の広がりの幅(radian)、θは回折角2θ/2(degree)を示す。
【0094】
(リチウムイオン二次電池の作製)
ポリフッ化ビニリデン5重量部を含有したノルマルメチルピロリドン溶液に正極活物質であるリチウム遷移金属複合酸化物粉末90重量部、導電剤として炭素粉末5重量部とを加え、混練してペーストを調製し、これをドクターブレード法にてアルミニウム極板に塗布し、乾燥して正極板とする。また負極活物質に炭素材料を用いて同様にして銅極板に塗布し、負極板を作製する。セパレーターに多孔性プロピレンフィルムを用い、電解液としてエチレンカーボネイト:ジエチルカーボネイト=1:1(体積比)の混合溶媒にLiPFを1mol/lの濃度で溶解した溶液を用いてリチウムイオン二次電池を作製する。本実施例では正極板、負極板、セパレータを薄いシート状に成形し、これらを巻回し、金属ラミネート樹脂フィルムの電池ケースに収納し、ラミネート型電池とする。
【0096】
(極板密度の測定)
正極活物質であるリチウム遷移金属複合酸化物粉末95重量部及びポリフッ化ビニリデン5重量部を含有したノルマルメチルピロリドン溶液とを混練してペーストを調製し、これをドクターブレード法にてアルミニウム極板に塗布し、乾燥して正極板とする。正極板を所定の大きさ(2×2.5cm)に裁断した後、一軸プレス機にて極板を加圧し、加圧後の極板の厚さと重量から極板密度を得る。
【0097】
(ドライアウトの評価)
正極活物質であるリチウム遷移金属複合酸化物粉末95重量部及びポリフッ化ビニリデン5重量部を含有したノルマルメチルピロリドン溶液とを混練してペーストを調製し、これをドクターブレード法にてアルミニウム極板に塗布し、乾燥して正極板とする。正極を所定の大きさに裁断した後一軸プレス機にて極板を加圧し、加圧後の正極板をガラス容器に入れてアルゴンボックス内でプロピレンカーボネート液に浸す。3分間真空にしてプロピレンカーボネート液を正極板に浸透させた後、アルゴンボックスから正極板を取り出し、正極板の時間毎の重量を量る。時間毎の正極板の重量から最初の正極板の重量を引いて、プロピレンカーボネート液の減少量を計算する。プロピレンカーボネートの減少量が多ければ、電解液の移動が容易であることになり、ドライアウトが防止できると判断できる。プロピレンカーボネートの減少量が少なければ、電解液の移動が困難であり、ドライアウトが生じやすいと判断できる。
【0098】
結果を表1、図1に示す。粒度分布を図3に示す。
【0099】
〔実施例2〕
所定の組成比のマンガンイオンとマグネシウムイオンを含む水溶液中に炭酸水素ナトリウム水溶液を加え、マンガンとマグネシウムを共沈させ、共沈物を得た。
得られた共沈物を濾過、水洗後、乾燥したのち、第1の共沈物はそのままにし、第2の共沈物にはオルトホウ酸を200ppm混合した。第1の共沈物は、炭酸リチウムを所定の組成比となるように混合し、大気雰囲気中にて、930℃の温度で12時間焼成を行った。第2の共沈物は、炭酸リチウムを所定の組成比となるように混合し、大気雰囲気中にて、930℃の温度で12時間焼成を行った。こうして第1の粒度分布を有し一次粒子径が4μmのリチウム遷移金属複合酸化物と、第2の粒度分布を有し一次粒子径が15μmの範囲にあるリチウム遷移金属複合酸化物を得た。
第1の粒度分布を有し一次粒子径が4μmのリチウム遷移金属複合酸化物からなる第1の粒子群を選択し、第2の粒度分布を有し一次粒子径が15μmの範囲にあるリチウム遷移金属複合酸化物からなる第2の粒子群からなる第2の粒子群を選択し、選択された第1の粒子群と第2の粒子群を混合した。第2の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、70重量%とし、第1の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、30重量%とした。こうしてLi1.073Mn1.915Mg0.010.0023が得られた。
【0100】
粒度分布を図4に示す。
【0101】
〔実施例3〕
所定の組成比のマンガンイオンとマグネシウムイオンを含む水溶液中に炭酸水素ナトリウム水溶液を加え、マンガンとマグネシウムを共沈させ、共沈物を得た。
得られた共沈物を濾過、水洗後、乾燥したのち、第1の共沈物はそのままにし、第2の共沈物にはオルトホウ酸を100ppm混合した。第1の共沈物は、炭酸リチウムを所定の組成比となるように混合し、大気雰囲気中にて、930℃の温度で12時間焼成を行った。第2の共沈物は、炭酸リチウムを所定の組成比となるように混合し、大気雰囲気中にて、930℃の温度で12時間焼成を行った。こうして第1の粒度分布を有し一次粒子径が4μmのリチウム遷移金属複合酸化物と、第2の粒度分布を有し一次粒子径が8μmの範囲にあるリチウム遷移金属複合酸化物を得た。
第1の粒度分布を有し一次粒子径が4μmのリチウム遷移金属複合酸化物からなる第1の粒子群を選択し、第2の粒度分布を有し一次粒子径が8μmの範囲にあるリチウム遷移金属複合酸化物からなる第2の粒子群からなる第2の粒子群を選択し、選択された第1の粒子群と第2の粒子群を混合した。第2の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、70重量%とし、第1の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、30重量%とした。こうしてLi1.073Mn1.916Mg0.010.0012が得られた。
【0102】
以下、実施例1と同様にして非水電解液二次電池用正極活物質の評価を行った。結果を表1、図1に示す。粒度分布を図5に示す。
【0103】
〔実施例4〕
所定の組成比のマンガンイオンとマグネシウムイオンを含む水溶液中に炭酸水素ナトリウム水溶液を加え、マンガンとマグネシウムを共沈させ、共沈物を得た。
得られた共沈物を濾過、水洗後、乾燥したのち、第1の共沈物はそのままにし、第2の共沈物にはオルトホウ酸を300ppm混合した。第1の共沈物は、炭酸リチウムを所定の組成比となるように混合し、大気雰囲気中にて、930℃の温度で12時間焼成を行った。第2の共沈物は、炭酸リチウムを所定の組成比となるように混合し、大気雰囲気中にて、930℃の温度で12時間焼成を行った。こうして第1の粒度分布を有し一次粒子径が4μmのリチウム遷移金属複合酸化物と、第2の粒度分布を有し一次粒子径が20μmの範囲にあるリチウム遷移金属複合酸化物を得た。
第1の粒度分布を有し一次粒子径が4μmのリチウム遷移金属複合酸化物からなる第1の粒子群を選択し、第2の粒度分布を有し一次粒子径が20μmの範囲にあるリチウム遷移金属複合酸化物からなる第2の粒子群からなる第2の粒子群を選択し、選択された第1の粒子群と第2の粒子群を混合した。第2の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、60重量%とし、第1の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、40重量%とした。こうしてLi1.072Mn1.915Mg0.010.003が得られた。
【0104】
粒度分布を図6に示す。
【0105】
〔比較例1〕
所定の組成比のマンガンイオンとマグネシウムイオンを含む水溶液中に炭酸水素ナトリウム水溶液を加え、マンガンとマグネシウムを共沈させ、共沈物を得た。
得られた共沈物を濾過、水洗後、乾燥したのち、炭酸リチウムを所定の組成比となるように混合し、大気雰囲気中にて930℃で12時間焼成した。そして乳鉢にて粉砕しLi1.073Mn1.917Mg0.01が得られた。
【0106】
以下、実施例1と同様にして非水電解液二次電池用正極活物質の評価を行った。結果を表1、図1に示す。粒度分布を図7に示す。
【0111】
表1及び図1から明らかなように、本発明の非水電解液二次電池用正極活物質は、極板密度が比較例1に比べて向上していることがわかる。またドライアウトも防止できていることがわかる。
【0112】
これに対して、比較例1は、極板密度が本発明の非水電解液二次電池用正極活物質に比べて劣っている。また、ドライアウトも防止できていない。
【0113】
【表1】
Figure 0004940530
【0114】
また実施例1、実施例2および実施例3において、それぞれ第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の混合割合を変化させて、変化させたときの極板密度を測定した。結果を表2〜表4、図2に示す。
【0115】
【表2】
Figure 0004940530
【0116】
【表3】
Figure 0004940530
【0117】
【表4】
Figure 0004940530
【0118】
この結果から、第2の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、60重量%〜70重量%であり、第1の粒子群であるリチウム遷移金属複合酸化物の第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の合計に対する混合割合は、30重量%〜40重量%であることがより好ましいことがわかる。
【0129】
以上に説明したように、本発明の非水電解液二次電池用正極活物質は、極板密度が向上するとともにドライアウトを防止することができ優れた電池特性を有する。したがって、本発明の非水電解液二次電池用正極活物質は、リチウムイオン二次電池等の非水電解液二次電池に好適に用いられる。
【図面の簡単な説明】
【図1】プレス圧の変化に伴う極板密度の変化を示す図である。
【図2】第1の粒子群であるリチウム遷移金属複合酸化物と第2の粒子群であるリチウム遷移金属複合酸化物の混合割合の変化に伴う極板密度の変化を示す図である。
【図3】実施例1の粒度分布を示す図である。
【図4】実施例2の粒度分布を示す図である。
【図5】実施例3の粒度分布を示す図である。
【図6】実施例4の粒度分布を示す図である。
【図7】比較例1の粒度分布を示す図である。
【図8】比較例2の粒度分布を示す図である。
【図9】比較例3の粒度分布を示す図である。
【図10】スピネル構造のリチウム遷移金属複合酸化物を示す図である。
【図11】活物質の結着模式図である。
【図12】円筒型電池の断面図である。
【図13】コイン型電池の構造を示す図である。
【図14】角型電池の構造を示す図である。
【符号の説明】
1…8aサイト
2…32eサイト
3…16dサイト
4…結着剤
5…活物質
11…負極
12…集電体
13…正極
14…セパレーター
21…第1の粒度分布
22…第2の粒度分布[0001]
BACKGROUND OF THE INVENTION
The present invention relates to a non-aqueous electrolyte secondary battery and a positive electrode active material thereof, in particular, a lithium transition metal composite oxide having a spinel structure. For example, it is used for mobile phones, personal computers, and electric vehicles.
[0002]
[Prior art]
Non-aqueous electrolyte secondary batteries are characterized by higher operating voltage and higher energy density than conventional nickel cadmium secondary batteries, and are widely used as power sources for electronic devices. As the positive electrode active material of this non-aqueous electrolyte secondary battery, LiCoO2, LiNiO2, LiMn2O4And lithium transition metal composite oxides represented by
[0003]
Among them, LiMn2O4Since manganese, which is a constituent element, is present in a large amount as a resource, raw materials are easily available at low cost. In addition, there is a feature that the load on the environment is small. Furthermore, even if all the Li ions in the crystal are desorbed by the deintercalation reaction, the crystal structure exists stably. For this reason, LiCoO2, LiNiO2Compared to LiMn2O4The secondary battery using the battery generates little heat in an overcharged state.
[0004]
In mobile electronic devices such as mobile phones and notebook computers, so far LiMn2O4Sufficient battery characteristics were obtained with a non-aqueous electrolyte secondary battery using the above.
[0005]
However, at present, mobile devices such as mobile phones, notebook computers, and digital cameras have a more severe usage environment due to high functionality such as the addition of various functions and use at high and low temperatures. It has become a thing. In addition, application to power sources such as batteries for electric vehicles is expected. Under such circumstances, the conventional LiMn2O4In a non-aqueous electrolyte secondary battery using, sufficient battery characteristics cannot be obtained, and further improvements are required.
[0006]
[Problems to be solved by the invention]
The objective of this invention is providing the positive electrode active material for non-aqueous-electrolyte secondary batteries which has the outstanding battery characteristic also in the severer use environment. That is, an object of the present invention is to provide a positive electrode active material for a non-aqueous electrolyte secondary battery that can improve the electrode plate density and prevent dry-out during charging and discharging.
[0007]
[Means for Solving the Problems]
The positive electrode active material for a non-aqueous electrolyte secondary battery described in the present invention is a positive electrode active material for a non-aqueous electrolyte secondary battery having at least a lithium transition metal composite oxide having a spinel structure, and the lithium transition metal The composite oxide includes at least a first lithium transition metal composite oxide and a second lithium transition metal composite oxide, and the first lithium transition metal composite oxide includes an element that increases a secondary particle size, and It is smaller than the 2nd lithium transition metal complex oxide containing a compound.
[0008]
The improvement of the electrode plate density is greatly related to the improvement of the battery capacity. The electrode plate density can be improved by increasing the pressing pressure. However, when the press pressure is increased, the lithium transition metal composite oxide particles are broken, fine powder is generated, the lithium transition metal composite oxide is displaced, and dry-out of the electrolyte solution is caused. Dryout is the biggest cause of deterioration of battery characteristics. In order to prevent this dry-out, it is preferable to increase the particle size, but the large particle lithium transition metal composite oxide has a low electrode plate density. Therefore, there is a trade-off between improving the electrode plate density and preventing dryout.
[0009]
Having at least two or more types of lithium transition metal composite oxide, and at least the first lithium transition metal composite oxide being smaller than the second lithium transition metal composite oxide, the filling property to the electrode plate is improved and the electrode The plate density is improved. By containing an element and / or compound that increases the secondary particle size in the second lithium transition metal composite oxide, the size of the two or more lithium transition metal composite oxide particles can be controlled. . As a result, a positive electrode active material for a non-aqueous electrolyte secondary battery that can prevent dry-out can be obtained even if the press plate pressure is increased to improve the electrode plate density.
[0010]
The first lithium transition metal composite oxide is preferably less than the second lithium transition metal composite oxide. Since the first lithium transition metal composite oxide is smaller than the second lithium transition metal composite oxide containing an element and / or compound that increases the secondary particle size, the small particles existing between the large particles The ratio can be controlled. As a result, the electrode plate density can be improved more effectively and dry-out can be prevented.
[0011]
The positive electrode active material for a non-aqueous electrolyte secondary battery described in the present invention is a positive electrode active material for a non-aqueous electrolyte secondary battery having at least a lithium transition metal composite oxide having a spinel structure, and the lithium transition metal The composite oxide has a first lithium manganate and a second lithium manganate, and the first lithium manganate is smaller than the second lithium manganate containing boron.
[0012]
When at least two types of lithium manganate are included and at least the first lithium manganate is smaller than the second lithium manganate, the filling property of the electrode plate is improved and the electrode plate density is improved. By containing boron in the second lithium manganate, the size of the two types of lithium manganate particles can be controlled. As a result, a positive electrode active material for a non-aqueous electrolyte secondary battery that can prevent dry-out can be obtained even if the press plate pressure is increased to improve the electrode plate density.
[0013]
The first lithium manganate is preferably less than the second lithium manganate. Since the first lithium manganate is less than the second lithium manganate containing boron, the proportion of small particles existing between large particles can be controlled. As a result, the electrode plate density can be improved more effectively and dry-out can be prevented.
[0014]
The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery described in the present invention is a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery having at least a spinel-structure lithium transition metal composite oxide. Selecting a first particle group comprising a lithium transition metal composite oxide having a first particle size distribution and a primary particle size in the range of 10 μm or less, and secondary particles larger than the first particle size distribution Selecting a second particle group comprising a lithium transition metal composite oxide having a second particle size distribution as a diameter and a primary particle diameter in the range of 8 μm to 150 μm, and the selected first particle group And a step of mixing the lithium transition metal composite oxide which is the selected second particle group and the lithium transition metal composite oxide.
