Nothing Special   »   [go: up one dir, main page]

JP2004203009A - Optical film, manufacturing method thereof and polarizer and display device using the same - Google Patents

Optical film, manufacturing method thereof and polarizer and display device using the same Download PDF

Info

Publication number
JP2004203009A
JP2004203009A JP2003010483A JP2003010483A JP2004203009A JP 2004203009 A JP2004203009 A JP 2004203009A JP 2003010483 A JP2003010483 A JP 2003010483A JP 2003010483 A JP2003010483 A JP 2003010483A JP 2004203009 A JP2004203009 A JP 2004203009A
Authority
JP
Japan
Prior art keywords
thirteen
layer
fifteen
film
och
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2003010483A
Other languages
Japanese (ja)
Other versions
JP4196686B2 (en
Inventor
Takashi Murakami
隆 村上
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Konica Minolta Inc
Original Assignee
Konica Minolta Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Konica Minolta Inc filed Critical Konica Minolta Inc
Priority to JP2003010483A priority Critical patent/JP4196686B2/en
Publication of JP2004203009A publication Critical patent/JP2004203009A/en
Application granted granted Critical
Publication of JP4196686B2 publication Critical patent/JP4196686B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

<P>PROBLEM TO BE SOLVED: To provide an optical film having a metal compound layer formed by plasma treatment, having a stable and excellent endurance performance even when it is subjected to cycle treatment or long-time treatment under conditions of high temperature and high humidity and exhibiting a low reflectance and reduced nonuniformity of color, and also to provide a polarizer and an image display device which are stable even under the conditions of high temperature and high humidity by using the film. <P>SOLUTION: The optical film has at least two active ray-cured resin layers each having a film thickness of 0.5 μm or more on at least one side of a plastic base sheet. At least the lower active ray-cured resin layer contains a plasticizer, and the film has a metal compound layer formed on the upper active ray-cured resin layer directly or with another layer interposed, by the plasma treatment in a gas atmosphere near the atmospheric pressure which contains nitrogen in the main. <P>COPYRIGHT: (C)2004,JPO&NCIPI

Description

【0001】
【発明の属する技術分野】
本発明は、プラスチックフィルム特にセルロースエステルフィルムに複数のハードコート層を設け、その上に大気圧もしくはその近傍の圧力下のプラズマ処理により金属化合物薄膜を形成させた光学フィルム及びその製造方法に関する。更にこれらの光学フィルムから作製される偏光板及び表示装置に関する。
【0002】
【従来の技術】
近年、パーソナルコンピューター、ワードプロセッサー、時計や電卓等に使用される液晶ディスプレイ、プラズマディスプレイ、有機EL等は過酷な環境下で使用されることが多くなって来ている。従って、液晶ディスプレイ等の表示装置に用いられる偏光板、偏光板用保護フィルム、位相差フィルム、反射防止フィルム、帯電防止フィルム、透明導電フィルム、プラズマディスプレイパネル用前面フィルター、無機ELパネルあるいは有機ELパネル用前面フィルム等の光学フィルムについても、当然過酷な環境下でも特性が変化しないよう、例えば、高温高湿下で劣化のないことや寸法安定性に優れていることなどの耐久性が要求される。
【0003】
従来、このような高機能性の薄膜の形成方法は、塗布に代表される塗膜硬化法か、あるいは、スパッタリング法、真空蒸着法、イオンプレーティング法等の真空を用いた乾式薄膜形成法等によってなされていた。
【0004】
上記真空を用いた乾式薄膜形成法は、高精度の薄膜が形成出来るため、高性能の薄膜を形成するには好ましい方法である。しかし、乾式薄膜形成法に用いる真空装置は、被処理基材が大きくなると、装置が非常に大型化し、値段も高額になる他、真空排気にも膨大に時間を費やし、生産性が上げられないデメリットが大きい。
【0005】
上記、真空装置を用いることによる低生産性のデメリットを克服する方法として、大気圧または大気圧近傍の圧力下で放電し、反応性ガスをプラズマ励起し、基材上に薄膜を形成する方法として、大気圧プラズマ法が知られている。
【0006】
上記のような高機能な薄膜を載せる基材としては従来セルローストリアセテート(以降略してTACとすることがある)フィルムが良好な光透過性及び小さい複屈折を有することなどの利点から用いられて来た。
【0007】
一方、表示装置に使用される偏光板はTACフィルムである偏光板用保護フィルムと偏光膜を貼り合わせて出来ているが、吸水し易い偏光膜をカバーする偏光板用保護フィルムの性質が偏光板の特性に影響を与え、カーナビゲーションのように車内で高温高湿に曝されることによる耐久性が問題となっている。また、一般に使用されている表示装置についても経時での同様な劣化現象が見られる。従って、偏光板用保護フィルムは、上述の高温高湿下で劣化のないことや寸法安定性に優れていることなどの良好な耐湿耐熱性が当然要求される。TACフィルムの偏光板用保護フィルムには、フィルムに適度な柔軟性を付与するために、TACフィルム中にリン酸エステル等の可塑剤が含有されている。しかしながら、このような偏光板用保護フィルムを使用した偏光板を高温高湿下で使用した場合、薄膜にクラックがはいったり、偏光板用保護フィルムが偏光膜から剥離したり、あるいは偏光板用保護フィルムが着色する等の問題が発生することがあった。
【0008】
このようなTACフィルムに高機能薄膜を付与した光学フィルムはやはり何らかの影響を受け、薄膜が経時劣化する場合が多い。
【0009】
その中で特許文献1には、2周波印加による大気圧プラズマにより、トリアセチルセルロース上に大気圧プラズマ処理を行うものが記載されている。
【0010】
そこでは、大気圧条件下で、高周波電源を用いた高周波交流パルス波を印加して安定した放電状態を実現させたパルスプラズマの発生方法が提案されている。
【0011】
これは、大気圧近傍の圧力下において対向電極の少なくとも一方の対向面に固体誘電体を設置し、該対向電極間にパルス化された電界を印加することによりグロー放電を生じさせる方法であって、高周波交流パルス波を印加してプラズマを生成することを特徴とするグロー放電プラズマ発生方法、特に放電開始時に高電圧直流をパルス化した電界を印加した後に、高周波交流パルス波を印加してグロー放電プラズマを発生する方法であるが、得られる光学フィルムは耐久性等で十分な安定化は得られない。
【0012】
また、特許文献2にもトリアセチルセルロース上に大気圧プラズマ処理を行うものが記載してあり、TAC等の吸湿性を有するフィルム基材の表面上に、常圧プラズマを用いて薄膜を連続的に形成するにあたり、その基材フィルムに皺が発生することを防止するようにしているが十分でない。
【0013】
即ち、大気圧近傍の圧力下において、フィルム基材Fを対向電極間に通過させながら、対向電極間にパルス電圧を印加することにより放電プラズマを発生させ、その放電プラズマを用いてフィルム基材Fの表面に薄膜を連続的に形成する方法において、金属元素含有アルコキシド0.01〜5体積%、アルゴンガス50〜99.99体積%からなるガス雰囲気下で、対向電極間に、電界強度が1〜90kV/cmとなるようにパルス電圧を印加して薄膜を形成するとともに、その成膜中におけるフィルム基材Fの温度を100℃以下に制御することで、プラズマ放電空間でのフィルム基材の温度(含水率)の変動を抑えるようにしてあるが十分な効果が得られていない。
【0014】
更に、特許文献3には大気圧プラズマ処理で金属化合物層を形成することが開示され、金属化合物層には主に窒素を含有する大気圧によるプラズマを用いることが記載されている。
【0015】
また、特許文献4にはプラスチックフィルムに2層からなるハードコートを施したものが開示されている。
【0016】
【特許文献1】
特開2002−110397号公報
【0017】
【特許文献2】
特開2002−26632号公報
【0018】
【特許文献3】
特開平11−181573号公報
【0019】
【特許文献4】
特開2000−52472号公報
【0020】
【発明が解決しようとする課題】
このように、大気圧プラズマ処理は真空プロセスを用いる方法と比較して安価に機能性膜を形成できるが、反応ガスとして、ヘリウム等の希ガスを用いると安価にできるメリットが失われてしまう。そのため、窒素雰囲気でのプラズマ処理法が提案されているが、窒素雰囲気でのプラズマ処理ではヘリウムよりも安定なプラズマ放電を起こしにくく、膜質が劣ってしまったり、膜質をあげるため放電を強くすると均一な膜が得にくく、すじ状の故障が発生しやすくその改善が求められていた。
【0021】
本発明は、このようなすじ状の故障を低減し、且つ、均一な金属化合物層を形成した光学フィルム及び光学フィルムの製造方法を提案するものであり、更には、高温高湿条件でも物性変動することなく、耐久性に優れかつ均一な金属化合物層を形成した光学フィルム、特に反射光の色むらが低減された光学フィルムを提供し、また、真空プロセスを必要としない大幅なコスト低減を可能にした製造方法を確立し、そのような光学フィルムを用いた偏光板及び表示装置を提供することを課題目的にするものである。
【0022】
【課題を解決するための手段】
この目的は次の技術手段(1)〜(7)の何れかによって達成される。
【0023】
(1) プラスチックの基材シートの少なくとも片方の面に、各々の膜厚が0.5μm以上の少なくとも2層の活性線硬化樹脂層を有し、少なくとも下層の活性線硬化樹脂層は可塑剤を含有し、上層の活性線硬化樹脂層の上に直接又は他の層を介して主に窒素を含有する大気圧近傍のガス雰囲気下でプラズマ処理によって形成された金属化合物層を有することを特徴とする光学フィルム。
【0024】
(2) 前記光学フィルムが分子内に3個以上の芳香族環を有する化合物を含有することを特徴とする(1)項に記載の光学フィルム。
【0025】
(3) プラスチックの基材シートの少なくとも片方の面に、各々の膜厚が0.5μm以上の少なくとも2層のハードコート層の性能を有する活性線硬化樹脂層を形成させ、更にその上に直接又は他の層を介して主に窒素を含有する大気圧近傍のガス雰囲気下でプラズマ処理によって金属化合物層を形成させることを特徴とする光学フィルムの製造方法。
【0026】
(4) 前記プラズマ処理が対向する少なくとも2つの電極との間に窒素を主成分とするガスを供給し、該第1電極と該第2電極との間に高周波電圧を印加することにより前記ガスを励起し、活性線硬化樹脂層が施された前記基材シートを励起された該ガスに晒すことにより該基材シートに施した活性線硬化樹脂層上に金属化合物層を形成させるものであり、該高周波電圧が、第1の周波数ωの電圧成分と、該第1の周波数ωより高い第2の周波数ωの電圧成分とを有することを特徴とする(3)項に記載の光学フィルムの製造方法。
【0027】
(5) 前記ハードコート層として可塑剤を含有する活性線硬化樹脂層を形成した後、巻き取ることなく2層目の活性線硬化樹脂層を設け、更にその上に直接又は他の層を介して主に窒素を含有する大気圧近傍のガス雰囲気下でプラズマ処理によって2層以上の金属化合物層を連続的に形成させることを特徴とする(3)又は(4)項に記載の光学フィルムの製造方法。
【0028】
(6) (1)又は(2)項に記載の光学フィルムを有することを特徴とする偏光板。
【0029】
(7) (1)は(2)項に記載の光学フィルムを有することを特徴とする表示装置。
【0030】
以下、本発明を更に詳細に述べる。
本発明に用いられるプラスチックの基材シートとしては、ポリエチレンテレフタレート等のポリエステル、ポリカーボネート、環状ポリオレフィン、ポリサルフォン、ポリアクリレート、セルロースエステル、ノルボルネン系樹脂(例えばアートン(JSR社製)、ゼオネクス、ゼオノア(日本ゼオン社製))等が用いられるが、特にこれに限定はされない。この中でもセルロースエステル(例えばコニカ(株)製のKC4UX2MW、KC8UX2MW、KC8UN、KC5UN、KC4UY、KC12UR)が好ましく用いられる。
【0031】
以下の説明では基材シートはセルロースエステルを用いて行う。