[0015]
By passing through these steps, the proportion of small particles existing between large particles can be controlled. Therefore, it is possible to obtain a positive electrode active material for a non-aqueous electrolyte secondary battery that has a high electrode plate density and can prevent dryout.
[0016]
The lithium transition metal composite oxide that is the second particle group preferably contains boron. By containing boron, the size of the lithium manganate particles can be controlled. As a result, a positive electrode active material for a non-aqueous electrolyte secondary battery that can prevent dry-out can be obtained even if the press plate pressure is increased to improve the electrode plate density.
[0017]
The first particle size distribution is preferably prepared such that the secondary particle size is in the range of 1 μm to 50 μm. Non-aqueous electrolyte secondary battery that can prevent degradation of cycle charge / discharge characteristics and elution of manganese that causes dryout, and can prevent dryout even if the press plate pressure is increased to increase the electrode plate density A positive electrode active material can be obtained.
[0018]
The second particle size distribution is preferably prepared such that its secondary particle size is in the range of 8 μm to 150 μm. Non-aqueous electrolyte solution that can prevent the precipitation of lithium transition metal composite oxide particles during the preparation of the positive electrode mixture, and can prevent dry-out even if the press plate pressure is increased to increase the electrode plate density. A positive electrode active material for a secondary battery can be obtained.
[0019]
The lithium transition metal composite oxide has a general formula of LiaMn3-aO4 + f(A represents a number satisfying 0.8 ≦ a ≦ 1.2, and f represents a number satisfying −0.5 ≦ f ≦ 0.5). A positive electrode active material for a non-aqueous electrolyte secondary battery having excellent overcharge characteristics and electrode plate density used for mobile phones and electric tools can be obtained. Furthermore, since the dry-out at the time of charging / discharging which becomes the cause of reducing a battery characteristic can be prevented, the positive electrode active material for nonaqueous electrolyte secondary batteries used for an electric vehicle is obtained.
[0020]
The mixing ratio of the lithium transition metal composite oxide which is the first particle group and the lithium transition metal composite oxide which is the second particle group of the lithium transition metal composite oxide which is the second particle group is 50% by weight to 90% by weight of the lithium transition metal composite oxide which is the first particle group of the lithium transition metal composite oxide which is the first particle group and the lithium which is the second particle group The mixing ratio with respect to the total of the transition metal composite oxides is preferably 10% by weight to 50% by weight. In this way, by controlling the proportion of small particles that can exist between large particles, it is possible to more effectively improve the electrode plate density and prevent dryout, and the positive electrode active for a non-aqueous electrolyte secondary battery. A substance can be obtained.
[0021]
DETAILED DESCRIPTION OF THE INVENTION
Hereinafter, the positive electrode active material for a non-aqueous electrolyte secondary battery according to the present invention will be described with reference to embodiments, examples, and FIGS. However, the present invention is not limited to this embodiment, examples, and FIGS.
[0022]
(Positive electrode active material for non-aqueous electrolyte secondary battery)
The positive electrode active material for a non-aqueous electrolyte secondary battery of the present invention comprises at least a lithium transition metal composite oxide having a spinel structure. Spinel structure is a double oxide AB2O4This is one of the typical crystal structure types found in type compounds (A and B are metal elements). Lithium occupies the tetrahedral site of the 8a site 1, oxygen occupies the 32e site 2, and the transition metal occupies the octahedral site of the 16d site 3.
[0023]
Examples of the lithium transition metal composite oxide having a spinel structure include lithium manganate and lithium titanate. Lithium manganate is preferable. In the case of lithium manganate, a positive electrode active material for a non-aqueous electrolyte secondary battery having excellent overcharge characteristics and electrode plate density used for mobile phones and electric tools can be obtained. Furthermore, since the dry-out at the time of charging / discharging which becomes the cause of reducing a battery characteristic can be prevented, the positive electrode active material for nonaqueous electrolyte secondary batteries used for an electric vehicle is obtained.
[0024]
The lithium transition metal composite oxide according to the present invention has at least a first lithium transition metal composite oxide and a second lithium transition metal composite oxide, and the first lithium transition metal composite oxide has a secondary It is smaller than the 2nd lithium transition metal complex oxide containing the element and / or compound which enlarges a particle diameter.
[0025]
The lithium transition metal composite oxide according to the present invention includes at least a first lithium transition metal composite oxide and a second lithium transition metal composite oxide. The first lithium transition metal composite oxide and the second lithium transition metal composite oxide may be the same or different. The first lithium transition metal composite oxide may be lithium manganate, and the second lithium transition metal composite oxide may be lithium titanate. The first lithium transition metal composite oxide may be lithium titanate, and the second lithium transition metal composite oxide may be lithium manganate. Preferably, the first lithium transition metal composite oxide is lithium manganate, and the second lithium transition metal composite oxide is also lithium manganate. At this time, a positive electrode active material for a non-aqueous electrolyte secondary battery having excellent overcharge characteristics and electrode plate density used for mobile phones and electric tools is obtained. Furthermore, since the dry-out at the time of charging / discharging which becomes the cause of reducing a battery characteristic can be prevented, the positive electrode active material for nonaqueous electrolyte secondary batteries used for an electric vehicle is obtained.
[0026]
The 1st lithium transition metal complex oxide which concerns on this invention is smaller than the 2nd lithium transition metal complex oxide containing the element and / or compound which enlarges a secondary particle diameter. As the element and / or compound for increasing the secondary particle size, boron compounds, chlorine compounds and vanadium compounds are preferable. These have an effect as a flux and can prevent dryout during charging and discharging. More preferred is a boron compound.
[0027]
The boron compound is not particularly limited. For example, boric acid, lithium borate, boride, boron oxide, boron phosphate or the like is used. Preferred are boric acid and lithium borate. The chlorine compound is not particularly limited. For example, lithium chloride, sodium chloride, hydrogen chloride, hydrochloric acid, chlorine oxide, fluorinated chlorine oxide, or the like is used. Lithium chloride and sodium chloride are preferred. The vanadium compound is not particularly limited. For example, vanadium oxide, vanadium chloride, vanadium fluoride, vanadium hydroxide, or the like is used. Vanadium oxide is preferred.
[0028]
Small means that the particle diameter or specific surface area diameter is small. The particle diameter includes a primary particle diameter and a secondary particle diameter. The secondary particle diameter includes the median diameter. Preferably, the secondary particle diameter and the median diameter are small. More preferably, the median diameter is small. General lithium transition metal composite oxide particles are composed of primary particles grown reflecting the crystal form of the lithium transition metal composite oxide, and secondary particles formed by aggregation or sintering. The diameter of such a primary particle is called a primary particle diameter, and the diameter of a secondary particle is called a secondary particle.
[0029]
The method for measuring the specific surface area diameter is not particularly limited. For example, it can be measured using a Fischer sub-sieve sizer (FSSS) by the air permeation method. The median diameter means a particle diameter at which the volume cumulative frequency of the particle size distribution of the secondary particles reaches 50%. The method for measuring the median diameter is not particularly limited. For example, the particle size distribution is measured by a laser diffraction scattering method, an integrated distribution using the logarithm of the volume-based particle diameter is obtained, and the particle diameter when occupying 50% of the entire lithium transition metal composite oxide powder, that is, oversize 50 % Particle size. The measuring method of a primary particle diameter is not specifically limited. For example, it can be measured using an image analysis method (microscope method).
[0030]
The lithium transition metal composite oxide according to the present invention has at least a first lithium transition metal composite oxide and a second lithium transition metal composite oxide, and the first lithium transition metal composite oxide has a secondary Since the median diameter is smaller than that of the second lithium transition metal composite oxide containing an element and / or compound that increases the particle diameter, the electrode plate density can be improved and dry out can be prevented. A positive electrode active material for a non-aqueous electrolyte secondary battery with improved overcharge characteristics can be obtained.
[0031]
The first lithium transition metal composite oxide according to the present invention is preferably less than the second lithium transition metal composite oxide. Less is that the mixing ratio of the first lithium transition metal composite oxide to the total of the first lithium transition metal composite oxide and the second lithium transition metal composite oxide is that of the second lithium transition metal composite oxide. It means being less than the mixing ratio with respect to the total of the first lithium transition metal composite oxide and the second lithium transition metal composite oxide. Further, the weight of the first lithium transition metal composite oxide may be less than the weight of the second lithium transition metal composite oxide.
[0032]
The lithium transition metal composite oxide according to the present invention has a first lithium manganate and a second lithium manganate, and the first lithium manganate is more than the second lithium manganate containing boron. small.
[0033]
In the present invention, boron may be dissolved in the second lithium manganate or may be present on the surface of the lithium manganate particles. Preferably, it has a first lithium manganate and a second lithium manganate, and the first lithium manganate is smaller than the second lithium manganate having boron on the surface of the particles. It is a positive electrode active material for non-aqueous electrolyte secondary batteries. At this time, since boron improves the ease of passing electrons in lithium manganate, cycle charge / discharge characteristics and thermal stability are improved. The lithium manganate particles may be primary particles or secondary particles.