本発明において、後述のごとく、ドープ調製工程がセルロースエステル溶液調製工程とインライン添加液調製工程に分かれており、それらをインラインで合流し混合してドープを調製することが好ましい。そこで、本発明において、後述の流延ダイに導入する状態のものをドープといい、合流する前のもの、即ち、基材となるセルロースエステルを含有する液をセルロースエステル溶液、また可塑剤やUV剤やマット剤等微粒子等を含有するものをインライン添加液ということとする。
【0032】
〔基材シートのフィルム〕
本発明に用いる基材シートFの一例はセルロースエステルフィルムの層構成が1層の基層を有するもので最も一般的に用いられるものであり、他の例は多層構造のものであり、1層の基層と少なくとも1層の表層を有するものであり層数は2層以上で、形成された一つの表層あるいは基層が複数層からなっているものでも良い。
【0033】
図1(a)は単層構造の、図1(b)は3層構造のフィルムの断面を模式的に示したものであり、図中21と23は表層、また22は基層を示している。
【0034】
〔共流延と逐次流延〕
本発明に用いる多層構造のセルロースエステルフィルムは、溶液流延製膜過程において、共流延または逐次流延によりドープを多層に積層して得られるものである。
【0035】
図2は共流延ダイ及び流延して多層構造ウェブ(流延直後はウェブをドープ膜ともいうことがある)を形成したところを表した図である。共流延は図2に示すように、共流延ダイ10の口金部分11に複数(図2では三つ)の表層用スリット13と15、基層用スリット14を有しており、金属支持体16の上に同時にそれぞれのスリットから表層用ドープ17、基層用ドープ18、及び表層用ドープ19を流延することにより、表層21/基層22/表層23の多層構造の基材シートFとしてのウェブ20を形成する。
【0036】
図3は逐次流延ダイ及び流延された多層構造のウェブを表した図である。逐次流延は、図3に示すように、金属支持体16の上方に複数(図3では三つ)の表層用流延ダイ30、基層用ダイ31及び表層用流延ダイ32を異なった場所に順に設置し、最初に表層用ダイ30から片方の表層となる表層用ドープ33が流延されて表層ドープ膜36を金属支持体16上に形成し、次に基層用ドープ34が基層用ダイ31から表層ドープ膜36の上に基層ドープ膜37を形成し、更に次の表層用ダイ32から表層用ドープ35を流延して表層ドープ膜38を形成することにより、表層/基層/表層をもつ基材シートFとしての多層構造ウェブ39を形成する。
【0037】
図4は別のタイプの共流延ダイの断面を示した図である。本体中で3層が合流する共流延ダイ50は、基層用のスリット52、表層用のスリット51と53中にそれぞれ、基層用ドープ56、表層用ドープ55と57が導入されており、それが合流スリット58で合流し、層流をなしてスリット54を通過し、金属支持体16の上に表層/基層/表層の3層揃って流延する様式の基材シートFである。
【0038】
図2、3及び4で示したような多層構造ウェブの表層が基層より幅広く、基層ウェブを表層ウェブが包み込むように流延するのが好ましい。
【0039】
尚、単層構造の基材シートを作るには前記ダイのなかの何れか1つののスリットを用いて1層のみを流延して基材シートを作ることができる。
【0040】
〔溶液流延製膜方法〕
本発明のセルロースエステルフィルムは、溶液流延製膜法により製膜される。ここで、本発明に係わる溶液流延製膜方法について図5を用いて説明する。
【0041】
図5は、本発明に係わる溶液流延製膜装置のドープ調製工程、流延工程を模式的に示した図である。以下の工程は2層共流延を例として、代表的な工程を説明する。
【0042】
▲1▼セルロースエステル溶液調製工程:
後述のセルロースエステルに対する良溶媒を主とする有機溶媒に溶解釜101中でセルロースエステルや可塑剤等の添加剤を攪拌しながら溶解し、セルロースエステル溶液100を形成する工程である。溶解には、常圧で行う方法、主溶媒の沸点以下で行う方法、主溶媒の沸点以上で加圧して行う高温溶解方法、冷却して溶解する冷却溶解方法、かなりの高圧で行う高圧溶解方法等種々の溶解方法があるが、本発明においては、高温溶解方法が好ましく用いられる。溶解後セルロースエステル溶液100を送液ポンプ102で濾過器103(フィルタープレス型)で濾過し、ストックタンク104で静置して脱泡し、流延のために送液ポンプ105(加圧型定量ギヤポンプ等が多く用いられる)で溶液を移送し、濾過器106を経てマット剤分散液あるいは紫外線吸収剤添加液等のインライン添加液110と合流する合流管120で混合するために導管108で移送する。基層あるいは表層に使用するドープでマット剤あるいは紫外線吸収剤等の添加剤を含有しない場合には、濾過器106を経た後は流延ダイに直送することが行われる。
【0043】
濾過については、このセルロースエステル溶液をフィルタープレス用の濾紙などの適当な濾材を用いて濾過する。本発明における濾過材としては、不溶物などを除去するために絶対濾過精度が小さい方が好ましいが、絶対濾過精度が小さすぎると濾過材の目詰まりが発生しやすいという問題点があり、絶対濾過精度8μm以下の濾材が好ましく、1〜8μmの範囲の濾材がより好ましく、3〜6μmの範囲の濾材が更に好ましい。濾紙としては、例えば市販品の安積濾紙(株)のNo.244や277などを挙げることが出来、好ましく用いられる。更なる濾過の濾材の材質は特に制限はなく、通常の濾材を使用することが出来るが、ポリプロピレン、テフロン(R)等のプラスチック製の濾材やステンレス等の金属製の濾材が繊維の脱落等がなく好ましい。濾過は通常の方法で行うことが出来るが、加圧下で、使用有機溶媒の常圧での沸点以上で、且つ有機溶媒が沸騰しない範囲の温度で加熱または保温しながら濾過する方法が、濾過材前後の差圧(以下、濾圧とすることがある)の上昇が小さく、好ましい。好ましい温度範囲は使用有機溶媒に依存するが、45〜120℃であり、45〜70℃がより好ましく、45〜55℃の範囲であることが更に好ましい。濾圧は小さい方が好ましく、0.3〜1.6MPaであることが好ましく、0.3〜1.2MPaであることがより好ましく、0.3〜1.0MPaであることが更に好ましい。なお、予め溶解釜101内で紫外線吸収剤をセルロースエステル溶液に添加してもよい。
【0044】
また、分子内に3個以上の芳香族環を有する化合物としてはトリフェニレン環を有する化合物あるいは次の化1に示す1,3,5−トリアジン化合物が好ましい。
【0045】
【化1】

Figure 2004203009
【0046】
上記添加剤の具体的例の一つとしてトリフェニレン環を有する化合物が挙げられ、その中でも、下記一般式(I)で表される化合物であることが好ましい。
【0047】
【化2】
Figure 2004203009
【0048】
一般式(I)において、R、R、R、R、R及びRは、各々水素原子、ハロゲン原子、ニトロ、スルホ、脂肪族基、芳香族基、複素環基、−O−R11、−S−R12、−CO−R13、−O−CO−R14、−CO−O−R15、−O−CO−O−R16、−NR1718、−CO−NR1920、−NR21−CO−R22、−O−CO−NR2324、−SiR252627、−O−SiR282930、−S−CO−R31、−O−SO−R32、−SO−R33、−NR34−CO−O−R35、−SO−R36又は−NR37−CO−NR3839
11、R12、R13、R14、R15、R16、R17、R18、R19、R20、R21、R22、R23、R24、R25、R26、R27、R28、R29、R30、R31、R32、R33、R34、R35、R36、R37、R38及びR39は、水素原子、脂肪族基、芳香族基又は複素環基である。また、RとR、RとR又はRとRは互いに結合して環を形成してもよい。
【0049】
、R、R、R、R及びRは、−O−R11、−S−R12、−O−CO−R14、−O−CO−O−R16、−NR1718、−NR21−CO−R22又は−O−CO−NR2324であることが好ましく、−O−R11、−S−R12、−O−CO−R14、−O−CO−O−R16又は−O−CO−NR2324であることがより好ましく、−O−R11又は−O−CO−R14であることがさらに好ましく、−O−CO−R14であることが最も好ましい。
【0050】
11、R12、R13、R14、R15、R16、R17、R18、R19、R20、R21、R22、R23、R24、R25、R26、R27、R28、R29、R30、R31、R32、R33、R34、R35、R36、R37、R38及びR39は、各々水素原子、脂肪族基又は芳香族基であることが好ましい。−O−CO−R14のR14は、芳香族基であることが最も好ましい。
【0051】
一般式(I)において、R、R、R、R、R及びRは、同一の基であることが好ましい。
【0052】
脂肪族基としては、例えばアルキル基、アルケニル基、アルキニル基、置換アルキル基、置換アルケニル基又は置換アルキニル基があげられる。
【0053】
アルキル基は、環状(例えばシクロアルキル基等)であってもよく、また、アルキル基は分岐をしていてもよい。アルキル基の炭素原子数は、1〜30であることが好ましく、1〜20であることがさらに好ましく、1〜10であることが最も好ましい。
【0054】
アルキル基の具体例としては、例えばメチル、エチル、i−プロピル、ブチル、i−ブチル、s−ブチル、t−ブチル、t−ペンチル、ヘキシル、オクチル、t−オクチル、ドデシル又はテトラコシル等の各基が挙げられる。
【0055】
アルケニル基は、環状(シクロアルケニル基)であってもよく、また、アルケニル基は、分岐していてもよい。さらに、アルケニル基は、二つ以上の二重結合を有していてもよい。
【0056】
アルケニル基の炭素原子数は、2〜30であることが好ましく、2〜20であることがさらに好ましく、2〜10であることが最も好ましい。
【0057】
アルケニル基の具体例としては、ビニル、アリル又は3−ヘプテニルが挙げられる。アルキニル基は、環状(シクロアルキニル基)であってもよく、また、アルキニル基は、分岐を有していてもよい。
【0058】
さらに、アルキニル基は、二つ以上の三重結合を有していてもよい。アルキニル基の炭素原子数は、2〜30であることが好ましく、2〜20であることがさらに好ましく、2〜10であることが最も好ましい。
【0059】
アルキニル基の具体例としては、エチニル、2−プロピニル、1−ペンチニル及び2,4−オクタジイニル等の各基が挙げられる。
【0060】
置換アルキル基、置換アルケニル基及び置換アルキニル基の置換基の具体例としては、例えばハロゲン原子、ニトロ、スルホ、芳香族基、複素環基、−O−R41、−S−R42、−CO−R43、−O−CO−R44、−CO−O−R45、−O−CO−O−R46、−NR4748、−CO−NR4950、−NR51−CO−R52、−O−CO−NR5354、−SiR55565758又は−O−SiR59606162が等が挙げられる。
【0061】
41、R42、R43、R44、R45、R46、R47、R48、R49、R50、R51、R52、R53、R54、R55、R56、R57、R58、R59、R60、R61又はR62は、水素原子、脂肪族基、芳香族基又は複素環基である。置換アルキル基のアルキル部分は、上記アルキル基と同様である。
【0062】
置換アルキル基の具体例としては、ベンジル、フェネチル、2−メトキシエチル、エトキシメチル、2−(2−メトキシエトキシ)エチル、2−ヒドロキシエチル、ヒドロキシメチル、2−カルボキシエチル、カルボキシメチル、エトキシカルボニルメチル、4−アクリロイルオキシブチル、トリクロロメチル又はパーフルオロペンチル等の各基が挙げられる。置換アルケニル基のアルケニル部分は、上記アルケニル基と同様である。置換アルケニル基の具体例としては、例えばスチリル及び4−メトキシスチリル等の各基が挙げられる。
【0063】
置換アルキニル基のアルキニル部分は、上記アルキニル基と同様である。置換アルキニル基の具体例としては、4−ブトキシフェニルエチニル、4−プロピルフェニルエチニル又はトリメチルシリルエチニル等の各基が挙げられる。
【0064】
本発明において、芳香族基は、アリール基及び置換アリール基を意味する。
アリール基の炭素原子数は、6〜30であることが好ましく、6〜20であることがさらに好ましく、6〜10であることが最も好ましい。
【0065】
アリール基の具体例としては、例えば、フェニル、1−ナフチル又は2−ナフチル等の各基が挙げられる。
【0066】
置換アリール基の置換基の具体例としては、例えば、ハロゲン原子、ニトロ基、スルホ基、脂肪族基、芳香族基、複素環基、−O−R71、−S−R72、−CO−R73、−O−CO−R74、−CO−O−R75、−O−CO−O−R76、−NR7778、−CO−NR7980、−NR81−CO−R82、−O−CO−NR8384、−SiR85868788又は−O−SiR89909192等が挙げられる。
【0067】
71、R72、R73、R74、R75、R76、R77、R78、R79、R80、R81、R82、R83、R84、R85、R86、R87、R88、R89、R90、R91及びR92は、水素原子、脂肪族基、芳香族基又は複素環基である。
【0068】
置換アリール基のアリール部分は、上記アリール基と同義である。
置換アリール基の具体例としては、p−ビフェニリル、4−フェニルエチニルフェニル、2−メトキシフェニル、3−メトキシフェニル、4−メトキシフェニル、2−エトキシフェニル、3−エトキシフェニル、4−エトキシフェニル、2−プロポキシフェニル、3−プロポキシフェニル、4−プロポキシフェニル、2−ブトキシフェニル、3−ブトキシフェニル、4−ブトキシフェニル、2−ヘキシルオキシフェニル、3−ヘキシルオキシフェニル、4−ヘキシルオキシフェニル、2−オクチルオキシフェニル、3−オクチルオキシフェニル、4−オクチルオキシフェニル、2−ドデシルオキシフェニル、3−ドデシルオキシフェニル、4−ドデシルオキシフェニル、2−テトラコシルオキシフェニル、3−テトラコシルオキシフェニル、4−テトラコシルオキシフェニル、3,4−ジメトキシフェニル、3,4−ジエトキシフェニル、3,4−ジヘキシルオキシフェニル、2,4−ジメトキシフェニル、2,4−ジエトキシフェニル、2,4−ジヘキシルオキシフェニル、3,5−ジメトキシフェニル、3,5−ジメトキシフェニル、3,5−ジヘキシルオキシフェニル、3,4,5−トリメトキシフェニル、3,4,5−トリエトキシフェニル、3,4,5−トリヘキシルオキシフェニル、2,4,6−トリメトキシフェニル、2,4,6−トリエトキシフェニル、2,4,6−トリヘキシルオキシフェニル、2−フルオロフェニル、3−フルオロフェニル、4−フルオロフェニル、2−クロロフェニル、3−クロロフェニル、4−クロロフェニル、2−ブロモフェニル、3−ブロモフェニル、4−ブロモフェニル、3,4−ジフルオロフェニル、3,4−ジクロロフェニル、3,4−ジブロモフェニル、2,4−ジフルオロフェニル、2,4−ジクロロフェニル、2,4−ジブロモフェニル、3,5−ジフルオロフェニル、3,5−ジクロロフェニル、3,5−ジブロモフェニル、3,4,5−トリフルオロフェニル、3,4,5−トリクロロフェニル、3,4,5−トリブロモフェニル、2,4,6−トリフルオロフェニル、2,4,6−トリクロロフェニル、2,4,6−トリブロモフェニル、ペンタフルオロフェニル、ペンタクロロフェニル、ペンタブロモフェニル、2−ヨードフェニル、3−ヨードフェニル、4−ヨードフェニル、2−ホルミルフェニル、3−ホルミルフェニル、4−ホルミルフェニル、2−ベンゾイルフェニル、3−ベンゾイルフェニル、4−ベンゾイルフェニル、2−カルボキシフェニル、3−カルボキシフェニル、4−カルボキシフェニル、o−トリル、m−トリル、p−トリル、2−エチルフェニル、3−エチルフェニル、4−エチルフェニル、2−(2−メトキシエトキシ)フェニル、3−(2−メトキシエトキシ)フェニル、4−(2−メトキシエトキシ)フェニル、2−エトキシカルボニルフェニル、3−エトキシカルボニルフェニル、4−エトキシカルボニルフェニル、2−ベンゾイルオキシフェニル、3−ベンゾイルオキシフェニル及び4−ベンゾイルオキシフェニル等の各基が挙げられる。
【0069】
本発明においては、複素環基は置換基を有していてもよい。複素環基中の複素環は5員環又は6員環であることが好ましい。複素環基中の複素環に脂肪族環、芳香族環又は他の複素環が縮合していてもよい。複素環中のヘテロ原子としては、例えばB、N、O、S、Se又はTe等の各原子が挙げられる。
【0070】
複素環基中の複素環の具体例としては、例えば、ピロリジン環、モルホリン環、2−ボラ−1,3−ジオキソラン環及び1,3−チアゾリジン環等が挙げられる。
【0071】
不飽和複素環基中の不飽和複素環の具体例としては、例えば、イミダゾール環、チアゾール環、ベンゾチアゾール環、ベンゾオキサゾール環、ベンゾトリアゾール環、ベンゾセレナゾール環、ピリジン環、ピリミジン環又はキノリン環等が挙げられる。
【0072】
複素環基の置換基の具体例としては、前記置換アリール基の置換基の具体例と同様である。
【0073】
トリフェニレン環を有する化合物の分子量は、300〜2000であることが好ましい。化合物の沸点は260℃以上であることが好ましい。沸点は、市販の測定装置(例えば、TG/DTA100、セイコー電子工業(株)製)を用いて測定できる。以下に、トリフェニレン環を有する化合物の具体例を示す。
【0074】
尚、以下に示す複数のRは同一の基を意味する。
【0075】
【化3】
Figure 2004203009
【0076】
(1)フルオロ
(2)クロロ
(3)ブロモ
(4)ホルミル
(5)ベンゾイル
(6)カルボキシル
(7)ブチルアミノ
(8)ジベンジルアミノ
(9)トリメチルシリルオキシ
(10)1−ペンチニル
(11)エトキシカルボニル
(12)2−ヒドロキシエトキシカルボニル
(13)フェノキシカルボニル
(14)N−フェニルカルバモイル
(15)N,N−ジエチルカルバモイル
(16)4−メトキシベンゾイルオキシ
(17)N−フェニルカルバモイルオキシ
(18)ヘキシルオキシ
(19)4−ヘキシルオキシベンゾイルオキシ
(20)エトキシ
(21)ベンゾイルオキシ
(22)m−ドデシルオキシフェニルチオ
(23)t−オクチルチオ
(24)p−フルオロベンゾイルチオ
(25)イソブチリルチオ
(26)p−メチルベンゼンスルフィニル
(27)エタンスルフィニル
(28)ベンゼンスルホニル
(29)メタンスルホニル
(30)2−メトキシエトキシ
(31)プロポキシ
(32)2−ヒドロキシエトキシ
(33)2−カルボキシエトキシ
(34)3−ヘプテニルオキシ
(35)2−フェニルエトキシ
(36)トリクロロメトキシ
(37)2−プロピニルオキシ
(38)2,4−オクタジイニルオキシ
(39)パーフルオロペンチルオキシ
(40)エトキシカルボニルメトキシ
(41)p−メトキシフェノキシ
(42)m−エトキシフェノキシ
(43)o−クロロフェノキシ
(44)m−ドデシルオキシフェノキシ
(45)4−ピリジルオキシ
(46)ペンタフルオロベンゾイルオキシ
(47)p−ヘキシルオキシベンゾイルオキシ
(48)1−ナフトイルオキシ
(49)2−ナフトイルオキシ
(50)5−イミダゾールカルボニルオキシ
(51)o−フェノキシカルボニルベンゾイルオキシ
(52)m−(2−メトキシエトキシ)ベンゾイルオキシ
(53)o−カルボキシベンゾイルオキシ
(54)p−ホルミルベンゾイルオキシ
(55)m−エトキシカルボニルベンゾイルオキシ
(56)p−ピバロイルベンゾイルオキシ
(57)プロピオニルオキシ
(58)フェニルアセトキシ
(59)シンナモイルオキシ
(60)ヒドロキシアセトキシ
(61)エトキシカルボニルアセトキシ
(62)m−ブトキシフェニルプロピオロイルオキシ
(63)プロピオロイルオキシ
(64)トリメチルシリルプロピオロイルオキシ
(65)4−オクテノイルオキシ
(66)3−ヒドロキシプロピオニルオキシ
(67)2−メトキシエトキシアセトキシ
(68)パーフルオロブチリルオキシ
(69)メタンスルホニルオキシ
(70)p−トルエンスルホニルオキシ
(71)トリエチルシリル
(72)m−ブトキシフェノキシカルボニルアミノ
(73)ヘキシル
(74)フェニル
(75)4−ピリジル
(76)ベンジルオキシカルボニルオキシ
(77)m−クロロベンズアミド
(78)4−メチルアニリノ
【0077】
【化4】
Figure 2004203009
【0078】
(79)ニトロ
(80)スルホ
(81)ホルミル
(82)カルボキシル
(83)メトキシカルボニル
(84)ベンジルオキシカルボニル
(85)フェノキシカルボニル
【0079】
【化5】
Figure 2004203009
【0080】
(86)ブトキシ
(87)ヘキシルオキシ
(88)ドデシルオキシ
(89)ヘキサノイルオキシ
(90)カルボキシメトキシ
【0081】
【化6】
Figure 2004203009
【0082】
【化7】
Figure 2004203009
【0083】
【化8】
Figure 2004203009
【0084】
【化9】
Figure 2004203009
【0085】
【化10】
Figure 2004203009
【0086】
【化11】
Figure 2004203009
【0087】
円盤状化合物としては、1,3,5−トリアジン環を有する化合物又はポルフィリン骨格を有する化合物を好ましく用いることができる。
【0088】
1,3,5−トリアジン環を有する化合物は、中でも、下記一般式(III)で表される化合物が好ましい。
【0089】
【化12】
Figure 2004203009
【0090】
一般式(III)において、Xは、単結合、−NR−、−O−又は−S−であり;Xは単結合、−NR−、−O−又は−S−であり;Xは単結合、−NR−、−O−又は−S−であり;R、R及びRはアルキル基、アルケニル基、アリール基又は複素環基であり;そして、R、R及びRは、水素原子、アルキル基、アルケニル基、アリール基又は複素環基である。一般式(I)で表される化合物は、メラミン化合物であることが特に好ましい。
【0091】
メラミン化合物では、一般式(I)において、X、X及びXが、それぞれ、−NR−、−NR−及び−NR−であるか、あるいは、X、X及びXが単結合であり、かつ、R、R及びRが窒素原子に遊離原子価をもつ複素環基である。−X−R、−X−R及び−X−Rは、同一の置換基であることが好ましい。R、R及びRは、アリール基であることが特に好ましい。R、R及びRは、水素原子であることが特に好ましい。
【0092】
上記アルキル基は、環状アルキル基よりも鎖状アルキル基である方が好ましい。分岐を有する鎖状アルキル基よりも、直鎖状アルキル基の方が好ましい。
【0093】
アルキル基の炭素原子数は、1〜30であることが好ましく、1〜20であることがより好ましく、1〜10であることがさらに好ましく、1〜8であることがさらにまた好ましく、1〜6であることが最も好ましい。アルキル基は置換基を有していてもよい。
【0094】
置換基の具体例としては、例えばハロゲン原子、アルコキシ基(例えばメトキシ、エトキシ、エポキシエチルオキシ等の各基)及びアシルオキシ基(例えば、アクリロイルオキシ、メタクリロイルオキシ)等が挙げられる。上記アルケニル基は、環状アルケニル基よりも鎖状アルケニル基である方が好ましい。分岐を有する鎖状アルケニル基よりも、直鎖状アルケニル基の方が好ましい。アルケニル基の炭素原子数は、2〜30であることが好ましく、2〜20であることがより好ましく、2〜10であることがさらに好ましく、2〜8であることがさらにまた好ましく、2〜6であることが最も好ましい。アルケニル基は、置換基を有していてもよい。
【0095】
置換基の具体例としては、ハロゲン原子、アルコキシ基(例えば、メトキシ、エトキシ、エポキシエチルオキシ等の各基)又はアシルオキシ基(例えば、アクリロイルオキシ、メタクリロイルオキシ等の各基)が挙げられる。
【0096】
上記アリール基は、フェニル基又はナフチル基であることが好ましく、フェニル基であることが特に好ましい。アリール基は置換基を有していてもよい。
【0097】
置換基の具体例としては、例えば、ハロゲン原子、ヒドロキシル、シアノ、ニトロ、カルボキシル、アルキル基、アルケニル基、アリール基、アルコキシ基、アルケニルオキシ基、アリールオキシ基、アシルオキシ基、アルコキシカルボニル基、アルケニルオキシカルボニル基、アリールオキシカルボニル基、スルファモイル、アルキル置換スルファモイル基、アルケニル置換スルファモイル基、アリール置換スルファモイル基、スルホンアミド基、カルバモイル、アルキル置換カルモイル基、アルケニル置換カルバモイル基、アリール置換カルバモイル基、アミド基、アルキルチオ基、アルケニルチオ基、アリールチオ基及びアシル基が含まれる。上記アルキル基は、前述したアルキル基と同義である。
【0098】
アルコキシ基、アシルオキシ基、アルコキシカルボニル基、アルキル置換スルファモイル基、スルホンアミド基、アルキル置換カルバモイル基、アミド基、アルキルチオ基とアシル基のアルキル部分も、前述したアルキル基と同義である。
【0099】
上記アルケニル基は、前述したアルケニル基と同義である。
アルケニルオキシ基、アシルオキシ基、アルケニルオキシカルボニル基、アルケニル置換スルファモイル基、スルホンアミド基、アルケニル置換カルバモイル基、アミド基、アルケニルチオ基及びアシル基のアルケニル部分も、前述したアルケニル基と同義である。
【0100】
上記アリール基の具体例としては、例えば、フェニル、α−ナフチル、β−ナフチル、4−メトキシフェニル、3,4−ジエトキシフェニル、4−オクチルオキシフェニル又は4−ドデシルオキシフェニル等の各基が挙げられる。
【0101】
アリールオキシ基、アシルオキシ基、アリールオキシカルボニル基、アリール置換スルファモイル基、スルホンアミド基、アリール置換カルバモイル基、アミド基、アリールチオ基およびアシル基の部分の例は、上記アリール基と同義である。
【0102】
、X又はXが−NR−、−O−又は−S−である場合の複素環基は、芳香族性を有することが好ましい。
【0103】
芳香族性を有する複素環基中の複素環としては、一般に不飽和複素環であり、好ましくは最多の二重結合を有する複素環である。複素環は、5員環、6員環又は7員環であることが好ましく、5員環又は6員環であることがさらに好ましく、6員環であることが最も好ましい。
【0104】
複素環中のヘテロ原子は、N、S又はO等の各原子であることが好ましく、N原子であることが特に好ましい。
【0105】
芳香族性を有する複素環としては、ピリジン環(複素環基としては、例えば、2−ピリジル又は4−ピリジル等の各基)が特に好ましい。複素環基は、置換基を有していてもよい。複素環基の置換基の例は、上記アリール部分の置換基の例と同様である。
【0106】
、X又はXが単結合である場合の複素環基は、窒素原子に遊離原子価をもつ複素環基であることが好ましい。窒素原子に遊離原子価をもつ複素環基は、5員環、6員環又は7員環であることが好ましく、5員環又は6員環であることがさらに好ましく、5員環であることが最も好ましい。複素環基は、複数の窒素原子を有していてもよい。
【0107】
また、複素環基中のヘテロ原子は、窒素原子以外のヘテロ原子(例えば、O原子、S原子)を有していてもよい。複素環基は、置換基を有していてもよい。複素環基の置換基の具体例は、上記アリール部分の置換基の具体例と同義である。
【0108】
以下に、窒素原子に遊離原子価をもつ複素環基の具体例を示す。
【0109】
【化13】
Figure 2004203009
【0110】
【化14】
Figure 2004203009
【0111】
1,3,5−トリアジン環を有する化合物の分子量は、300〜2000であることが好ましい。該化合物の沸点は、260℃以上であることが好ましい。沸点は、市販の測定装置(例えば、TG/DTA100、セイコー電子工業(株)製)を用いて測定できる。
【0112】
以下に、1,3,5−トリアジン環を有する化合物の具体例を示す。
なお、以下に示す複数のRは、同一の基を表す。
【0113】
【化15】
Figure 2004203009
【0114】
(1)ブチル
(2)2−メトキシ−2−エトキシエチル
(3)5−ウンデセニル
(4)フェニル
(5)4−エトキシカルボニルフェニル
(6)4−ブトキシフェニル
(7)p−ビフェニリル
(8)4−ピリジル
(9)2−ナフチル
(10)2−メチルフェニル
(11)3,4−ジメトキシフェニル
(12)2−フリル
【0115】
【化16】
Figure 2004203009
【0116】
【化17】
Figure 2004203009
【0117】
(14)フェニル
(15)3−エトキシカルボニルフェニル
(16)3−ブトキシフェニル
(17)m−ビフェニリル
(18)3−フェニルチオフェニル
(19)3−クロロフェニル
(20)3−ベンゾイルフェニル
(21)3−アセトキシフェニル
(22)3−ベンゾイルオキシフェニル
(23)3−フェノキシカルボニルフェニル
(24)3−メトキシフェニル
(25)3−アニリノフェニル
(26)3−イソブチリルアミノフェニル
(27)3−フェノキシカルボニルアミノフェニル
(28)3−(3−エチルウレイド)フェニル
(29)3−(3,3−ジエチルウレイド)フェニル
(30)3−メチルフェニル
(31)3−フェノキシフェニル
(32)3−ヒドロキシフェニル
(33)4−エトキシカルボニルフェニル
(34)4−ブトキシフェニル
(35)p−ビフェニリル
(36)4−フェニルチオフェニル
(37)4−クロロフェニル
(38)4−ベンゾイルフェニル
(39)4−アセトキシフェニル
(40)4−ベンゾイルオキシフェニル
(41)4−フェノキシカルボニルフェニル
(42)4−メトキシフェニル
(43)4−アニリノフェニル
(44)4−イソブチリルアミノフェニル
(45)4−フェノキシカルボニルアミノフェニル
(46)4−(3−エチルウレイド)フェニル
(47)4−(3,3−ジエチルウレイド)フェニル
(48)4−メチルフェニル
(49)4−フェノキシフェニル
(50)4−ヒドロキシフェニル
(51)3,4−ジエトキシカルボニルフェニル
(52)3,4−ジブトキシフェニル
(53)3,4−ジフェニルフェニル
(54)3,4−ジフェニルチオフェニル
(55)3,4−ジクロロフェニル
(56)3,4−ジベンゾイルフェニル
(57)3,4−ジアセトキシフェニル
(58)3,4−ジベンゾイルオキシフェニル
(59)3,4−ジフェノキシカルボニルフェニル
(60)3,4−ジメトキシフェニル
(61)3,4−ジアニリノフェニル
(62)3,4−ジメチルフェニル
(63)3,4−ジフェノキシフェニル