[0034]
A boron compound may be used instead of boron. The boron compound is not particularly limited. For example, boric acid, lithium borate, boride, boron oxide, boron phosphate or the like is used. Preferred are boric acid and lithium borate.
[0035]
In the present invention, the boron compound may be dissolved in the second lithium manganate or may have a boron compound on the surface of the lithium manganate particles. Preferably, the first lithium manganate and the second lithium manganate are included, and the first lithium manganate is smaller than the second lithium manganate having lithium borate on the surface of the particles. And a positive electrode active material for a non-aqueous electrolyte secondary battery. At this time, since lithium borate improves the ease of passing electrons in lithium manganate, cycle charge / discharge characteristics and thermal stability are improved. The lithium manganate particles may be primary particles or secondary particles.
[0036]
Even if boron and / or lithium borate are present on the surface of the lithium manganate particles, the effect of the present invention is exhibited. For example, even when boron and / or lithium borate is coated on the entire surface of the lithium manganate particle, boron and / or lithium borate is coated on a part of the surface of the lithium manganate particle. Even if it is carried out, cycle charge / discharge characteristics and thermal stability are improved.
[0037]
More preferably, boron and / or lithium borate is coated on the entire surface of the lithium manganate particles. In this case, it is possible to obtain a positive electrode active material for a non-aqueous electrolyte secondary battery in which not only cycle charge / discharge characteristics and thermal stability but also storage characteristics are improved.
Further, boron and / or lithium borate may be present at least on the surface of the particles. Therefore, boron and / or lithium borate may be present inside the particles.
[0038]
Whether boric acid and / or lithium borate is present on the surface of the lithium manganate particles can be analyzed by various methods. For example, analysis can be performed by Auger electron spectroscopy (AES) or X-ray photoelectron spectroscopy (XPS).
[0039]
The amount of boron contained in the second lithium manganate is preferably 50 ppm to 500 ppm with respect to the second lithium manganate. At this time, the effect of the present invention is clearly shown. Preferably it is 100 ppm-400 ppm, More preferably, it is 150 ppm-350 ppm. At this time, the electrode plate density is improved and dry-out can be prevented without deteriorating the overcharge characteristics.
[0040]
Small means that the particle diameter or specific surface area diameter is small. The particle diameter includes a primary particle diameter and a secondary particle diameter. The secondary particle diameter includes the median diameter. Preferably, the secondary particle diameter and the median diameter are small. More preferably, the median diameter is small. General lithium manganate particles are composed of primary particles grown reflecting the crystal form of lithium manganate and secondary particles formed by aggregation or sintering. The diameter of such a primary particle is called a primary particle diameter, and the diameter of a secondary particle is called a secondary particle.
[0041]
The first lithium manganate according to the present invention is preferably less than the second lithium manganate. The small amount means that the mixing ratio of the first lithium manganate to the total of the first lithium manganate and the second lithium manganate is such that the first lithium manganate and the second manganate are mixed with the second lithium manganate. It means less than the mixing ratio with respect to the total of lithium. The weight of the first lithium manganate may be less than the weight of the second lithium manganate.
[0042]
The lithium manganate according to the present invention preferably has the general formula LiaMn3-aO4 + f(A represents a number satisfying 0.8 ≦ a ≦ 1.2, and f represents a number satisfying −0.5 ≦ f ≦ 0.5). The general formula is LiaMn3-aO4 + f(A represents a number satisfying 0.8 ≦ a ≦ 1.2, and f represents a number satisfying −0.5 ≦ f ≦ 0.5). A positive electrode active material for a non-aqueous electrolyte secondary battery having excellent overcharge characteristics and electrode plate density used for telephones, electric tools and the like can be obtained. Furthermore, since the dry-out at the time of charging / discharging which becomes the cause of reducing a battery characteristic can be prevented, the positive electrode active material for nonaqueous electrolyte secondary batteries used for an electric vehicle is obtained.
[0043]
(Method for producing positive electrode active material for non-aqueous electrolyte secondary battery)
The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to the present invention includes a first particle comprising a lithium transition metal composite oxide having a first particle size distribution and a primary particle diameter of 10 μm or less. A step of selecting a group, and a second composed of a lithium transition metal composite oxide having a second particle size distribution having a larger secondary particle size than the first particle size distribution and having a primary particle size in the range of 8 μm to 150 μm. And a step of mixing a lithium transition metal composite oxide that is the selected first particle group and a lithium transition metal composite oxide that is the selected second particle group. Have.
[0044]
Hereinafter, the positive electrode active material for a non-aqueous electrolyte secondary battery according to the present invention (Li1.072Mn1.914Mg0.01B0.0035O4The manufacturing method is not limited to the present manufacturing method except for the above steps.
[0045]
A sodium hydrogen carbonate aqueous solution is added to an aqueous solution containing manganese ions and magnesium ions having a predetermined composition ratio to coprecipitate manganese and magnesium to obtain a coprecipitate.
[0046]
The manganese source is not particularly limited. Basically, any salt that can form an aqueous solution can be used. For example, manganese chloride, manganese iodide, manganese sulfate, manganese nitrate or the like is used. Preferably, MnSO4, MnCl2Etc. are used.
[0047]
The magnesium source is not particularly limited. Basically, any salt that can form an aqueous solution can be used. For example, magnesium chloride, magnesium iodide, magnesium perchlorate, magnesium sulfate, magnesium nitrate and the like are used. Preferably, MgSO4, Mg (NO3)2Etc. are used.
[0048]
Moreover, although the sodium hydrogencarbonate aqueous solution is added, it is not necessarily restricted to this, What is necessary is just alkaline solutions, such as sodium hydroxide aqueous solution, potassium hydroxide aqueous solution, lithium hydroxide aqueous solution.
[0049]
Next, the obtained coprecipitate is filtered, washed with water, and dried. The first coprecipitate is left as it is, and a predetermined amount of orthoboric acid is mixed with the second coprecipitate. The first coprecipitate is mixed with lithium carbonate so as to have a predetermined composition ratio, and is fired at a temperature of 800 ° C. to 1000 ° C. for 5 hours to 15 hours in air or in a weakly oxidizing atmosphere. The second coprecipitate is mixed with lithium carbonate so as to have a predetermined composition ratio, and fired in air or in a weakly oxidizing atmosphere at a temperature of 800 ° C. to 1000 ° C. for 5 hours to 15 hours. Thus, the lithium transition metal composite oxide having the first particle size distribution and the primary particle diameter in the range of 10 μm or less, and the lithium transition metal composite oxide having the second particle size distribution and the primary particle diameter in the range of 8 μm to 150 μm. Obtain an oxide. 3 to 6 show a first particle size distribution 21 and a second particle size distribution 22 in the present invention.
[0050]
If the primary particle size exceeds 10 μm with the first particle size distribution, the difference between small particles and large particles becomes small, which is not preferable. Preferably, it has the first particle size distribution and the primary particle size is 2 μm to 8 μm. If the second particle size distribution and the primary particle size is smaller than 8 μm or larger than 150 μm, it becomes difficult to maintain the balance between the small particles and the large particles. Since sedimentation occurs, it is not preferable. Preferably, the lithium transition metal composite oxide has a second particle size distribution and a primary particle size in the range of 10 μm to 80 μm.
[0051]
What is mixed with the coprecipitate is not limited to lithium carbonate. Basically, any lithium compound can be used. For example, lithium fluoride, lithium chloride, lithium bromide, lithium iodide, lithium oxide, lithium peroxide, lithium hydroxide, or the like is used. Preferably Li2CO3, LiOH, LiOH · H2O, Li2O, LiCl, LiNO3, Li2SO4, LiHCO3, Li (CH3COO) or the like is used.
[0052]
You may mix a sulfur containing compound, the compound containing a halogen element, etc. with a coprecipitate and a lithium compound.
[0053]
The sulfur-containing compound is not particularly limited. For example, sulfide, sulfur iodide, hydrogen sulfide, sulfuric acid and its salt, nitrogen sulfide and the like are used. Preferably Li2SO4, MnSO4, (NH4)2SO4, Al2(SO4)3, MgSO4Etc. are used.
[0054]
The compound containing a halogen element is not particularly limited. For example, hydrogen fluoride, oxygen fluoride, hydrofluoric acid, hydrogen chloride, hydrochloric acid, chlorine oxide, fluorinated chlorine oxide, bromine oxide, bromine fluorosulfate, hydrogen iodide, iodine oxide, periodic acid and the like are used. Preferably, NH4F, NH4Cl, NH4Br, NH4I, LiF, LiCl, LiBr, LiI, MnF2, MnCl2, MnBr2, MnI2Etc. are used.
[0055]
The firing temperature is preferably 850 ° C. to 950 ° C., and the firing time is preferably 8 to 14 hours. When the firing temperature is lower than 800 ° C., unreacted raw materials may remain in the positive electrode active material for a non-aqueous electrolyte secondary battery, and sufficient characteristics that can achieve the object of the present invention may not be obtained. Further, when baked at a temperature higher than 1000 ° C., a by-product is likely to be generated, resulting in a decrease in discharge capacity per unit weight, a decrease in cycle charge / discharge characteristics, and a decrease in operating voltage. When the firing time is less than 5 hours, the diffusion reaction between the particles of the raw material mixture does not proceed, and the target positive electrode active material for a non-aqueous electrolyte secondary battery cannot be obtained. In addition, firing for longer than 15 hours is not preferable because coarse particles are formed by sintering.
[0056]
A first particle group made of a lithium transition metal composite oxide having a first particle size distribution and a primary particle size in the range of 10 μm or less is selected, and a second particle size larger than the first particle size distribution is obtained. A second particle group consisting of a second particle group consisting of a lithium transition metal complex oxide having a particle size distribution of 2 and a primary particle diameter in the range of 8 μm to 150 μm, and the selected first particle group And the second particle group are mixed.
[0057]
The lithium transition metal composite oxide which is the second particle group preferably contains boron. In the present invention, boron may be dissolved in the lithium transition metal composite oxide that is the second particle group, or boron may be present on the surface of the lithium transition metal composite oxide particles. If the surface of the particles of the lithium transition metal composite oxide that is the second particle group has boron, boron improves the ease of passing electrons in the lithium transition metal composite oxide, High load characteristics are improved. The particles of the lithium transition metal composite oxide may be primary particles or secondary particles.