(64)3,4−ジヒドロキシフェニル
(65)2−ナフチル
(66)3,4,5−トリエトキシカルボニルフェニル
(67)3,4,5−トリブトキシフェニル
(68)3,4,5−トリフェニルフェニル
(69)3,4,5−トリフェニルチオフェニル
(70)3,4,5−トリクロロフェニル
(71)3,4,5−トリベンゾイルフェニル
(72)3,4,5−トリアセトキシフェニル
(73)3,4,5−トリベンゾイルオキシフェニル
(74)3,4,5−トリフェノキシカルボニルフェニル
(75)3,4,5−トリメトキシフェニル
(76)3,4,5−トリアニリノフェニル
(77)3,4,5−トリメチルフェニル
(78)3,4,5−トリフェノキシフェニル
(79)3,4,5−トリヒドロキシフェニル
【0118】
【化18】
Figure 2004203009
【0119】
(80)フェニル
(81)3−エトキシカルボニルフェニル
(82)3−ブトキシフェニル
(83)m−ビフェニリル
(84)3−フェニルチオフェニル
(85)3−クロロフェニル
(86)3−ベンゾイルフェニル
(87)3−アセトキシフェニル
(88)3−ベンゾイルオキシフェニル
(89)3−フェノキシカルボニルフェニル
(90)3−メトキシフェニル
(91)3−アニリノフェニル
(92)3−イソブチリルアミノフェニル
(93)3−フェノキシカルボニルアミノフェニル
(94)3−(3−エチルウレイド)フェニル
(95)3−(3,3−ジエチルウレイド)フェニル
(96)3−メチルフェニル
(97)3−フェノキシフェニル
(98)3−ヒドロキシフェニル
(99)4−エトキシカルボニルフェニル
(100)4−ブトキシフェニル
(101)p−ビフェニリル
(102)4−フェニルチオフェニル
(103)4−クロロフェニル
(104)4−ベンゾイルフェニル
(105)4−アセトキシフェニル
(106)4−ベンゾイルオキシフェニル
(107)4−フェノキシカルボニルフェニル
(108)4−メトキシフェニル
(109)4−アニリノフェニル
(110)4−イソブチリルアミノフェニル
(111)4−フェノキシカルボニルアミノフェニル
(112)4−(3−エチルウレイド)フェニル
(113)4−(3,3−ジエチルウレイド)フェニル
(114)4−メチルフェニル
(115)4−フェノキシフェニル
(116)4−ヒドロキシフェニル
(117)3,4−ジエトキシカルボニルフェニル
(118)3,4−ジブトキシフェニル
(119)3,4−ジフェニルフェニル
(120)3,4−ジフェニルチオフェニル
(121)3,4−ジクロロフェニル
(122)3,4−ジベンゾイルフェニル
(123)3,4−ジアセトキシフェニル
(124)3,4−ジベンゾイルオキシフェニル
(125)3,4−ジフェノキシカルボニルフェニル
(126)3,4−ジメトキシフェニル
(127)3,4−ジアニリノフェニル
(128)3,4−ジメチルフェニル
(129)3,4−ジフェノキシフェニル
(130)3,4−ジヒドロキシフェニル
(131)2−ナフチル
(132)3,4,5−トリエトキシカルボニルフェニル
(133)3,4,5−トリブトキシフェニル
(134)3,4,5−トリフェニルフェニル
(135)3,4,5−トリフェニルチオフェニル
(136)3,4,5−トリクロロフェニル
(137)3,4,5−トリベンゾイルフェニル
(138)3,4,5−トリアセトキシフェニル
(139)3,4,5−トリベンゾイルオキシフェニル
(140)3,4,5−トリフェノキシカルボニルフェニル
(141)3,4,5−トリメトキシフェニル
(142)3,4,5−トリアニリノフェニル
(143)3,4,5−トリメチルフェニル
(144)3,4,5−トリフェノキシフェニル
(145)3,4,5−トリヒドロキシフェニル
【0120】
【化19】
Figure 2004203009
【0121】
(146)フェニル
(147)4−エトキシカルボニルフェニル
(148)4−ブトキシフェニル
(149)p−ビフェニリル
(150)4−フェニルチオフェニル
(151)4−クロロフェニル
(152)4−ベンゾイルフェニル
(153)4−アセトキシフェニル
(154)4−ベンゾイルオキシフェニル
(155)4−フェノキシカルボニルフェニル
(156)4−メトキシフェニル
(157)4−アニリノフェニル
(158)4−イソブチリルアミノフェニル
(159)4−フェノキシカルボニルアミノフェニル
(160)4−(3−エチルウレイド)フェニル
(161)4−(3,3−ジエチルウレイド)フェニル
(162)4−メチルフェニル
(163)4−フェノキシフェニル
(164)4−ヒドロキシフェニル
【0122】
【化20】
Figure 2004203009
【0123】
(165)フェニル
(166)4−エトキシカルボニルフェニル
(167)4−ブトキシフェニル
(168)p−ビフェニリル
(169)4−フェニルチオフェニル
(170)4−クロロフェニル
(171)4−ベンゾイルフェニル
(172)4−アセトキシフェニル
(173)4−ベンゾイルオキシフェニル
(174)4−フェノキシカルボニルフェニル
(175)4−メトキシフェニル
(176)4−アニリノフェニル
(177)4−イソブチリルアミノフェニル
(178)4−フェノキシカルボニルアミノフェニル
(179)4−(3−エチルウレイド)フェニル
(180)4−(3,3−ジエチルウレイド)フェニル
(181)4−メチルフェニル
(182)4−フェノキシフェニル
(183)4−ヒドロキシフェニル
【0124】
【化21】
Figure 2004203009
【0125】
(184)フェニル
(185)4−エトキシカルボニルフェニル
(186)4−ブトキシフェニル
(187)p−ビフェニリル
(188)4−フェニルチオフェニル
(189)4−クロロフェニル
(190)4−ベンゾイルフェニル
(191)4−アセトキシフェニル
(192)4−ベンゾイルオキシフェニル
(193)4−フェノキシカルボニルフェニル
(194)4−メトキシフェニル
(195)4−アニリノフェニル
(196)4−イソブチリルアミノフェニル
(197)4−フェノキシカルボニルアミノフェニル
(198)4−(3−エチルウレイド)フェニル
(199)4−(3,3−ジエチルウレイド)フェニル
(200)4−メチルフェニル
(201)4−フェノキシフェニル
(202)4−ヒドロキシフェニル
【0126】
【化22】
Figure 2004203009
【0127】
(203)フェニル
(204)4−エトキシカルボニルフェニル
(205)4−ブトキシフェニル
(206)p−ビフェニリル
(207)4−フェニルチオフェニル
(208)4−クロロフェニル
(209)4−ベンゾイルフェニル
(210)4−アセトキシフェニル
(211)4−ベンゾイルオキシフェニル
(212)4−フェノキシカルボニルフェニル
(213)4−メトキシフェニル
(214)4−アニリノフェニル
(215)4−イソブチリルアミノフェニル
(216)4−フェノキシカルボニルアミノフェニル
(217)4−(3−エチルウレイド)フェニル
(218)4−(3,3−ジエチルウレイド)フェニル
(219)4−メチルフェニル
(220)4−フェノキシフェニル
(221)4−ヒドロキシフェニル
【0128】
【化23】
Figure 2004203009
【0129】
(222)フェニル
(223)4−ブチルフェニル
(224)4−(2−メトキシ−2−エトキシエチル)フェニル
(225)4−(5−ノネニル)フェニル
(226)p−ビフェニリル
(227)4−エトキシカルボニルフェニル
(228)4−ブトキシフェニル
(229)4−メチルフェニル
(230)4−クロロフェニル
(231)4−フェニルチオフェニル
(232)4−ベンゾイルフェニル
(233)4−アセトキシフェニル
(234)4−ベンゾイルオキシフェニル
(235)4−フェノキシカルボニルフェニル
(236)4−メトキシフェニル
(237)4−アニリノフェニル
(238)4−イソブチリルアミノフェニル
(239)4−フェノキシカルボニルアミノフェニル
(240)4−(3−エチルウレイド)フェニル
(241)4−(3,3−ジエチルウレイド)フェニル
(242)4−フェノキシフェニル
(243)4−ヒドロキシフェニル
(244)3−ブチルフェニル
(245)3−(2−メトキシ−2−エトキシエチル)フェニル
(246)3−(5−ノネニル)フェニル
(247)m−ビフェニリル
(248)3−エトキシカルボニルフェニル
(249)3−ブトキシフェニル
(250)3−メチルフェニル
(251)3−クロロフェニル
(252)3−フェニルチオフェニル
(253)3−ベンゾイルフェニル
(254)3−アセトキシフェニル
(255)3−ベンゾイルオキシフェニル
(256)3−フェノキシカルボニルフェニル
(257)3−メトキシフェニル
(258)3−アニリノフェニル
(259)3−イソブチリルアミノフェニル
(260)3−フェノキシカルボニルアミノフェニル
(261)3−(3−エチルウレイド)フェニル
(262)3−(3,3−ジエチルウレイド)フェニル
(263)3−フェノキシフェニル
(264)3−ヒドロキシフェニル
(265)2−ブチルフェニル
(266)2−(2−メトキシ−2−エトキシエチル)フェニル
(267)2−(5−ノネニル)フェニル
(268)o−ビフェニリル
(269)2−エトキシカルボニルフェニル
(270)2−ブトキシフェニル
(271)2−メチルフェニル
(272)2−クロロフェニル
(273)2−フェニルチオフェニル
(274)2−ベンゾイルフェニル
(275)2−アセトキシフェニル
(276)2−ベンゾイルオキシフェニル
(277)2−フェノキシカルボニルフェニル
(278)2−メトキシフェニル
(279)2−アニリノフェニル
(280)2−イソブチリルアミノフェニル
(281)2−フェノキシカルボニルアミノフェニル
(282)2−(3−エチルウレイド)フェニル
(283)2−(3,3−ジエチルウレイド)フェニル
(284)2−フェノキシフェニル
(285)2−ヒドロキシフェニル
(286)3,4−ジブチルフェニル
(287)3,4−ジ(2−メトキシ−2−エトキシエチル)フェニル
(288)3,4−ジフェニルフェニル
(289)3,4−ジエトキシカルボニルフェニル
(290)3,4−ジドデシルオキシフェニル
(291)3,4−ジメチルフェニル
(292)3,4−ジクロロフェニル
(293)3,4−ジベンゾイルフェニル
(294)3,4−ジアセトキシフェニル
(295)3,4−ジメトキシフェニル
(296)3,4−ジ−N−メチルアミノフェニル
(297)3,4−ジイソブチリルアミノフェニル
(298)3,4−ジフェノキシフェニル
(299)3,4−ジヒドロキシフェニル
(300)3,5−ジブチルフェニル
(301)3,5−ジ(2−メトキシ−2−エトキシエチル)フェニル
(302)3,5−ジフェニルフェニル
(303)3,5−ジエトキシカルボニルフェニル
(304)3,5−ジドデシルオキシフェニル
(305)3,5−ジメチルフェニル
(306)3,5−ジクロロフェニル
(307)3,5−ジベンゾイルフェニル
(308)3,5−ジアセトキシフェニル
(309)3,5−ジメトキシフェニル
(310)3,5−ジ−N−メチルアミノフェニル
(311)3,5−ジイソブチリルアミノフェニル
(312)3,5−ジフェノキシフェニル
(313)3,5−ジヒドロキシフェニル
(314)2,4−ジブチルフェニル
(315)2,4−ジ(2−メトキシ−2−エトキシエチル)フェニル
(316)2,4−ジフェニルフェニル
(317)2,4−ジエトキシカルボニルフェニル
(318)2,4−ジドデシルオキシフェニル
(319)2,4−ジメチルフェニル
(320)2,4−ジクロロフェニル
(321)2,4−ジベンゾイルフェニル
(322)2,4−ジアセトキシフェニル
(323)2,4−ジメトキシフェニル
(324)2,4−ジ−N−メチルアミノフェニル
(325)2,4−ジイソブチリルアミノフェニル
(326)2,4−ジフェノキシフェニル
(327)2,4−ジヒドロキシフェニル
(328)2,3−ジブチルフェニル
(329)2,3−ジ(2−メトキシ−2−エトキシエチル)フェニル
(330)2,3−ジフェニルフェニル
(331)2,3−ジエトキシカルボニルフェニル
(332)2,3−ジドデシルオキシフェニル
(333)2,3−ジメチルフェニル
(334)2,3−ジクロロフェニル
(335)2,3−ジベンゾイルフェニル
(336)2,3−ジアセトキシフェニル
(337)2,3−ジメトキシフェニル
(338)2,3−ジ−N−メチルアミノフェニル
(339)2,3−ジイソブチリルアミノフェニル
(340)2,3−ジフェノキシフェニル
(341)2,3−ジヒドロキシフェニル
(342)2,6−ジブチルフェニル
(343)2,6−ジ(2−メトキシ−2−エトキシエチル)フェニル
(344)2,6−ジフェニルフェニル
(345)2,6−ジエトキシカルボニルフェニル
(346)2,6−ジドデシルオキシフェニル
(347)2,6−ジメチルフェニル
(348)2,6−ジクロロフェニル
(349)2,6−ジベンゾイルフェニル
(350)2,6−ジアセトキシフェニル
(351)2,6−ジメトキシフェニル
(352)2,6−ジ−N−メチルアミノフェニル
(353)2,6−ジイソブチリルアミノフェニル
(354)2,6−ジフェノキシフェニル
(355)2,6−ジヒドロキシフェニル
(356)3,4,5−トリブチルフェニル
(357)3,4,5−トリ(2−メトキシ−2−エトキシエチル)フェニル
(358)3,4,5−トリフェニルフェニル
(359)3,4,5−トリエトキシカルボニルフェニル
(360)3,4,5−トリドデシルオキシフェニル
(361)3,4,5−トリメチルフェニル
(362)3,4,5−トリクロロフェニル
(363)3,4,5−トリベンゾイルフェニル
(364)3,4,5−トリアセトキシフェニル
(365)3,4,5−トリメトキシフェニル
(366)3,4,5−トリ−N−メチルアミノフェニル
(367)3,4,5−トリイソブチリルアミノフェニル
(368)3,4,5−トリフェノキシフェニル
(369)3,4,5−トリヒドロキシフェニル
(370)2,4,6−トリブチルフェニル
(371)2,4,6−トリ(2−メトキシ−2−エトキシエチル)フェニル
(372)2,4,6−トリフェニルフェニル
(373)2,4,6−トリエトキシカルボニルフェニル
(374)2,4,6−トリドデシルオキシフェニル
(375)2,4,6−トリメチルフェニル
(376)2,4,6−トリクロロフェニル
(377)2,4,6−トリベンゾイルフェニル
(378)2,4,6−トリアセトキシフェニル(379)2,4,6−トリメトキシフェニル
(380)2,4,6−トリ−N−メチルアミノフェニル
(381)2,4,6−トリイソブチリルアミノフェニル
(382)2,4,6−トリフェノキシフェニル(383)2,4,6−トリヒドロキシフェニル
(384)ペンタフルオロフェニル
(385)ペンタクロロフェニル
(386)ペンタメトキシフェニル
(387)6−N−メチルスルファモイル−8−メトキシ−2−ナフチル
(388)5−N−メチルスルファモイル−2−ナフチル