[0058]
A boron compound may be used instead of boron. The boron compound is not particularly limited. For example, boric acid, lithium borate, boride, boron oxide, boron phosphate or the like is used. Preferred are boric acid and lithium borate.
[0059]
In the present invention, the boron compound may be dissolved in the lithium transition metal composite oxide as the second particle group, or may have a boron compound on the surface of the lithium transition metal composite oxide particles. It is preferable to have lithium borate on the surface of the particles of the lithium transition metal composite oxide that is the second particle group. At this time, since lithium borate improves the ease of passing electrons in the lithium transition metal composite oxide, cycle charge / discharge characteristics and high load characteristics are improved. The particles of the lithium transition metal composite oxide may be primary particles or secondary particles.
[0060]
Even if boron and / or lithium borate are present on the surface of the lithium transition metal composite oxide particles, the effects of the present invention are exhibited. For example, even when boron and / or lithium borate is coated on the entire surface of the lithium transition metal composite oxide particles, boron and / or lithium borate is used as the lithium transition metal composite oxide particles. Even when the surface is partially covered, the cycle charge / discharge characteristics and thermal stability are improved.
[0061]
More preferably, boron and / or lithium borate is coated over the entire surface of the lithium transition metal composite oxide particles. In this case, it is possible to obtain a positive electrode active material for a non-aqueous electrolyte secondary battery in which not only cycle charge / discharge characteristics and thermal stability but also storage characteristics are improved.
Further, boron and / or lithium borate may be present at least on the surface of the particles. Therefore, boron and / or lithium borate may be present inside the particles.
[0062]
Whether boric acid and / or lithium borate is present on the surface of the lithium transition metal composite oxide particles can be analyzed by various methods. For example, analysis can be performed by Auger electron spectroscopy (AES) or X-ray photoelectron spectroscopy (XPS).
[0063]
The amount of boron contained in the lithium transition metal composite oxide that is the second particle group is preferably 50 ppm to 500 ppm with respect to the lithium transition metal composite oxide that is the second particle group. At this time, the effect of the present invention is clearly shown. Preferably it is 100 ppm-400 ppm, More preferably, it is 150 ppm-350 ppm. At this time, the electrode plate density is improved and dry-out can be prevented without deteriorating the overcharge characteristics.
[0064]
The first particle size distribution is preferably prepared such that the secondary particle size is in the range of 1 μm to 50 μm. If the secondary particle diameter is smaller than 1 μm, the specific surface area of the lithium transition metal composite oxide increases, and manganese elution that causes deterioration of cycle charge / discharge characteristics and dryout occurs. If the secondary particle diameter is larger than 50 μm, it cannot contribute to mixing with large particles as small particles, and is not effective in achieving the object of the present invention. More preferably, the secondary particle size of the first particle size distribution is adjusted in the range of 1 μm to 30 μm.
[0065]
The second particle size distribution is preferably prepared such that the secondary particle size is in the range of 8 μm to 150 μm. If the secondary particle size is smaller than 8 μm, it is impossible to contribute to mixing with small particles as large particles, which is not effective for achieving the object of the present invention. If the secondary particle diameter is larger than 150 μm, precipitation of lithium transition metal composite oxide particles during production of the positive electrode mixture occurs, which is not preferable. More preferably, the secondary particle size of the second particle size distribution is adjusted in the range of 10 μm to 50 μm.
[0066]
The lithium transition metal composite oxide has a general formula of LiaMbMn3-a-bAgXcBdSeDhO4 + f(M represents aluminum and / or magnesium, A represents at least one selected from the group consisting of titanium, zirconium and hafnium, X represents at least one selected from the group consisting of fluorine, chlorine, bromine and iodine, B Represents boron, S represents sulfur, D represents sodium and / or calcium, a represents a number satisfying 0.8 ≦ a ≦ 1.2, and b represents a number satisfying 0 ≦ b ≦ 0.2. C represents a number satisfying 0 ≦ c ≦ 0.05, d represents a number satisfying 0 ≦ d ≦ 0.02, e represents a number satisfying 0 ≦ e ≦ 0.1, and f represents -0.5 ≦ f ≦ 0.5, g represents a number satisfying 0 ≦ g ≦ 0.1, and h represents a number satisfying 0 ≦ h ≦ 0.015. It is preferable.
[0067]
The mixing ratio of the lithium transition metal composite oxide which is the first particle group and the lithium transition metal composite oxide which is the second particle group of the lithium transition metal composite oxide which is the second particle group is 50 wt. % To 90% by weight of the lithium transition metal composite oxide that is the first particle group of the lithium transition metal composite oxide that is the first particle group and the lithium transition metal composite oxide that is the second particle group. The mixing ratio relative to the total is preferably 10% by weight to 50% by weight. If the mixing ratio is not within this range, the electrode plate density cannot be increased efficiently. When the mixing ratio of small particles is large, the surface of the electrode plate is crushed by the press at the time of electrode plate production, making it difficult for the electrolyte to enter and exit, resulting in dryout. More preferably, the mixing ratio of the lithium transition metal composite oxide that is the first particle group of the lithium transition metal composite oxide that is the second particle group and the total of the lithium transition metal composite oxide that is the second particle group Is 55% by weight to 75% by weight, and the lithium transition metal composite oxide that is the first particle group of the lithium transition metal composite oxide that is the first particle group and the lithium transition metal that is the second particle group The mixing ratio with respect to the total of the composite oxide is 25% by weight to 45% by weight.
[0068]
You may grind | pulverize the lithium transition metal complex oxide obtained by the said baking with a mortar, a ball mill, a vibration mill, a pin mill, etc. Specific surface area of 0.2 m by the above method2/G-1.2m2/ G of the positive electrode active material for a non-aqueous electrolyte secondary battery of the present invention can be obtained.
[0069]
By using the above manufacturing method, it is possible to obtain a target positive electrode active material for a non-aqueous electrolyte secondary battery.
[0070]
In addition, by coprecipitation of manganese and magnesium with carbonate, Li1.072Mn1.914Mg0.01B0.0035O4However, a manganese compound and a magnesium compound may be mixed so as to have a predetermined composition ratio and fired.
[0071]
(Non-aqueous electrolyte secondary battery)
The positive electrode active material for a non-aqueous electrolyte secondary battery according to the present invention is suitably used for non-aqueous electrolyte secondary batteries such as lithium ion secondary batteries and lithium ion polymer secondary batteries.
[0072]
The non-aqueous electrolyte secondary battery may be a conventionally known non-aqueous electrolyte secondary battery in which the positive electrode active material may be the positive electrode active material of the present invention, and other configurations are not particularly limited. Any non-aqueous electrolyte secondary battery including a positive electrode active material layer mainly composed of the lithium transition metal composite oxide according to the present invention may be used.
[0073]
By using lithium cobaltate and / or lithium nickelate together with the positive electrode active material of the present invention as a positive electrode active material, not only overcharge characteristics, thermal stability and safety, but also excellent discharge capacity, load characteristics, and output characteristics A nonaqueous electrolyte secondary battery can be obtained.
[0074]
The general formula is Li1 + xCoO2Lithium cobaltate represented by (x represents a number satisfying −0.5 ≦ x ≦ 0.5) is preferable. The lithium cobaltate is at least a part selected from the group consisting of magnesium, aluminum, calcium, vanadium, titanium, chromium, manganese, iron, cobalt, nickel, copper, zinc, strontium, zirconium, niobium, molybdenum and tin. It may be substituted with one kind.
[0075]
The general formula is Li1 + xNiO2Lithium nickelate represented by (x represents a number satisfying −0.5 ≦ x ≦ 0.5) is preferable. The lithium nickelate is at least a part selected from the group consisting of magnesium, aluminum, calcium, vanadium, titanium, chromium, manganese, iron, cobalt, nickel, copper, zinc, strontium, zirconium, niobium, molybdenum and tin. It may be substituted with one kind.
[0076]
The positive electrode using the positive electrode active material mainly composed of the lithium transition metal composite oxide according to the present invention is preferably produced as follows. A positive electrode mixture is formed by mixing the lithium transition metal composite oxide powder according to the present invention with a carbon-based conductive agent such as acetylene black or graphite, a binder, and a solvent or dispersion medium of the binder. . The positive electrode mixture is made into a slurry or a kneaded material, applied or supported on a current collector 12 such as an aluminum foil, and press-rolled to form a positive electrode active material layer on the current collector 12.
[0077]
As the binder, polyvinylidene fluoride, polytetrafluoroethylene, polyamide acrylic resin, or the like can be used.
[0078]
It is considered that the lithium transition metal composite oxide according to the present invention has good mixing properties with the conductive agent powder, and the internal resistance of the battery is reduced. For this reason, the charge / discharge characteristics, particularly the discharge capacity, are improved. Further, when kneaded with the binder, the lithium transition metal composite oxide of the present invention is excellent in fluidity, easily entangled with the polymer of the binder, and has excellent binding properties. Furthermore, since it is spherical without containing coarse particles, the surface of the coating film surface of the produced positive electrode 13 is excellent in smoothness. For this reason, the coating surface of the positive electrode plate has excellent binding properties and is not easily peeled off, and the surface is smooth and the lithium ion on and off of the coating surface due to charging / discharging is uniformly performed, so the cycle charge / discharge characteristics are remarkably improved. Is obtained.
[0079]
For example, as the negative electrode active material, metallic lithium, a lithium alloy, or a compound capable of occluding and releasing lithium ions can be used. As the lithium alloy, for example, a LiAl alloy, a LiSn alloy, a LiPb alloy, or the like can be used. As a compound capable of occluding and releasing lithium ions, carbon materials such as graphite and graphite can be used. Further, an oxide capable of inserting / extracting lithium ions such as tin oxide and titanium oxide may be used.