(389)6−N−フェニルスルファモイル−2−ナフチル
(390)5−エトキシ−7−N−メチルスルファモイル−2−ナフチル
(391)3−メトキシ−2−ナフチル
(392)1−エトキシ−2−ナフチル
(393)6−N−フェニルスルファモイル−8−メトキシ−2−ナフチル
(394)5−メトキシ−7−N−フェニルスルファモイル−2−ナフチル
(395)1−(4−メチルフェニル)−2−ナフチル
(396)6,8−ジ−N−メチルスルファモイル−2−ナフチル
(397)6−N−2−アセトキシエチルスルファモイル−8−メトキシ−2−ナフチル
(398)5−アセトキシ−7−N−フェニルスルファモイル−2−ナフチル
(399)3−ベンゾイルオキシ−2−ナフチル
(400)5−アセチルアミノ−1−ナフチル
(401)2−メトキシ−1−ナフチル(402)4−フェノキシ−1−ナフチル
(403)5−N−メチルスルファモイル−1−ナフチル
(404)3−N−メチルカルバモイル−4−ヒドロキシ−1−ナフチル
(405)5−メトキシ−6−N−エチルスルファモイル−1−ナフチル
(406)7−テトラデシルオキシ−1−ナフチル
(407)4−(4−メチルフェノキシ)−1−ナフチル
(408)6−N−メチルスルファモイル−1−ナフチル
(409)3−N,N−ジメチルカルバモイル−4−メトキシ−1−ナフチル
(410)5−メトキシ−6−N−ベンジルスルファモイル−1−ナフチル
(411)3,6−ジ−N−フェニルスルファモイル−1−ナフチル
(412)メチル
(413)エチル
(414)ブチル
(415)オクチル
(416)ドデシル
(417)2−ブトキシ−2−エトキシエチル
(418)ベンジル
(419)4−メトキシベンジル
【0130】
【化24】
Figure 2004203009
【0131】
(424)メチル
(425)フェニル
(426)ブチル
【0132】
【化25】
Figure 2004203009
【0133】
(430)メチル
(431)エチル
(432)ブチル
(433)オクチル
(434)ドデシル
(435)2−ブトキシ2−エトキシエチル
(436)ベンジル
(437)4−メトキシベンジル
【0134】
【化26】
Figure 2004203009
【0135】
【化27】
Figure 2004203009
【0136】
本発明においては、1,3,5−トリアジン環を有する化合物として、メラミンポリマーを用いてもよい。メラミンポリマーは、下記一般式(IV)で示すメラミン化合物とカルボニル化合物との重合反応により合成することが好ましい。
【0137】
【化28】
Figure 2004203009
【0138】
上記合成反応スキームにおいて、R11、R12、R13、R14、R15及びR16は、水素原子、アルキル基、アルケニル基、アリール基又は複素環基である。
【0139】
上記アルキル基、アルケニル基、アリール基及び複素環基及びこれらの置換基は前記一般式(I)で説明した各基、それらの置換基と同義である。
【0140】
メラミン化合物とカルボニル化合物との重合反応は、通常のメラミン樹脂(例えば、メラミンホルムアルデヒド樹脂等)の合成方法と同様である。また、市販のメラミンポリマー(メラミン樹脂)を用いてもよい。
【0141】
メラミンポリマーの分子量は、2千〜40万であることが好ましい。メラミンポリマーの繰り返し単位の具体例を以下に示す。
【0142】
【化29】
Figure 2004203009
【0143】
MP−1:R13、R14、R15、R16:CHOH
MP−2:R13、R14、R15、R16:CHOCH
MP−3:R13、R14、R15、R16:CHO−i−C
MP−4:R13、R14、R15、R16:CHO−n−C
MP−5:R13、R14、R15、R16:CHNHCOCH=CH
MP−6:R13、R14、R15、R16:CHNHCO(CHCH=CH(CHCH
MP−7:R13、R14、R15:CHOH;R16:CHOCH
MP−8:R13、R14、R16:CHOH;R15:CHOCH
MP−9:R13、R14:CHOH;R15、R16:CHOCH
MP−10:R13、R16:CHOH;R14、R15:CHOCH
MP−11:R13:CHOH;R14、R15、R16:CHOCH
MP−12:R13、R14、R16:CHOCH;R15:CHOH
MP−13:R13、R16:CHOCH;R14、R15:CHOH
MP−14:R13、R14、R15:CHOH;R16:CHO−i−C
MP−15:R13、R14、R16:CHOH;R15:CHO−i−C
MP−16:R13、R14:CHOH;R15、R16:CHO−i−C
MP−17:R13、R16:CHOH;R14、R15:CHO−i−C
MP−18:R13:CHOH;R14、R15、R16:CHO−i−C
MP−19:R13、R14、R16:CHO−i−C;R15:CHOH
MP−20:R13、R16:CHO−i−C;R14、R15:CHOH
MP−21:R13、R14、R15:CHOH;R16:CHO−n−C
MP−22:R13、R14、R16:CHOH;R15:CHO−n−C
MP−23:R13、R14:CHOH;R15、R16:CHO−n−C
MP−24:R13、R16:CHOH;R14、R15:CHO−n−C
MP−25:R13:CHOH;R14、R15、R16:CH2O−n−C
MP−26:R13、R14、R16:CHO−n−C;R15:CHOH
MP−27:R13、R16:CHO−n−C;R14、R15:CHOH
MP−28:R13、R14:CHOH;R15:CHOCH;R16:CHO−n−C
MP−29:R13、R14:CHOH;R15:CHO−n−C;R16:CHOCH
MP−30:R13、R16:CHOH;R14:CHOCH;R15:CHO−n−C
MP−31:R13:CHOH;R14、R15:CHOCH;R16:CHO−n−C
MP−32:R13:CHOH;R14、R16:CHOCH;R15:CHO−n−C
MP−33:R13:CHOH;R14:CHOCH;R15、R16:CHO−n−C
MP−34:R13:CHOH;R14、R15:CHO−n−C;R16:CHOCH
MP−35:R13、R14:CHOCH;R15:CHOH;R16:CHO−n−C
MP−36:R13、R16:CHOCH;R14:CHOH;R15:CHO−n−C
MP−37:R13:CHOCH;R14、R15:CHOH;R16:CHO−n−C
MP−38:R13、R16:CHO−n−C;R14:CHOCH;R15:CHOH
MP−39:R13:CHOH;R14:CHOCH;R15:CHO−n−C4H9;R16:CHNHCOCH=CH
MP−40:R13:CHOH;R14:CHOCH;R15:CHNHCOCH=CH;R16:CHO−n−C
MP−41:R13:CHOH;R14:CHO−n−C;R15:CHNHCOCH=CH;R16:CHOCH
MP−42:R13:CHOCH;R14:CHOH;R15:CHO−n−C;R16:CHNHCOCH=CH
MP−43:R13:CHOCH;R14:CHOH;R15:CHNHCOCH=CH;R16:CHO−n−C
MP−44:R13:CHO−n−C;R14:CHOCH;R15:CHOH;R16:CHNHCOCH=CH
MP−45:R13:CHOH;R14:CHOCH;R15:CHNHCO(CHCH=CH(CHCH;R16:CHNHCOCH=CH
MP−46:R13:CHOH;R14:CHOCH;R15:CHNHCOCH=CH;R16:CHNHCO(CHCH=CH(CHCH
MP−47:R13:CHOH;R14:CHNHCO(CHCH=CH(CHCH;R15:CHNHCOCH=CH;R16:CHOCH
MP−48:R13:CHOCH;R14:CHOH;R15:CHNHCO(CHCH=CH(CHCH;R16:CHNHCOCH=CH
MP−49:R13:CHOCH;R14:CHOH;R15:CHNHCOCH=CH;R16:CHNHCO(CHCH=CH(CHCH
MP−50:R13:CHNHCO(CHCH=CH(CHCH;R14:CHOCH;R15:CHOH;R16:CHNHCOCH=CH
【0144】
【化30】
Figure 2004203009
【0145】
MP−51:R13、R14、R15、R16:CHOH
MP−52:R13、R14、R15、R16:CHOCH
MP−53:R13、R14、R15、R16:CHO−i−C
MP−54:R13、R14、R15、R16:CHO−n−C
MP−55:R13、R14、R15、R16:CHNHCOCH=CH
MP−56:R13、R14、R15、R16:CHNHCO(CHCH=CH(CHCH
MP−57:R13、R14、R15:CHOH;R16:CHOCH
MP−58:R13、R14、R16:CHOH;R15:CHOCH
MP−59:R13、R14:CHOH;R15、R16:CHOCH
MP−60:R13、R16:CHOH;R14、R15:CHOCH
MP−61:R13:CHOH;R14、R15、R16:CHOCH
MP−62:R13、R14、R16:CHOCH;R15:CHOH
MP−63:R13、R16:CHOCH;R14、R15:CHOH
MP−64:R13、R14、R15:CHOH;R16:CHO−i−C
MP−65:R13、R14、R16:CHOH;R15:CHO−i−C
MP−66:R13、R14:CHOH;R15、R16:CHO−i−C
MP−67:R13、R16:CHOH;R14、R15:CHO−i−C
MP−68:R13:CHOH;R14、R15、R16:CHO−i−C
MP−69:R13、R14、R16:CHO−i−C;R15:CHOH
MP−70:R13、R16:CHO−i−C;R14、R15:CHOH
MP−71:R13、R14、R15:CHOH;R16:CHO−n−C
MP−72:R13、R14、R16:CHOH;R15:CHO−n−C
MP−73:R13、R14:CHOH;R15、R16:CHO−n−C
MP−74:R13、R16:CHOH;R14、R15:CHO−n−C
MP−75:R13:CHOH;R14、R15、R16:CHO−n−C
MP−76:R13、R14、R16:CHO−n−C;R15:CHOH
MP−77:R13、R16:CHO−n−C;R14、R15:CHOH
MP−78:R13、R14:CHOH;R15:CHOCH;R16:CHO−n−C
MP−79:R13、R14:CHOH;R15:CHO−n−C;R16:CHOCH
MP−80:R13、R16:CHOH;R14:CHOCH;R15:CHO−n−C
MP−81:R13:CHOH;R14、R15:CHOCH;R16:CHO−n−C
MP−82:R13:CHOH;R14、R16:CHOCH;R15:CHO−n−C
MP−83:R13:CHOH;R14:CHOCH;R15、R16:CHO−n−C
MP−84:R13:CHOH;R14、R15:CHO−n−C;R16:CHOCH
MP−85:R13、R14:CHOCH;R15:CHOH;R16:CHO−n−C
MP−86:R13、R16:CHOCH;R14:CHOH;R15:CHO−n−C
MP−87:R13:CHOCH;R14、R15:CHOH;R16:CHO−n−C
MP−88:R13、R16:CHO−n−C;R14:CHOCH;R15:CHOH
MP−89:R13:CHOH;R14:CHOCH;R15:CHO−n−C;R16:CHNHCOCH=CH
MP−90:R13:CHOH;R14:CHOCH;R15:CHNHCOCH=CH;R16:CHO−n−C
MP−91:R13:CHOH;R14:CHO−n−C;R15:CHNHCOCH=CH;R16:CHOCH
MP−92:R13:CHOCH;R14:CHOH;R15:CHO−n−C;R16:CHNHCOCH=CH
MP−93:R13:CHOCH;R14:CHOH;R15:CHNHCOCH=CH;R16:CHO−n−C
MP−94:R13:CHO−n−C;R14:CHOCH;R15:CHOH;R16:CHNHCOCH=CH
MP−95:R13:CHOH;R14:CHOCH;R15:CHNHCO(CHCH=CH(CHCH;R16:CHNHCOCH=CH
MP−96:R13:CHOH;R14:CHOCH;R15:CHNHCOCH=CH;R16:CHNHCO(CHCH=CH(CHCH
MP−97:R13:CHOH;R14:CHNHCO(CHCH=CH(CHCH;R15:CHNHCOCH=CH;R16:CHOCH
MP−98:R13:CHOCH;R14:CHOH;R15:CHNHCO(CHCH=CH(CHCH;R16:CHNHCOCH=CH
MP−99:R13:CHOCH;R14:CHOH;R15:CHNHCOCH=CH;R16:CHNHCO(CHCH=CH(CHCH
MP−100:R13:CHNHCO(CHCH=CH(CHCH;R14:CHOCH;R15:CHOH;R16:CHNHCOCH=CH
【0146】
【化31】
Figure 2004203009
【0147】
MP−101:R13、R14、R15、R16:CHOH
MP−102:R13、R14、R15、R16:CHOCH
MP−103:R13、R14、R15、R16:CHO−i−C
MP−104:R13、R14、R15、R16:CHO−n−C
MP−105:R13、R14、R15、R16:CHNHCOCH=CH
MP−106:R13、R14、R15、R16:CHNHCO(CHCH=CH(CHCH
MP−107:R13、R14、R15:CHOH;R16:CHOCH
MP−108:R13、R14、R16:CHOH;R15:CHOCH
MP−109:R13、R14:CHOH;R15、R16:CHOCH
MP−110:R13、R16:CHOH;R14、R15:CHOCH
MP−111:R13:CHOH;R14、R15、R16:CHOCH
MP−112:R13、R14、R16:CHOCH;R15:CHOH
MP−113:R13、R16:CHOCH;R14、R15:CHOH
MP−114:R13、R14、R15:CHOH;R16:CHO−i−C
MP−115:R13、R14、R16:CHOH;R15:CHO−i−C
MP−116:R13、R14:CHOH;R15、R16:CHO−i−C
MP−117:R13、R16:CHOH;R14、R15:CHO−i−C
MP−118:R13:CHOH;R14、R15、R16:CHO−i−C
MP−119:R13、R14、R16:CHO−i−C;R15:CHOH
MP−120:R13、R16:CHO−i−C;R14、R15:CHOH
MP−121:R13、R14、R15:CHOH;R16:CHO−n−C
MP−122:R13、R14、R16:CHOH;R15:CHO−n−C
MP−123:R13、R14:CHOH;R15、R16:CHO−n−C
MP−124:R13、R16:CHOH;R14、R15:CHO−n−C
MP−125:R13:CHOH;R14、R15、R16:CHO−n−C
MP−126:R13、R14、R16:CHO−n−C;R15:CHOH
MP−127:R13、R16:CHO−n−C;R14、R15:CHOH
MP−128:R13、R14:CHOH;R15:CHOCH;R16:CHO−n−C