[0080]
The electrolyte solution is not particularly limited as long as it is a compound that does not change or decompose at the operating voltage. Examples of solvents that can be used include organic solvents such as dimethoxyethane, diethoxyethane, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl formate, γ-butyrolactone, 2-methyltetrahydrofuran, dimethyl sulfoxide, and sulfolane. In addition, two or more kinds selected from the above-mentioned organic solvent group may be mixed and used.
[0081]
Examples of the electrolyte that can be used include lithium salts such as lithium perchlorate, lithium tetrafluoroborate, lithium tetrafluorophosphate, and lithium trifluoromethanoate. The above solvent and electrolyte are mixed and used as an electrolytic solution. Here, a gelling agent or the like may be added and used as a gel, or may be used after being absorbed in a hygroscopic polymer. Further, a solid electrolyte having conductivity of inorganic or organic lithium ions may be used.
[0082]
Furthermore, as the separator 14, a porous film made of polyethylene, polypropylene, or the like can be used. Using the positive electrode active material for a non-aqueous electrolyte secondary battery according to the present invention, the negative electrode active material, the electrolytic solution, and the separator, a non-aqueous electrolyte secondary battery is obtained in accordance with a conventional method. Thereby, the outstanding battery characteristic which was not able to be achieved conventionally is realizable.
[0083]
Further, a strip-shaped positive electrode configured by forming a positive electrode active material layer using the positive electrode active material for a non-aqueous electrolyte secondary battery according to the present invention as a positive electrode active material on both surfaces of the strip-shaped positive electrode current collector, Each of the negative electrode active material layers includes a negative electrode active material layer formed on each side of the negative electrode current collector, and each of the negative electrode active material layers is laminated in a state where the positive electrode and the negative electrode are stacked with a band separator. By winding, a spiral wound body in which a strip separator is interposed between the strip-shaped positive electrode and the strip-shaped negative electrode can be formed into a non-aqueous electrolyte secondary battery. With this configuration, the manufacturing process is simple, the positive electrode active material layer and the negative electrode active material layer are not easily cracked or peeled off from the strip separator, the battery capacity can be increased, and the energy density can be increased. . In particular, the positive electrode active material for a non-aqueous electrolyte secondary battery according to the present invention has a high electrode plate density and excellent filling properties, and is easily compatible with a binder. Therefore, the positive electrode has a high charge / discharge capacity and excellent binding properties and surface smoothness, so that the positive electrode active material layer can be prevented from being cracked or peeled off.
[0084]
The shape of the nonaqueous electrolyte secondary battery may be a cylindrical shape, a coin shape, a square shape, or the like.
[0085]
(Applications for non-aqueous electrolyte secondary batteries)
The application of the non-aqueous electrolyte secondary battery using the positive electrode active material for a non-aqueous electrolyte secondary battery according to the present invention is not particularly limited. For example, notebook computers, pen input computers, pocket computers, notebook word processors, pocket word processors, electronic book players, mobile phones, cordless phones, electronic notebooks, calculators, LCD TVs, electric shavers, electric tools, electronic translators, car phones , Portable printer, transceiver, pager, handy terminal, portable copy, voice input device, memory card, backup power supply, tape recorder, radio, headphone stereo, handy cleaner, portable CD, video movie, navigation system, etc. Can be used. Also lighting equipment, air conditioner, TV, stereo, water heater, refrigerator, oven microwave, dishwasher, washing machine, dryer, game machine, toy, road conditioner, medical equipment, automobile, electric car, golf cart, electric cart It can be used as a power source for power storage systems. It can also be used for civilian use, military use, and space use.
[0086]
Hereinafter, although the Example is given and demonstrated about the positive electrode active material for nonaqueous electrolyte secondary batteries which concerns on this invention, it is not limited to this Example.
[0087]
【Example】
[Example 1]
A sodium hydrogen carbonate aqueous solution was added to an aqueous solution containing manganese ions and magnesium ions having a predetermined composition ratio to coprecipitate manganese and magnesium to obtain a coprecipitate.
The obtained coprecipitate was filtered, washed with water and dried, and then the first coprecipitate was left as it was, and the second coprecipitate was mixed with 300 ppm of orthoboric acid. The first coprecipitate was mixed with lithium carbonate so as to have a predetermined composition ratio, and baked in an air atmosphere at a temperature of 930 ° C. for 12 hours. The second coprecipitate was mixed with lithium carbonate so as to have a predetermined composition ratio, and baked in an air atmosphere at a temperature of 930 ° C. for 12 hours. Thus, a lithium transition metal composite oxide having a first particle size distribution and a primary particle diameter of 4 μm and a lithium transition metal composite oxide having a second particle size distribution and a primary particle diameter of 20 μm were obtained.
Lithium transition having a first particle size distribution and a first particle group made of a lithium transition metal composite oxide having a primary particle size of 4 μm and a second particle size distribution having a primary particle size of 20 μm A second particle group composed of a second particle group composed of a metal composite oxide was selected, and the selected first particle group and second particle group were mixed. The mixing ratio of the lithium transition metal composite oxide that is the first particle group of the lithium transition metal composite oxide that is the second particle group and the lithium transition metal composite oxide that is the second particle group is 70 wt%. %, And the mixing ratio with respect to the total of the lithium transition metal composite oxide that is the first particle group and the lithium transition metal composite oxide that is the second particle group of the lithium transition metal composite oxide that is the first particle group is 30% by weight. Thus Li1.072Mn1.914Mg0.01B0.0035O4was gotten.
[0088]
(Evaluation of positive electrode active material for non-aqueous electrolyte secondary battery)
The positive electrode active material for a non-aqueous electrolyte secondary battery according to the present invention performs composition analysis, specific surface area, and particle size distribution measurement by the following methods. In addition, a test battery is prepared and evaluated.
[0089]
(Composition analysis)
A predetermined amount of a positive electrode active material for a non-aqueous electrolyte secondary battery is dissolved in nitric acid, and the content of each constituent element other than halogen elements and oxygen is quantified by plasma emission spectroscopy (ICP) analysis. A predetermined amount of the positive electrode active material for a non-aqueous electrolyte secondary battery is added to pure water and stirred to obtain a supernatant aqueous solution. The halogen element in the supernatant aqueous solution is quantified by an ion meter using an anion selective electrode as an indicator electrode.
[0090]
(Powder evaluation)
The specific surface area of the positive electrode active material for a non-aqueous electrolyte secondary battery is measured by a constant pressure BET adsorption method using nitrogen gas. The median diameter is obtained by measuring the particle size distribution by the laser diffraction scattering method, obtaining an integrated distribution using the logarithm of the volume-based particle diameter, and the particle diameter when occupying 50% of the entire lithium transition metal composite oxide powder, Measure as particle size with 50% oversize. The primary particle size is measured using an image analysis method (microscope method).
[0091]
(Measurement of crystallite diameter)
Measurement is performed using RINT2500V manufactured by Rigaku Denki Co., Ltd. CuKα1 is used as the X-ray source, and the X-ray diffraction pattern is measured at a tube current of 100 mA and a tube voltage of 40 kV. It is calculated by the Scherrer formula expressed by the following formula from the diffraction peak due to the (400) plane.
[0092]
[Expression 1]
Figure 0004940530
[0093]
In the equation, D is the crystallite size (Å), K is the Scherrer constant (K = 1.05 when β is calculated from the integral width), and λ is the wavelength of the X-ray source (CuKα1 = 1.540562Å). , Β is the width (radian) of the diffraction line spread depending on the crystallite size, and θ is the diffraction angle 2θ / 2 (degree).
[0094]
(Production of lithium ion secondary battery)
To a normal methylpyrrolidone solution containing 5 parts by weight of polyvinylidene fluoride, 90 parts by weight of lithium transition metal composite oxide powder as a positive electrode active material and 5 parts by weight of carbon powder as a conductive agent were added and kneaded to prepare a paste. This is applied to an aluminum electrode plate by a doctor blade method and dried to obtain a positive electrode plate. Similarly, a carbon material is used as the negative electrode active material and applied to the copper electrode plate to produce a negative electrode plate. A porous propylene film is used as a separator, and LiPF is used as a mixed solvent of ethylene carbonate: diethyl carbonate = 1: 1 (volume ratio) as an electrolytic solution.6A lithium ion secondary battery is manufactured using a solution in which is dissolved at a concentration of 1 mol / l. In this embodiment, a positive electrode plate, a negative electrode plate, and a separator are formed into a thin sheet, wound, and stored in a battery case of a metal laminate resin film to obtain a laminate type battery.
[0096]
(Measurement of electrode plate density)
A paste was prepared by kneading 95 parts by weight of a lithium transition metal composite oxide powder, which is a positive electrode active material, and a normal methylpyrrolidone solution containing 5 parts by weight of polyvinylidene fluoride, and this was applied to an aluminum electrode plate by a doctor blade method. It is applied and dried to form a positive electrode plate. After the positive electrode plate is cut into a predetermined size (2 × 2.5 cm), the electrode plate is pressed with a uniaxial press, and the electrode plate density is obtained from the thickness and weight of the electrode plate after pressurization.
[0097]
  (Dry out evaluation)
  A paste was prepared by kneading 95 parts by weight of a lithium transition metal composite oxide powder, which is a positive electrode active material, and a normal methylpyrrolidone solution containing 5 parts by weight of polyvinylidene fluoride, and this was applied to an aluminum electrode plate by a doctor blade method. It is applied and dried to form a positive electrode plate.After cutting the positive electrode to a predetermined size, press the electrode plate with a uniaxial press,The positive electrode plate is placed in a glass container and immersed in a propylene carbonate solution in an argon box. After making a vacuum for 3 minutes to allow the propylene carbonate solution to penetrate into the positive electrode plate, the positive electrode plate is taken out from the argon box and the positive electrode plate is weighed every hour. The amount of decrease in the propylene carbonate solution is calculated by subtracting the weight of the first positive electrode plate from the weight of the positive electrode plate per hour. If the amount of decrease in propylene carbonate is large, it is easy to move the electrolyte, and it can be determined that dryout can be prevented. If the amount of decrease in propylene carbonate is small, it can be determined that the electrolyte solution is difficult to move and that dryout is likely to occur.
[0098]
The results are shown in Table 1 and FIG. The particle size distribution is shown in FIG.
[0099]
[Example 2]
A sodium hydrogen carbonate aqueous solution was added to an aqueous solution containing manganese ions and magnesium ions having a predetermined composition ratio to coprecipitate manganese and magnesium to obtain a coprecipitate.
The obtained coprecipitate was filtered, washed with water, and dried. Then, the first coprecipitate was left as it was, and 200 ppm of orthoboric acid was mixed with the second coprecipitate. The first coprecipitate was mixed with lithium carbonate so as to have a predetermined composition ratio, and baked in an air atmosphere at a temperature of 930 ° C. for 12 hours. The second coprecipitate was mixed with lithium carbonate so as to have a predetermined composition ratio, and baked in an air atmosphere at a temperature of 930 ° C. for 12 hours. Thus, a lithium transition metal composite oxide having a first particle size distribution and a primary particle size of 4 μm and a lithium transition metal composite oxide having a second particle size distribution and a primary particle size of 15 μm were obtained.
Lithium transition having a first particle size distribution and a first particle group made of a lithium transition metal composite oxide having a primary particle size of 4 μm and a second particle size distribution having a primary particle size of 15 μm A second particle group composed of a second particle group composed of a metal composite oxide was selected, and the selected first particle group and second particle group were mixed. The mixing ratio of the lithium transition metal composite oxide that is the first particle group of the lithium transition metal composite oxide that is the second particle group and the lithium transition metal composite oxide that is the second particle group is 70 wt%. %, And the mixing ratio with respect to the total of the lithium transition metal composite oxide that is the first particle group and the lithium transition metal composite oxide that is the second particle group of the lithium transition metal composite oxide that is the first particle group is 30% by weight. Thus Li1.073Mn1.915Mg0.01B0.0023O4was gotten.
[0100]
The particle size distribution is shown in FIG.
[0101]
Example 3
A sodium hydrogen carbonate aqueous solution was added to an aqueous solution containing manganese ions and magnesium ions having a predetermined composition ratio to coprecipitate manganese and magnesium to obtain a coprecipitate.
The obtained coprecipitate was filtered, washed with water, and dried. Then, the first coprecipitate was left as it was, and the second coprecipitate was mixed with 100 ppm of orthoboric acid. The first coprecipitate was mixed with lithium carbonate so as to have a predetermined composition ratio, and baked in an air atmosphere at a temperature of 930 ° C. for 12 hours. The second coprecipitate was mixed with lithium carbonate so as to have a predetermined composition ratio, and baked in an air atmosphere at a temperature of 930 ° C. for 12 hours. Thus, a lithium transition metal composite oxide having a first particle size distribution and a primary particle size of 4 μm and a lithium transition metal composite oxide having a second particle size distribution and a primary particle size of 8 μm were obtained.
Lithium transition having a first particle size distribution and a first particle group made of a lithium transition metal composite oxide having a primary particle size of 4 μm and a second particle size distribution having a primary particle size of 8 μm A second particle group composed of a second particle group composed of a metal composite oxide was selected, and the selected first particle group and second particle group were mixed. The mixing ratio of the lithium transition metal composite oxide that is the first particle group of the lithium transition metal composite oxide that is the second particle group and the lithium transition metal composite oxide that is the second particle group is 70 wt%. %, And the mixing ratio with respect to the total of the lithium transition metal composite oxide that is the first particle group and the lithium transition metal composite oxide that is the second particle group of the lithium transition metal composite oxide that is the first particle group is 30% by weight. Thus Li1.073Mn1.916Mg0.01B0.0012O4was gotten.
[0102]
Hereinafter, the positive electrode active material for the nonaqueous electrolyte secondary battery was evaluated in the same manner as in Example 1. The results are shown in Table 1 and FIG. The particle size distribution is shown in FIG.
[0103]
Example 4
A sodium hydrogen carbonate aqueous solution was added to an aqueous solution containing manganese ions and magnesium ions having a predetermined composition ratio to coprecipitate manganese and magnesium to obtain a coprecipitate.
The obtained coprecipitate was filtered, washed with water and dried, and then the first coprecipitate was left as it was, and the second coprecipitate was mixed with 300 ppm of orthoboric acid. The first coprecipitate was mixed with lithium carbonate so as to have a predetermined composition ratio, and baked in an air atmosphere at a temperature of 930 ° C. for 12 hours. The second coprecipitate was mixed with lithium carbonate so as to have a predetermined composition ratio, and baked in an air atmosphere at a temperature of 930 ° C. for 12 hours. Thus, a lithium transition metal composite oxide having a first particle size distribution and a primary particle diameter of 4 μm and a lithium transition metal composite oxide having a second particle size distribution and a primary particle diameter of 20 μm were obtained.
Lithium transition having a first particle size distribution and a first particle group made of a lithium transition metal composite oxide having a primary particle size of 4 μm and a second particle size distribution having a primary particle size of 20 μm A second particle group composed of a second particle group composed of a metal composite oxide was selected, and the selected first particle group and second particle group were mixed. The mixing ratio of the lithium transition metal composite oxide that is the first particle group of the lithium transition metal composite oxide that is the second particle group and the lithium transition metal composite oxide that is the second particle group is 60% by weight. %, And the mixing ratio with respect to the total of the lithium transition metal composite oxide that is the first particle group and the lithium transition metal composite oxide that is the second particle group of the lithium transition metal composite oxide that is the first particle group is 40% by weight. Thus Li1.072Mn1.915Mg0.01B0.003O4was gotten.
[0104]
The particle size distribution is shown in FIG.
[0105]
[Comparative Example 1]
A sodium hydrogen carbonate aqueous solution was added to an aqueous solution containing manganese ions and magnesium ions having a predetermined composition ratio to coprecipitate manganese and magnesium to obtain a coprecipitate.
The obtained coprecipitate was filtered, washed with water, dried, mixed with lithium carbonate so as to have a predetermined composition ratio, and calcined at 930 ° C. for 12 hours in an air atmosphere. And pulverize in a mortar1.073Mn1.917Mg0.01O4was gotten.
[0106]
Hereinafter, the positive electrode active material for the nonaqueous electrolyte secondary battery was evaluated in the same manner as in Example 1. The results are shown in Table 1 and FIG. The particle size distribution is shown in FIG.
[0111]
  As is apparent from Table 1 and FIG. 1, it can be seen that the positive electrode active material for a non-aqueous electrolyte secondary battery of the present invention has an improved electrode plate density as compared with Comparative Example 1. I also know that it can prevent dryoutThe
[0112]
  On the other hand, Comparative Example 1 is an electrode plate denseDegreeIt is inferior to the positive electrode active material for a non-aqueous electrolyte secondary battery of the present invention. In addition, dryout cannot be prevented.
[0113]
[Table 1]
Figure 0004940530
[0114]
In Example 1, Example 2 and Example 3, the mixing ratio of the lithium transition metal composite oxide which is the first particle group and the lithium transition metal composite oxide which is the second particle group is changed, The electrode plate density was measured when it was changed. The results are shown in Tables 2 to 4 and FIG.
[0115]
[Table 2]
Figure 0004940530
[0116]
[Table 3]
Figure 0004940530
[0117]
[Table 4]
Figure 0004940530
[0118]
From this result, the mixing ratio with respect to the sum total of the lithium transition metal composite oxide which is the first particle group and the lithium transition metal composite oxide which is the second particle group of the lithium transition metal composite oxide which is the second particle group Is 60 wt% to 70 wt%, and the lithium transition metal composite oxide that is the first particle group of the lithium transition metal composite oxide that is the first particle group and the lithium transition metal that is the second particle group It can be seen that the mixing ratio relative to the total of the composite oxides is more preferably 30% by weight to 40% by weight.
[0129]
  As described above, the positive electrode active material for a non-aqueous electrolyte secondary battery according to the present invention has excellent battery characteristics that can improve the electrode plate density and prevent dryout.. ShiTherefore, the positive electrode active material for a non-aqueous electrolyte secondary battery of the present invention is suitably used for a non-aqueous electrolyte secondary battery such as a lithium ion secondary battery.
[Brief description of the drawings]
FIG. 1 is a graph showing changes in electrode plate density accompanying changes in press pressure.
FIG. 2 is a graph showing changes in electrode plate density accompanying changes in the mixing ratio of a lithium transition metal composite oxide that is a first particle group and a lithium transition metal composite oxide that is a second particle group.
3 is a graph showing the particle size distribution of Example 1. FIG.
4 is a graph showing the particle size distribution of Example 2. FIG.
5 is a graph showing the particle size distribution of Example 3. FIG.
6 is a graph showing the particle size distribution of Example 4. FIG.
7 is a graph showing the particle size distribution of Comparative Example 1. FIG.
8 is a graph showing the particle size distribution of Comparative Example 2. FIG.
9 is a graph showing the particle size distribution of Comparative Example 3. FIG.
FIG. 10 is a diagram showing a lithium transition metal composite oxide having a spinel structure.
FIG. 11 is a schematic view of binding of active materials.
FIG. 12 is a cross-sectional view of a cylindrical battery.
FIG. 13 is a diagram showing a structure of a coin-type battery.
FIG. 14 is a diagram showing a structure of a prismatic battery.
[Explanation of symbols]
1 ... 8a site
2 ... 32e site
3 ... 16d site
4 ... Binder
5 ... Active material
11 ... Negative electrode
12 ... current collector
13 ... Positive electrode
14 ... Separator
21 ... 1st particle size distribution
22 ... second particle size distribution