MP−129:R13、R14:CHOH;R15:CHO−n−C;R16:CHOCH
MP−130:R13、R16:CHOH;R14:CHOCH;R15:CHO−n−C
MP−131:R13:CHOH;R14、R15:CHOCH;R16:CHO−n−C
MP−132:R13:CHOH;R14、R16:CHOCH;R15:CHO−n−C
MP−133:R13:CHOH;R14:CHOCH;R15、R16:CHO−n−C
MP−134:R13:CHOH;R14、R15:CHO−n−C;R16:CHOCH
MP−135:R13、R14:CHOCH;R15:CHOH;R16:CHO−n−C
MP−136:R13、R16:CHOCH;R14:CHOH;R15:CHO−n−C
MP−137:R13:CHOCH;R14、R15:CHOH;R16:CHO−n−C
MP−138:R13、R16:CHO−n−C;R14:CHOCH;R15:CHOH
MP−139:R13:CHOH;R14:CHOCH;R15:CHO−n−C;R16:CHNHCOCH=CH
MP−140:R13:CHOH;R14:CHOCH;R15:CHNHCOCH=CH;R16:CHO−n−C
MP−141:R13:CHOH;R14:CHO−n−C;R15:CHNHCOCH=CH;R16:CHOCH
MP−142:R13:CHOCH;R14:CHOH;R15:CHO−n−C;R16:CHNHCOCH=CH
MP−143:R13:CHOCH;R14:CHOH;R15:CHNHCOCH=CH;R16:CHO−n−C
MP−144:R13:CHO−n−C;R14:CHOCH;R15:CHOH;R16:CHNHCOCH=CH
MP−145:R13:CHOH;R14:CHOCH;R15:CHNHCO(CHCH=CH(CHCH;R16:CHNHCOCH=CH
MP−146:R13:CHOH;R14:CHOCH;R15:CHNHCOCH=CH;R16:CHNHCO(CHCH=CH(CHCH
MP−147:R13:CHOH;R14:CHNHCO(CHCH=CH(CHCH;R15:CHNHCOCH=CH;R16:CHOCH
MP−148:R13:CHOCH;R14:CHOH;R15:CHNHCO(CHCH=CH(CHCH;R16:CHNHCOCH=CH
MP−149:R13:CHOCH;R14:CHOH;R15:CHNHCOCH=CH;R16:CHNHCO(CHCH=CH(CHCH
MP−150:R13:CHNHCO(CHCH=CH(CHCH;R14:CHOCH;R15:CHOH;R16:CHNHCOCH=CH
【0148】
【化32】
Figure 2004203009
【0149】
MP−151:R13、R14、R15、R16:CHOH
MP−152:R13、R14、R15、R16:CHOCH
MP−153:R13、R14、R15、R16:CHO−i−C
MP−154:R13、R14、R15、R16:CHO−n−C
MP−155:R13、R14、R15、R16:CHNHCOCH=CH
MP−156:R13、R14、R15、R16:CHNHCO(CHCH=CH(CHCH
MP−157:R13、R14、R15:CHOH;R16:CHOCH
MP−158:R13、R14、R16:CHOH;R15:CHOCH
MP−159:R13、R14:CHOH;R15、R16:CHOCH
MP−160:R13、R16:CHOH;R14、R15:CHOCH
MP−161:R13:CHOH;R14、R15、R16:CHOCH
MP−162:R13、R14、R16:CHOCH;R15:CHOH
MP−163:R13、R16:CHOCH;R14、R15:CHOH
MP−164:R13、R14、R15:CHOH;R16:CHO−i−C
MP−165:R13、R14、R16:CHOH;R15:CHO−i−C
MP−166:R13、R14:CHOH;R15、R16:CHO−i−C
MP−167:R13、R16:CHOH;R14、R15:CHO−i−C
MP−168:R13:CHOH;R14、R15、R16:CHO−i−C
MP−169:R13、R14、R16:CHO−i−C;R15:CHOH
MP−170:R13、R16:CHO−i−C;R14、R15:CHOH
MP−171:R13、R14、R15:CHOH;R16:CHO−n−C
MP−172:R13、R14、R16:CHOH;R15:CHO−n−C
MP−173:R13、R14:CHOH;R15、R16:CHO−n−C
MP−174:R13、R16:CHOH;R14、R15:CHO−n−C
MP−175:R13:CHOH;R14、R15、R16:CHO−n−C
MP−176:R13、R14、R16:CHO−n−C;R15:CHOH
MP−177:R13、R16:CHO−n−C;R14、R15:CHOH
MP−178:R13、R14:CHOH;R15:CHOCH;R16:CHO−n−C
MP−179:R13、R14:CHOH;R15:CHO−n−C;R16:CHOCH
MP−180:R13、R16:CHOH;R14:CHOCH;R15:CHO−n−C
MP−181:R13:CHOH;R14、R15:CHOCH;R16:CHO−n−C
MP−182:R13:CHOH;R14、R16:CHOCH;R15:CHO−n−C
MP−183:R13:CHOH;R14:CHOCH;R15、R16:CHO−n−C
MP−184:R13:CHOH;R14、R15:CHO−n−C;R16:CHOCH
MP−185:R13、R14:CHOCH;R15:CHOH;R16:CH2O−n−C
MP−186:R13、R16:CHOCH;R14:CHOH;R15:CHO−n−C
MP−187:R13:CHOCH;R14、R15:CHOH;R16:CHO−n−C
MP−188:R13、R16:CHO−n−C;R14:CHOCH;R :CHOH
MP−189:R13:CHOH;R14:CHOCH;R15:CHO−n−C;R16:CHNHCOCH=CH
MP−190:R13:CHOH;R14:CHOCH;R15:CHNHCOCH=CH;R16:CHO−n−C
MP−191:R13:CHOH;R14:CHO−n−C;R15:CHNHCOCH=CH;R16:CHOCH
MP−192:R13:CHOCH;R14:CHOH;R15:CHO−n−C;R16:CHNHCOCH=CH
MP−193:R13:CHOCH;R14:CHOH;R15:CHNHCOCH=CH;R16:CHO−n−C
MP−194:R13:CHO−n−C;R14:CHOCH;R15:CHOH;R16:CHNHCOCH=CH
MP−195:R13:CHOH;R14:CHOCH;R15:CHNHCO(CHCH=CH(CHCH;R16:CHNHCOCH=CH
MP−196:R13:CHOH;R14:CHOCH;R15:CHNHCOCH=CH;R16:CHNHCO(CHCH=CH(CHCH
MP−197:R13:CHOH;R14:CHNHCO(CHCH=CH(CHCH;R15:CHNHCOCH=CH;R16:CHOCH
MP−198:R13:CHOCH;R14:CHOH;R15:CHNHCO(CHCH=CH(CHCH;R16:CHNHCOCH=CH
MP−199:R13:CHOCH;R14:CHOH;R15:CHNHCOCH=CH;R16:CHNHCO(CHCH=CH(CHCH
MP−200:R13:CHNHCO(CHCH=CH(CHCH;R14:CHOCH;R15:CHOH;R16:CHNHCOCH=CH
本発明においては、上記繰り返し単位を二種類以上組み合わせたコポリマーを用いてもよい。二種類以上のホモポリマー又はコポリマーを併用してもよい。
【0150】
また、二種類以上の1,3,5−トリアジン環を有する化合物を併用してもよい。二種類以上の円盤状化合物(例えば、1,3,5−トリアジン環を有する化合物とポルフィリン骨格を有する化合物と)を併用してもよい。
【0151】
また、下記に本発明の上記以外の添加剤の具体例を挙げる。
【0152】
【化33】
Figure 2004203009
【0153】
【化34】
Figure 2004203009
【0154】
【化35】
Figure 2004203009
【0155】
【化36】
Figure 2004203009
【0156】
【化37】
Figure 2004203009
【0157】
【化38】
Figure 2004203009
【0158】
【化39】
Figure 2004203009
【0159】
ドープ中には、上記以外の添加剤、酸化防止剤、染料、蛍光増白剤(例えば特願2002−123821に記載されているもの)等も添加することができる。
【0160】
▲2▼−1インライン添加液(主に、紫外線吸収剤を含有する)調製工程
紫外線吸収剤を含有するインライン添加液として説明する。セルロースエステル溶液に使用する低級アルコール等の有機溶媒、後述の樹脂及び必要に応じ含有する紫外線吸収剤含有インライン添加液の調製方法は、十分に液中に均一に調製することが出来る方法であれば特に制限ないが、次の方法が好ましい。
【0161】
溶解釜111中に有機溶媒と紫外線吸収剤と必要に応じ後述の樹脂を加え、攪拌溶解して樹脂溶液とする。それを送液ポンプ112で濾過器113に送って凝集物を除きインライン添加液110とする(何回か同様な操作を繰り返し循環させてもよい)。そしてインライン添加液を切り替え弁119からストックタンク114に移送し、静置脱泡後、送液ポンプ115(例えば加圧型定量ギヤポンプ)で移送し、濾過器116で濾過して導管117で移送する。
【0162】
使用する有機溶媒は、ドープに使用する有機溶媒を用いることが好ましいが、特に限定はない。ドープに使用する低級アルコール類としては、メチルアルコール、エチルアルコール、プロピルアルコール、イソプロピルアルコール、ブチルアルコール等を挙げることが出来るが、特にエタノールが好ましい。
【0163】
必要に応じて紫外線吸収剤添加液にはセルロースエステルと相溶性の良い樹脂を添加することができる。セルロースエステルと相溶性の良い樹脂としては、ドープに使用するセルロースエステルでもよいが、特願2001−198450に記載の樹脂が、分散液濾過の際、目詰まりにくいので好ましく用いることが出来る。例えば、綜研化学(株)で市販しているアクトフロー・シリーズの樹脂等を好ましく用いることが出来る。
【0164】
インライン添加液は、最終濾過器116で濾過後は、ストックタンクなどに停滞させることなく、また送液ポンプを介すことなく導管で移送するのが好ましく、一方、導管で移送されて来る前記セルロースエステル溶液100と、合流管120で合流される。それにより両液の停滞や、送液ポンプによる新たな凝集物の発生がなく好ましい。これらの濾過はインラインミキサーの直前に配置されており、例えば濾材交換等に伴い経路から発生する大きな凝集物を送液中の微粒子分散液から、一度の濾過で、比較的大きな異物を確実に除去するための濾材で、前記の絶対濾過精度を有する長期に亘り使用が可能な耐有機溶媒性を有する金属製の濾過器が好ましい。濾材としては、耐久性の観点から金属、特にステンレス鋼が好ましい。目詰まりの観点から60〜80%の空孔率を有していることが好ましい。従って、最も好ましくは、絶対濾過精度30〜60μmであって、かつ空孔率60〜80%の金属製濾材で濾過することであり、これにより、長期に亘り、確実に粗大な異物を除くことが出来好ましい。絶対濾過精度30〜60μmでかつ空孔率60〜80%の金属製濾材としては、例えば、日本精線(株)製ファインポアNFシリーズのNF−10、同NF−12、同NF−13などを挙げることが出来、何れも好ましく用いられる。
【0165】
▲2▼−2インライン添加液(主に、微粒子分散液を含有する)調製工程
微粒子分散液を含有するインライン添加液として説明する。セルロースエステル溶液に使用する低級アルコール等の有機溶媒、後述の樹脂及び後述のマット剤微粒子を含有する微粒子剤分散液の調製方法は、十分に液中に均一に分散することが出来る方法であれば特に制限ないが、次の方法が好ましい。
【0166】
溶解釜111A中に有機溶媒と後述の樹脂を加え、攪拌溶解して樹脂溶液とし、この樹脂溶液にマット剤微粒子または微粒子分散液を加えて、マントンゴーリーン、サンドミル等の分散機(図示していない)で分散し、それを送液ポンプ112Aで濾過器113Aに送って凝集物を除きインライン添加液110Aとする(何回か同様な操作を繰り返し循環させてもよい)。そしてインライン添加液を切り替え弁119Aからストックタンク114Aに移送し、静置脱泡後、送液ポンプ115A(例えば加圧型定量ギヤポンプ)で移送し、濾過器116Aで濾過して導管117Aで移送する。なお、予め溶解釜111A内で紫外線吸収剤をインライン添加液に添加してもよい。
【0167】
本発明に係る微粒子の分散液を調製する方法としては、例えば以下に示すような3種類を挙げることが出来る。
【0168】
(調製方法A)
有機溶媒と微粒子を攪拌混合した後、分散機で分散を行う。これを微粒子の分散液とする。
【0169】
(調製方法B)
有機溶媒と微粒子を攪拌混合した後、分散機で分散を行い、微粒子の分散液とする。別に有機溶媒に少量の樹脂(微粒子に対して分散性がよく、液に適度に粘性を与えるもので、且つセルロースエステルと相溶性のある樹脂、またはセルロースエステル)を加え、攪拌溶解した樹脂溶液を用意する。これに前記微粒子分散液を加えて攪拌し、充分分散し、微粒子の分散液とする。
【0170】
(調製方法C)
有機溶媒に少量の樹脂(微粒子に対して分散性がよく、且つセルロースエステルと相溶性のある樹脂、またはセルロースエステル)を加え、攪拌溶解する。これに微粒子を加えて分散機で充分に分散をし、微粒子の分散液とする。
【0171】
調製方法Aは二酸化珪素微粒子の分散性に優れ、調製方法Cは二酸化珪素微粒子が再凝集しにくい点に優れている。調製方法Bは二酸化珪素微粒子の分散性と、二酸化珪素微粒子が再凝集しにくい等、両方に優れている好ましい調製方法である。
【0172】
調製方法A〜Cで分散調製した微粒子の分散液を含有するインライン添加液をセルロースエステル溶液に加えて攪拌しドープとするが、インライン添加液とセルロースエステル溶液をインライン中で合流させ、インラインミキサーで十分混合してドープとするのが好ましい。
【0173】
上記調製方法において、二酸化珪素微粒子を有機溶媒と混合して分散するときの二酸化珪素の濃度は5〜30質量%が好ましく、10〜25質量%がより好ましく、15〜20質量%が更に好ましい。分散濃度は高い方が、添加量に対する液濁度は低くなる傾向があり、得られるフィルムのヘイズが低く、凝集物がなく好ましい。
【0174】
使用する有機溶媒は、ドープに使用する有機溶媒を用いることが好ましいが、特に限定はない。ドープに使用する低級アルコール類としては、メチルアルコール、エチルアルコール、プロピルアルコール、イソプロピルアルコール、ブチルアルコール等を挙げることが出来るが、特にエタノールが好ましい。
【0175】
微粒子の分散性を助け、分散性を良好にし、且つセルロースエステルと相溶性の良い樹脂としては、ドープに使用するセルロースエステルでもよいが、特願2001−198450に記載の樹脂が、分散液濾過の際、目詰まりにくいので好ましく用いることが出来る。例えば、綜研化学(株)で市販しているアクトフロー・シリーズの樹脂等を好ましく用いることが出来る。
【0176】
(分散装置)
上記微粒子を分散する分散機は通常の分散機が使用出来る。分散機は大きく分けてメディア分散機とメディアレス分散機に分けられる。二酸化珪素微粒子の分散にはメディアレス分散機がヘイズが低く好ましい。メディア分散機としてはボールミル、サンドミル、ダイノミルなどがあげられる。メディアレス分散機としては超音波型、遠心型、高圧型などがあるが、本発明においては高圧分散装置が好ましい。高圧分散装置は、微粒子と溶媒を混合した組成物を、細管中に高速通過させることで、高剪断や高圧状態など特殊な条件を作り出す装置である。
【0177】
高圧分散装置で処理する場合、例えば、管径1〜2000μmの細管中で装置内部の最大圧力条件が10MPa以上であることが好ましい。更に好ましくは20MPa以上である。またその際、最高到達速度が100m/秒以上に達するもの、伝熱速度が420kJ/時間以上に達するものが好ましい。上記のような高圧分散装置にはMicrofluidics Corporation社製超高圧ホモジナイザ(商品名マイクロフルイダイザ)あるいはナノマイザ社製ナノマイザがあり、他にもマントンゴーリン型高圧分散装置、例えばイズミフードマシナリ製ホモジナイザ、三和機械(株)社製UHN−01等を挙げることが出来る。
【0178】
インライン添加液は、最終濾過器116Aで濾過後は、ストックタンクなどに停滞させることなく、また送液ポンプを介すことなく導管で移送するのが好ましく、一方、導管で移送されて来る前記セルロースエステル溶液100Aと、合流管120Aで合流され混合器121で混合されながらダイへ供給される。それにより両液の停滞や、送液ポンプによる新たな凝集物の発生がなく好ましい。これらの濾過はインラインミキサーの直前に配置されており、例えば濾材交換等に伴い経路から発生する大きな凝集物を送液中の微粒子分散液から、一度の濾過で、比較的大きな異物を確実に除去するための濾材で、前記の絶対濾過精度を有する長期に亘り使用が可能な耐有機溶媒性を有する金属製の濾過器が好ましい。濾材としては、耐久性の観点から金属、特にステンレス鋼が好ましい。目詰まりの観点から60〜80%の空孔率を有していることが好ましい。従って、最も好ましくは、絶対濾過精度30〜60μmであって、かつ空孔率60〜80%の金属製濾材で濾過することであり、これにより、長期に亘り、確実に粗大な異物を除くことが出来好ましい。絶対濾過精度30〜60μmでかつ空孔率60〜80%の金属製濾材としては、例えば、日本精線(株)製ファインポアNFシリーズのNF−10、同NF−12、同NF−13などを挙げることが出来、何れも好ましく用いられる。
【0179】
《セルロースエステルフィルム及び下側のハードコート層としての活性線硬化樹脂層に中に用いる添加剤》
本発明に用いられるセルロースエステルフィルムの添加剤について説明する。
【0180】
(可塑剤)
可塑剤としては特に限定はないが、リン酸エステル系可塑剤、フタル酸エステル系可塑剤、トリメリット酸エステル系可塑剤、ピロメリット酸系可塑剤、グリコレート系可塑剤、クエン酸エステル系可塑剤、ポリエステル系可塑剤などを挙げることができる。
【0181】
リン酸エステル系としては、
例えば、トリフェニルホスフェート、トリクレジルホスフェート、クレジルジフェニルホスフェート、オクチルジフェニルホスフェート、ジフェニルビフェニルホスフェート、トリオクチルホスフェート、トリブチルホスフェート等;
フタル酸エステル系としては、
例えば、ジエチルフタレート、ジメトキシエチルフタレート、ジメチルフタレート、ジオクチルフタレート、ジブチルフタレート、ジ−2−エチルヘキシルフタレート、ブチルベンジルフタレート、ジシクロヘキシルフタレート、ジベンジルフタレート等;
トリメリット酸系可塑剤としては、例えば、トリブチルトリメリテート、トリフェニルトリメリテート、トリエチルトリメリテート等;
ピロメリット酸エステル系可塑剤としては、
例えば、テトラブチルピロメリテート、テトラフェニルピロメリテート、テトラエチルピロメリテート等;
グリセリンエステルとしては、
例えば、トリアセチン、トリブチリン等;
グリコール酸エステル系としては、エチルフタリルエチルグリコレート、メチルフタリルエチルグリコレート、ブチルフタリルブチルグリコレート等;
その他のカルボン酸エステルの例としては、オレイン酸ブチル、リシノール酸メチルアセチル、セバシン酸ジブチル、種々のトリメリット酸エステル、トリメチロールプロパントリベンゾエート、トリメチロールプロパンテトラベンゾエート等の多価アルコールエステルを挙げることができる。これらのうち、リン酸エステル系可塑剤またはグリコール酸エステル系の可塑剤が好ましい。
【0182】
これらの可塑剤を単独あるいは併用するのが好ましい。
また、可塑剤の使用量は、フィルム性能、加工性等の点で、セルロースエステルに対して1質量%〜30質量%であることが好ましい。
【0183】
また、インラインの添加剤は前述の化2〜化39及び紫外線吸収剤の中から選ぶことができる。
【0184】
▲3▼ドープ調製工程:
セルロースエステル溶液100及びインライン添加液110それぞれを送液ポンプ105及び115により移送し濾過器106及び116で濾過した導管108及び117中を移送し合流管120で両液を合流させる。合流した両液は導管内を層状で移送するためそのままでは混合しにくい。そこで、本発明においては、両液を合流後、インラインミキサーのような混合機121で十分に混合しながら次工程▲4▼に移送する。本発明で使用出来るインラインミキサーとしては、例えば、スタチックミキサーSWJ(東レ静止型管内混合器 Hi−Mixer、東レエンジニアリング製)が好ましい。インラインミキサーを用いる場合、セルロースエステルを高圧下で濃縮溶解したドープに適用することも出来る。
【0185】
上記ドープ調製工程は、微粒子を含有するドープを調製するもので、微粒子を含有する層、例えば共流延ダイの表層用スリットに導入するものである。当然のことながら、微粒子を含有しない層のドープは、上記微粒子の分散液を含むインライン添加液調製工程は使用しいが、微粒子に代えて紫外線吸収剤をインライン添加してもよい。セルロースエステルの種類、濃度、微粒子の有無、微粒子の濃度、有機化合物添加剤の有無、有機化合物の濃度等、このようなドープ調製工程を多層の数だけ(ドープ組成が同じ場合は共用することが出来る)設ける必要がある。後述の共流延ダイには、それぞれの目的に応じて成分を変更し調製したドープを各スリットに供給することになる。基層に用いられるドープの粘度は50〜10,000Pa・s(35℃にて)であることが好ましく、特に50〜1,000Pa・sであることが好ましい。表層に用いられるドープの粘度は0.1〜5,000Pa・sであることが好ましく、5〜1,000Pa・sであることがより好ましく、更に好ましくは10〜500Pa・s、特に好ましくは10〜50Pa・sである。本発明において、表層用ドープの粘度は基層用のそれより低いことが好ましい。
【0186】
図5で説明したドープ調製工程150を調製工程Aとし、例えば調製工程Aで調製されたドープが基層用のドープとすると、該ドープを共流延ダイ200の基層の導入口202に導入し、調製工程Bと図示していない同様な調製工程Cからのそれぞれのドープを、共流延ダイ200の表層ドープ導入口201と203にそれぞれ導入して共流延に供する。ドープ調製工程B及びCはドープ調製工程Aとと同様であってもよく、表層用ドープCの組成が同じであれば一つのドープ調製工程から分割して送液してもよい。
【0187】
図6は本発明に係わる溶液流延製膜装置の流延以降の工程を示した図である。以下、本発明に係わるセルロースエステルフィルムの作製の一例を図6を用いて説明する。
【0188】
▲4▼共流延工程:
上記したように、ドープ調製工程B、A及びCで調製したドープを、それぞれのインラインミキサーで混合調製し、各ドープを共流延ダイ200にそれぞれ導入口201、202及び203を通して導入し、無限に移送する無端の金属支持体204、例えばステンレスベルト、あるいは回転する金属ドラム等の金属支持体204上の流延位置に、共流延ダイ200から例えば3層のドープを共流延する工程である。金属支持体204の表面は鏡面となっていることが望ましい。共流延ダイ200(例えば加圧型共流延ダイ)は口金部分の三つのスリット形状を調製出来、膜厚を均一にし易いため好ましい。共流延ダイ200には、コートハンガーダイやTダイ等があるが、何れも好ましく用いられる。逐次流延の場合には、金属支持体204上に2基以上設け、2種類以上のドープ量を供給して多層ドープ膜を形成する。
【0189】
▲5▼溶媒蒸発工程:
例えば3層構成のウェブ(金属支持体上にドープを流延した以降のドープ膜の呼び方をウェブとする)206を金属支持体204上で加熱あるいは冷却して金属支持体204からウェブ206が剥離可能になるまで溶媒を蒸発させる工程である。溶媒を蒸発させるには、ウェブ206に風を当てる方法及び/または金属支持体204の裏面から液体または気体により伝熱させる方法、輻射熱により表裏から伝熱する方法等があるが、裏面液体伝熱の方法が乾燥効率がよく好ましい。またそれらを組み合わせる方法も好ましい。裏面液体伝熱の場合は、金属支持体上のウェブ温度がドープで使用されている有機溶媒の主溶媒または最も低い沸点を有する有機溶媒の沸点以下で加熱するのが好ましい。流延用の金属支持体の表面温度は10〜55℃、溶液の温度は25〜60℃、更に溶液の温度を支持体の温度と同じまたはそれ以上の温度にすることが好ましく、5℃以上の温度に設定することが更に好ましい。溶液温度、支持体温度は、高いほど溶媒の乾燥速度が速く出来るので好ましいが、あまり高すぎると発泡したり、平面性が劣化する場合がある。支持体の温度の更に好ましい範囲は、使用する有機溶媒に依存するが、20〜55℃、溶液温度の更に好ましい範囲は、35〜45℃である。
【0190】
▲6▼剥離工程:
金属支持体204上で溶媒が蒸発したウェブ206を、剥離位置205で剥離する工程である。剥離されたウェブ206は次工程▲7▼に送られる。剥離する時点でのウェブ206の残留溶媒量(後述の式)があまり大き過ぎると剥離し難かったり、逆に金属支持体204上で乾燥させ過ぎて剥離すると、剥離しにくくなったり、途中でウェブ206の一部が剥がれたりする。本発明において、薄手のウェブを金属支持体から剥離する際、平面性の劣化やつれがないように行うには、剥離張力として剥離出来る最低張力から170N/m以内の力で剥離することが好ましく、140N/m以内の力がより好ましい。
【0191】
製膜速度を上げる方法(残留溶媒量が出来るだけ多いうちに剥離するため製膜速度を上げることが出来る)としてゲル流延法(ゲルキャスティング)がある。それは、ドープ中にセルロースエステルに対する貧溶媒を加えて、ドープ流延後、ゲル化する方法、金属支持体の温度を低めてゲル化する方法等がある。金属支持体204上でゲル化させ剥離時の膜の強度を上げておくことによって、剥離を早め製膜速度を上げることが出来るのである。金属支持体204上でのウェブ206の乾燥が条件の強弱、金属支持体204の長さ等により5〜150質量%の範囲で剥離することが出来るが、残留溶媒量がより多い時点で剥離する場合、ウェブ206が柔らか過ぎると剥離時平面性を損なったり、剥離張力によるツレや縦スジが発生し易く、経済速度と品質との兼ね合いで剥離残留溶媒量を決められる。従って、本発明においては、該金属支持体204上の剥離位置における温度を好ましくは10〜40℃、更に好ましくは12〜30℃とし、且つ該剥離位置におけるウェブ206の残留溶媒量を10〜120質量%とすることが好ましい。
【0192】
製造時のセルロースエステルフィルムが良好な平面性を維持するために、金属支持体から剥離する際の残留溶媒量を10〜150質量%とすることが好ましく、より好ましくは80〜150質量%であり、更に好ましくは100〜130質量%である。剥離時のウェブの残留有機溶媒中に含まれる良溶媒の比率は30〜90%が好ましく、更に好ましくは、50〜85%であり、特に好ましくは、60〜80%である。
【0193】
本発明においては、残留溶媒量は下記の式で表わすことが出来る。
残留溶媒量(質量%)={(M−N)/N}×100
ここで、Mはウェブの任意時点での質量で、この乾燥によって揮発した成分の比率についてはガスクロマトグラフィーによって求めることが出来る。Nは該Mを110℃で3時間乾燥させた時の質量である。測定はヘッドスペースサンプラーを接続したガスクロマトグラフィーで測定する。本発明では、ヒューレット・パッカード社製ガスクロマトグラフィー5890型SERISIIとヘッドスペースサンプラーHP7694型を使用し、以下の測定条件で行った。
【0194】
ヘッドスペースサンプラー加熱条件:120℃、20分
GC導入温度:150℃
昇温:40℃、5分保持→100℃(8℃/分)
カラム:J&W社製DB−WAX(内径0.32mm、長さ30m)。
【0195】
本発明において、ドープの流延から剥離までのウェブの金属支持体上での乾燥時間は120秒以内であることが好ましく、更に30〜120秒が好ましく、更に30〜90秒であることが好ましい。この範囲で剥離したウェブの表面性は良好で、乾燥後のセルロースエステルフィルムに後述の金属化合物薄膜を施した際、平面性に優れ、且つ高温高湿条件下に繰り返し曝した際のクラックもなく優れた光学フィルムを得ることが出来る。
【0196】
▲7▼乾燥工程:
剥離後、一般には、ウェブ206をジグザグに配置したロール209に交互に通して搬送するロール乾燥装置208及び/またはクリップでウェブ206の両端をクリップして搬送するテンター装置207を用いてウェブ206を乾燥する。図6では、テンター装置207の後にロール乾燥装置208が配置されている。乾燥の手段はウェブの両面に熱風を吹かせるのが一般的であるが、風の代わりにマイクロウエーブを当てて加熱する手段もある。あまり急激な乾燥は出来上がりのフィルムの平面性を損ね易い。全体を通して、通常乾燥温度は40〜250℃の範囲で行われ、好ましくは110〜160℃で乾燥させることである。使用する溶媒によって、乾燥温度、乾燥風量及び乾燥時間が異なり、使用溶媒の種類、組合せに応じて乾燥条件を適宜選べばよい。210は出来上がったセルロースエステルフィルムの巻き取りである。セルロースエステルフィルムの乾燥工程において、残留溶媒量を1質量%以下にすることが好ましく、0.1質量%以下にして巻き取ることがより好ましい。
【0197】
以上の基材シートFは基層22と両側の表層21,23としたが、基層22だけの場合や基層22と何れかの表層にすることも製作は可能であり、何れも基材シートとしての効果を奏するる。このような基材シートを用いて作成した本発明の光学フィルムの模式的な断面図を図7の(a)、(b)、(c)に示す。
【0198】
《ハードコート層》
本発明に用いられ、基材シートの上に塗設されるハードコート層(活性線硬化樹脂層)について説明する。
【0199】
本発明の光学フィルムはセルロースエステルフィルム上に直接または他の層を介して金属化合物層を形成することを特徴としているが、図7の(a)、(b)、(c)に示すように、ハードコート層(活性線硬化樹脂層)あるいは他の層を介して形成することがより好ましい。ハードコート層の塗布は図8の模式図に示すように別位置に配した2つの押し出し式塗布装置401、402によって塗設することができる。