Claims (2)

少なくともスピネル構造のリチウム遷移金属複合酸化物を有する非水電解液二次電池用正極活物質であって、
前記リチウム遷移金属複合酸化物は、一次粒子径が2μm〜8μmである第1のマンガン酸リチウム及び一次粒子径が8μm〜150μmである第2のマンガン酸リチウムを有すると共に、
該第1のマンガン酸リチウムの一次粒子径は、ホウ素を50ppm〜500ppm含有する第2のマンガン酸リチウムの一次粒子径よりも小さい
ことを特徴とする非水電解液二次電池用正極活物質。
A positive electrode active material for a non-aqueous electrolyte secondary battery having at least a lithium transition metal composite oxide having a spinel structure,
The lithium transition metal composite oxide has a first lithium manganate having a primary particle diameter of 2 μm to 8 μm and a second lithium manganate having a primary particle diameter of 8 μm to 150 μm ,
The primary particle diameter of said 1st lithium manganate is smaller than the primary particle diameter of the 2nd lithium manganate containing 50 ppm-500 ppm of boron, The positive electrode active material for nonaqueous electrolyte secondary batteries characterized by the above-mentioned.
前記第1のマンガン酸リチウムの前記第1のマンガン酸リチウムと前記第2のマンガン酸リチウムの合計に対する混合割合(重量%)が、前記第2のマンガン酸リチウムの前記第1のマンガン酸リチウムと前記第2のマンガン酸リチウムの合計に対する混合割合(重量%)よりも少ないことを特徴とする請求項1に記載の非水電解液二次電池用正極活物質。The mixing ratio (% by weight) of the first lithium manganate to the total of the first lithium manganate and the second lithium manganate is such that the second lithium manganate and the first lithium manganate 2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the amount is less than a mixing ratio (% by weight) with respect to a total amount of the second lithium manganate.
JP2003028609A 2003-02-05 2003-02-05 Cathode active material for non-aqueous electrolyte secondary battery Expired - Lifetime JP4940530B2 (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2003028609A JP4940530B2 (en) 2003-02-05 2003-02-05 Cathode active material for non-aqueous electrolyte secondary battery

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
JP2003028609A JP4940530B2 (en) 2003-02-05 2003-02-05 Cathode active material for non-aqueous electrolyte secondary battery

Publications (2)

Publication Number Publication Date
JP2004241242A JP2004241242A (en) 2004-08-26
JP4940530B2 true JP4940530B2 (en) 2012-05-30

Family

ID=32956030

Family Applications (1)

Application Number Title Priority Date Filing Date
JP2003028609A Expired - Lifetime JP4940530B2 (en) 2003-02-05 2003-02-05 Cathode active material for non-aqueous electrolyte secondary battery

Country Status (1)

Country Link
JP (1) JP4940530B2 (en)

Families Citing this family (10)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP4766840B2 (en) * 2004-04-12 2011-09-07 住友金属鉱山株式会社 Positive electrode active material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
JP2006164689A (en) * 2004-12-06 2006-06-22 Enerstruct Kk Electrode structure, secondary battery, and capacitor
KR100670507B1 (en) * 2005-04-28 2007-01-16 삼성에스디아이 주식회사 Lithium secondary battery
JP5545790B2 (en) * 2007-07-23 2014-07-09 日立マクセル株式会社 Non-aqueous secondary battery and electronic device using the same
US8148015B2 (en) * 2008-03-21 2012-04-03 Byd Company Limited Cathode materials for lithium batteries
KR101264333B1 (en) * 2011-01-12 2013-05-14 삼성에스디아이 주식회사 Cathode active material, cathode and lithium battery containing the same, and preparation method thereof
JP5855988B2 (en) * 2011-03-30 2016-02-09 日本碍子株式会社 Positive electrode active material powder for lithium secondary battery, and lithium secondary battery
WO2017175697A1 (en) 2016-04-04 2017-10-12 株式会社Gsユアサ Power storage element
EP3509137B1 (en) 2016-09-07 2022-03-30 GS Yuasa International Ltd. Electricity storage element and method for producing electricity storage element
JP7324119B2 (en) * 2019-10-30 2023-08-09 パナソニックホールディングス株式会社 Positive electrode active material for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery

Family Cites Families (10)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP3512534B2 (en) * 1994-12-21 2004-03-29 株式会社リコー Rechargeable battery
JP3036674B2 (en) * 1995-01-17 2000-04-24 日本電池株式会社 Positive active material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery provided therewith
JP4124522B2 (en) * 1997-10-08 2008-07-23 日揮化学株式会社 Lithium / manganese composite oxide, production method and use thereof
JP3468098B2 (en) * 1998-05-29 2003-11-17 松下電器産業株式会社 Method for producing positive electrode active material for lithium secondary battery
JP2000082466A (en) * 1998-07-02 2000-03-21 Nippon Chem Ind Co Ltd Positive electrode active material and nonaqueous electrolyte secondary battery
JP2001048545A (en) * 1999-08-09 2001-02-20 Mitsubishi Chemicals Corp Production of lithium-manganese multiple oxide and secondary battery using the same
JP5199522B2 (en) * 1999-08-17 2013-05-15 日揮触媒化成株式会社 Spinel-type lithium / manganese composite oxide, its production method and use
JP4543474B2 (en) * 2000-02-03 2010-09-15 昭和電工株式会社 Positive electrode active material, method for producing the same, and non-aqueous secondary battery using the same
JP2001297767A (en) * 2000-04-11 2001-10-26 Japan Energy Corp Lithium secondary cell and positive electrode material for the same
JP4175026B2 (en) * 2001-05-31 2008-11-05 三菱化学株式会社 Method for producing lithium transition metal composite oxide and positive electrode material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery

Also Published As

Publication number Publication date
JP2004241242A (en) 2004-08-26

Similar Documents

Publication Publication Date Title
JP4096754B2 (en) Cathode active material for non-aqueous electrolyte secondary battery
JP5382025B2 (en) Nonaqueous electrolyte secondary battery, positive electrode active material for nonaqueous electrolyte secondary battery, and positive electrode mixture for nonaqueous electrolyte secondary battery
US7294435B2 (en) Positive electrode active material for nonaqueous electrolyte secondary battery, positive electrode mixture for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
JP2005251716A (en) Cathode active substance for nonaqueous electrolyte secondary battery, cathode mixture for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
JP2004227790A (en) Positive electrode active material for nonaqueous electrolyte solution secondary battery
JP2006012433A (en) Positive electrode active material for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery
JP2004193115A (en) Positive electrode active material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
JP2004235144A (en) Nonaqueous electrolyte secondary battery and negative electrode active substance therefor
JP2004311408A (en) Positive electrode active material for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery
JP2004103566A (en) Positive active substance for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery
JP2006012426A (en) Positive electrode active material for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery
JP2005044743A (en) Positive electrode activator of nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
JP2005222956A (en) Nonaqueous electrolytic solution secondary battery
JP4259393B2 (en) Positive electrode active material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
JP4876371B2 (en) Positive electrode active material for non-aqueous electrolyte secondary battery, positive electrode mixture for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
JP2005044722A (en) Cathode active substance for nonaqueous electrolyte solution secondary battery and nonaqueous electrolyte solution secondary battery
JP3856015B2 (en) Positive electrode secondary active material for nonaqueous electrolyte secondary battery, positive electrode active material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
JP4626141B2 (en) Positive electrode active material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
JP4940530B2 (en) Cathode active material for non-aqueous electrolyte secondary battery
JP2004327309A (en) Anode active material for nonaqueous electrolyte secondary battery
JP5044882B2 (en) Cathode active material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
JP5017010B2 (en) Lithium secondary battery
JP2004047448A (en) Positive electrode activator for nonaqueous electrolyte secondary battery
JP4492058B2 (en) Cathode active material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
JP2005158612A (en) Positive-electrode subsidiary active material for nonaqueous electrolytic secondary battery, positive-electrode active material for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and manufacturing method for nonaqueous electrolyte secondary battery

Legal Events

Date Code Title Description
A621 Written request for application examination

Free format text: JAPANESE INTERMEDIATE CODE: A621

Effective date: 20060127

A977 Report on retrieval

Free format text: JAPANESE INTERMEDIATE CODE: A971007

Effective date: 20081114

A131 Notification of reasons for refusal

Free format text: JAPANESE INTERMEDIATE CODE: A131

Effective date: 20091215

A521 Request for written amendment filed

Free format text: JAPANESE INTERMEDIATE CODE: A523

Effective date: 20100215

A131 Notification of reasons for refusal

Free format text: JAPANESE INTERMEDIATE CODE: A131

Effective date: 20110215

A521 Request for written amendment filed

Free format text: JAPANESE INTERMEDIATE CODE: A523

Effective date: 20110413

TRDD Decision of grant or rejection written
A01 Written decision to grant a patent or to grant a registration (utility model)

Free format text: JAPANESE INTERMEDIATE CODE: A01

Effective date: 20120131

A01 Written decision to grant a patent or to grant a registration (utility model)

Free format text: JAPANESE INTERMEDIATE CODE: A01

A61 First payment of annual fees (during grant procedure)

Free format text: JAPANESE INTERMEDIATE CODE: A61

Effective date: 20120213

R150 Certificate of patent or registration of utility model

Ref document number: 4940530

Country of ref document: JP

Free format text: JAPANESE INTERMEDIATE CODE: R150

Free format text: JAPANESE INTERMEDIATE CODE: R150

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20150309

Year of fee payment: 3

A521 Request for written amendment filed

Free format text: JAPANESE INTERMEDIATE CODE: A523

Effective date: 20100215

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20150309

Year of fee payment: 3

R250 Receipt of annual fees

Free format text: JAPANESE INTERMEDIATE CODE: R250

R250 Receipt of annual fees

Free format text: JAPANESE INTERMEDIATE CODE: R250

R250 Receipt of annual fees

Free format text: JAPANESE INTERMEDIATE CODE: R250

R250 Receipt of annual fees

Free format text: JAPANESE INTERMEDIATE CODE: R250

R250 Receipt of annual fees

Free format text: JAPANESE INTERMEDIATE CODE: R250

R250 Receipt of annual fees

Free format text: JAPANESE INTERMEDIATE CODE: R250

R250 Receipt of annual fees

Free format text: JAPANESE INTERMEDIATE CODE: R250

R255 Notification that request for automated payment was rejected

Free format text: JAPANESE INTERMEDIATE CODE: R2525

R250 Receipt of annual fees

Free format text: JAPANESE INTERMEDIATE CODE: R250

EXPY Cancellation because of completion of term