【0200】
ハードコート層(活性線硬化樹脂層)は、種々の機能を有していてもよく、例えば、防眩層やクリアハードコート層であってもよい。ハードコート層(活性線硬化樹脂層)はエチレン性不飽和モノマーを1種以上含む成分を重合させて形成した層であることが好ましい。
【0201】
エチレン性不飽和モノマーを含む成分を重合させて形成した樹脂層としては、活性線硬化樹脂あるいは熱硬化樹脂を硬化させて形成された層が好ましく用いられるが、特に好ましく用いられるのは活性線硬化樹脂層である。
【0202】
ここで、活性線硬化樹脂層とは紫外線や電子線のような活性線照射により架橋反応などを経て硬化する樹脂を主たる成分とする層をいう。
【0203】
活性線硬化樹脂としては紫外線硬化性樹脂や電子線硬化性樹脂などが代表的なものとして挙げられるが、紫外線や電子線以外の活性線照射によって硬化する樹脂でもよい。
【0204】
紫外線硬化性樹脂としては、例えば、紫外線硬化型アクリルウレタン系樹脂、紫外線硬化型ポリエステルアクリレート系樹脂、紫外線硬化型エポキシアクリレート系樹脂、紫外線硬化型ポリオールアクリレート系樹脂または紫外線硬化型エポキシ樹脂等を挙げることができる。
【0205】
具体例としては、例えば、トリメチロールプロパントリアクリレート、ジトリメチロールプロパンテトラアクリレート、ペンタエリスリトールトリアクリレート、ペンタエリスリトールテトラアクリレート、ジペンタエリスリトールヘキサアクリレート、アルキル変性ジペンタエリスリトールペンタアクリレート等を挙げることができる。
【0206】
紫外線硬化型アクリルウレタン系樹脂としては、一般にポリエステルポリオールにイソシアネートモノマー、もしくはプレポリマーを反応させて得られた生成物に更に2−ヒドロキシエチルアクリレート、2−ヒドロキシエチルメタクリレート(以下アクリレートにはメタクリレートを包含するものとしてアクリレートのみを表示する)、2−ヒドロキシプロピルアクリレート等の水酸基を有するアクリレート系のモノマーを反応させる容易に形成されるものを挙げることができ、特開昭59−151110号公報に記載のものを用いることができる。
【0207】
紫外線硬化型ポリエステルアクリレート系樹脂としては、一般にポリエステルポリオールに2−ヒドロキシエチルアクリレート、2−ヒドロキシアクリレート系のモノマーを反応させる容易に形成されるものを挙げることができ、特開昭59−151112号公報に記載のものを用いることができる。
【0208】
紫外線硬化型エポキシアクリレート系樹脂の具体例としては、エポキシアクリレートをオリゴマーとし、これに反応性希釈剤、光反応開始剤を添加し、反応させて生成するものを挙げることができ、特開平1−105738号公報に記載のものを用いることができる。
【0209】
これらの光反応開始剤としては、具体的には、ベンゾイン及び誘導体、アセトフェノン、ベンゾフェノン、ヒドロキシベンゾフェノン、ミヒラーズケトン、α−アミロキシムエステル、チオキサントン等及びこれらの誘導体を挙げることができる。光増感剤と共に使用してもよい。
【0210】
上記光反応開始剤も光増感剤としても使用できる。また、エポキシアクリレート系の光反応剤の使用の際、n−ブチルアミン、トリエチルアミン、トリ−n−ブチルホスフィン等の増感剤を用いることができる。
【0211】
樹脂モノマーとしては、例えば、不飽和二重結合が一つのモノマーとして、メチルアクリレート、エチルアクリレート、ブチルアクリレート、ベンジルアクリレート、シクロヘキシルアクリレート、酢酸ビニル、スチレン等の一般的なモノマーを挙げることができる。また不飽和二重結合を二つ以上持つモノマーとして、エチレングリコールジアクリレート、プロピレングリコールジアクリレート、ジビニルベンゼン、1,4−シクロヘキサンジアクリレート、1,4−シクロヘキシルジメチルアジアクリレート、前出のトリメチロールプロパントリアクリレート、ペンタエリスリトールテトラアクリルエステル等を挙げることができる。
【0212】
本発明において使用することができる紫外線硬化樹脂としては、例えばアデカオプトマーKR・BYシリーズ:KR−400、KR−410、KR−550、KR−566、KR−567、BY−320B(旭電化(株)製);コーエイハードA−101−KK、A−101−WS、C−302、C−401−N、C−501、M−101、M−102、T−102、D−102、NS−101、FT−102Q8、MAG−1−P20、AG−106、M−101−C(広栄化学(株)製);セイカビームPHC2210(S)、PHC X−9(K−3)、PHC2213、DP−10、DP−20、DP−30、P1000、P1100、P1200、P1300、P1400、P1500、P1600、SCR900(大日精化工業(株)製);KRM7033、KRM7039、KRM7130、KRM7131、UVECRYL29201、UVECRYL29202(ダイセル・ユーシービー(株)製);RC−5015、RC−5016、RC−5020、RC−5031、RC−5100、RC−5102、RC−5120、RC−5122、RC−5152、RC−5171、RC−5180、RC−5181(大日本インキ化学工業(株)製);オーレックスNo.340クリヤ(中国塗料(株)製);サンラッドH−601、RC−750、RC−700、RC−600、RC−501、RC−611、RC−612(三洋化成工業(株)製);SP−1509、SP−1507(昭和高分子(株)製);RCC−15C(グレース・ジャパン(株)製)、アロニックスM−6100、M−8030、M−8060(東亞合成(株)製)等の市販品から適宜選択して利用できる。
【0213】
以上、特に紫外線硬化樹脂層として説明したが他の活性線樹脂層であっても同様の効果を示す。
【0214】
これらの活性線硬化樹脂層は公知の方法で塗設することができる。
紫外線硬化性樹脂を光硬化反応により硬化皮膜層を形成するための光源としては、紫外線を発生する光源であれば制限なく使用できる。例えば、低圧水銀灯、中圧水銀灯、高圧水銀灯、超高圧水銀灯、カーボンアーク灯、メタルハライドランプ、キセノンランプ等を用いることができる。照射条件はそれぞれのランプによって異なるが、照射光量は20〜10000mJ/cm程度あればよく、好ましくは、50〜2000mJ/cmである。近紫外線領域〜可視光線領域にかけてはその領域に吸収極大のある増感剤を用いることによって効率よく形成することができる。
【0215】
紫外線硬化樹脂層組成物塗布液の有機溶媒としては、例えば、炭化水素類、アルコール類、ケトン類、エステル類、グリコールエーテル類、その他の有機溶媒の中から適宜選択し、あるいはこれらを混合し利用できる。プロピレングリコールモノアルキルエーテル(アルキル基の炭素原子数として1〜4)またはプロピレングリコールモノアルキルエーテル酢酸エステル(アルキル基の炭素原子数として1〜4)等を5質量%以上、より好ましくは5〜80質量%含有する上記有機溶媒を用いるのが好ましい。
【0216】
紫外線硬化性樹脂組成物塗布液の塗布方法としては、図8に示した前述の押し出し式塗布装置401,402を用いることができるが、塗布量はウェット膜厚として0.1〜30μmが適当で、好ましくは、0.5〜15μmである。
【0217】
塗布される紫外線硬化性樹脂組成物に対しては、図8に示すように塗布乾燥中又は後に、紫外線照射装置403,404によって紫外線を照射するのがよく、照射時間としては0.1秒〜5分が好ましく、紫外線硬化性樹脂の硬化効率または作業効率や生産性の観点から0.1秒〜10秒がより好ましい。
【0218】
こうして得た硬化樹脂層に、ブロッキングを防止するために、また耐擦り傷性等を高めるために、或いは防眩性を付与するために、無機化合物あるいは有機化合物の微粒子を加えることもでき、それらの種類としては、前述のマット剤の微粒子とほぼ同様である。
【0219】
これらの微粒子粉末の平均粒径としては、0.005μm〜5μmが好ましく0.01〜1μmであることが特に好ましい。粒径や材質(屈折率)の異なる粒子を2種以上含有することが好ましい。
【0220】
紫外線硬化樹脂組成物と微粒子粉末との割合は、該樹脂組成物100質量部に対して、0.1〜10質量部であることが好ましい。
【0221】
紫外線硬化樹脂層は、JIS B 0601で規定される中心線平均粗さ(Ra)が1〜50nmのクリアハードコート層であっても、Raが0.1〜1μmの防眩層であってもよい。
【0222】
紫外線硬化樹脂層は2層以上を重ねて塗設する。これにより、より硬度や耐摩擦性に優れたハードコート層を形成することができる。ハードコート層は鉛筆硬度で2H以上であることが好ましく、特に3H〜6Hであることが好ましい。又、必要に応じてセルロースエステルフィルムの両面にハードコート層を塗設することもできる。
【0223】
また、防眩性を付与するため上層の紫外線硬化樹脂層に微粒子を添加しても良く、2層とも微粒子を添加しても良い。
【0224】
上記ハードコート層の活性線樹脂層の添加物について述べる。
下層のハードコート層に可塑剤を含有させる量は0.5〜12質量%が好ましく、特に1〜10質量%が好ましい。可塑剤はハードコート塗布液にあらかじめ添加することができる。あるいは事前に可塑剤をプラスチック基材表面に塗布やスプレー或いはその他の方法で付着させておき、その上に下層の活性線硬化樹脂層を塗布することで下層の活性線硬化樹脂層中に可塑剤を含有させることができる。上層の活性線硬化樹脂層は可塑剤を含有しないことが好ましいが下層から溶出してきた可塑剤を若干含んでいても良い。可塑剤はセルロースエステル等の基材シートに添加することができる可塑剤が好ましく用いられる。
【0225】
本発明では2層のハードコート層を形成する際に1層目の塗布完了後に巻き取ることなく2層目も連続的に形成することによって、この上に形成した金属化合物層のすじむらが低減され、反射光の色むらもさらに低減することができる。
【0226】
連続的に2層のハードコート層を形成する際に、下層のハードコート層は塗布乾燥後紫外線を照射してハーフキュアの状態とし、その上に上層のハードコート層を形成することが好ましい。
【0227】
更に、本発明においては、プラズマ放電処理によって金属化合物層をハードコート層上に形成する方法が特に好ましく用いられる。
【0228】
以下に、プラズマ放電処理により金属化合物層を形成する方法を図9、図10を用いて説明する。
【0229】
図9は、本発明に有用なジェット方式の大気圧プラズマ放電処理装置の一例を示した概略図である。
【0230】
ジェット方式の大気圧プラズマ放電処理装置は、プラズマ放電処理装置、二つの電源を有する電圧印加手段の他に、図9では図示していない(後述の図11に図示してある)が、ガス供給手段、電極温度調節手段を有している装置である。
【0231】
プラズマ放電処理装置310は、第1電極311と第2電極312から構成されている対向電極を有しており、該対向電極間に、第1電極311からは第1電源321からの第1の周波数ωの高周波電圧Vが印加され、また第2電極312からは第2電源322からの第2の周波数ωの高周波電圧Vが印加されるようになっている。第1電源321は第2電源322より大きな高周波電圧(V>V)を印加出来る能力を有していればよく、また第1電源321の第1の周波数ωと第2電源322の第2の周波数ωの関係はω<ωである。
【0232】
第1電極311と第1電源321との間には、第1電源321からの電流Iが第1電極311に向かって流れるように第1フィルター323が設置されており、第1電源321からの電流Iをアース側へ通過しにくくし、第2電源322からの電流Iがアース側へ通過し易くするように設計されている。
【0233】
また、第2電極312と第2電源322との間には、第2電源322からの電流Iが第2電極312に向かって流れるように第2フィルター324が設置されており、第2電源322からの電流Iをアース側へ通過しにくくし、第1電源321からの電流Iをアース側へ通過し易くするように設計されている。
【0234】
第1電極311と第2電極312との対向電極間(放電空間)313に、ガス供給手段からガスGを導入し、第1電極311と第2電極312に高周波電圧を印加して放電を発生させ、ガスGをプラズマ状態にし対向電極の下側(紙面下側)にジェット状に吹き出させて、基材シートFに施したハードコート層の上に、処理位置314付近で薄膜を形成させる。プラズマ放電処理の際の基材シートFの温度によっては、得られる薄膜の物性や組成が変化することがあり、これに対して適宜制御することが望ましい。温度調節の媒体としては、蒸留水、油等の絶縁性材料が好ましく用いられる。プラズマ放電処理の際、幅手方向あるいは長手方向での基材の温度ムラが出来るだけ生じないように電極の表面の温度や基材シート表面の温度を均一に調節することが望まれる。
【0235】
また、図9に前述の高周波電圧(印加電圧)と放電開始電圧の測定に使用する測定器を示した。325及び326は高周波プローブであり、327及び328はオシロスコープである。
【0236】
ジェット方式の該大気圧プラズマ放電処理装置を複数基接して直列に並べることで連続的に高速で処理することも出来る。また各装置が異なったガスをジェット噴射すれば、異なった層の積層薄膜を形成することも出来る。
【0237】
図10は本発明に有用な別の大気圧プラズマ放電処理装置の一例を示す概略図である。
【0238】
この大気圧プラズマ放電処理装置は、少なくとも、プラズマ放電処理装置330、二つの電源を有する電圧印加手段340、ガス供給手段350、電極温度調節手段360を有している。
【0239】
ロール回転電極(第1電極)335と角筒型固定電極群(第2電極)336との対向電極間(放電空間)332で、基材シートF上にプラズマ放電処理によって金属化合物の薄膜を形成することができる。
【0240】
ロール回転電極(第1電極)335には第1電源341から周波数ωの高周波電圧Vを、また角筒型固定電極群(第2電極)336には第2電源342から周波数ωの高周波電圧Vを印加することができる。
【0241】
ロール回転電極(第1電極)335と第1電源341との間には、第1電源341からの電流Iがロール回転電極(第1電極)335に向かって流れるように第1フィルター343が設置されており、該第1フィルターは第1電源341からの電流Iをアース側へ通過しにくくし、第2電源342からの電流Iをアース側へ通過し易くするように設計されている。また、角筒型固定電極群(第2電極)336と第2電源342との間には、第2電源からの電流Iが第2電極に向かって流れるように第2フィルター344が設置されており、第2フィルター344は、第2電源342からの電流Iをアース側へ通過しにくくし、第1電源341からの電流Iをアース側へ通過し易くするように設計されている。
【0242】
なお、ロール回転電極335を第2電極、また角筒型固定電極群336を第1電極としてもよい。何れにしろ第1電極には第1電源が、また第2電極には第2電源が接続される。第1電源は第2電源より大きな高周波電圧(V>V)を印加出来る能力を有しており、また、周波数はω<ωとなる能力を有している。
【0243】
ガス供給手段350のガス供給装置351で発生させたガスGは、流量を制御して給気口352より、固定電極336の間から対向電極間332に供給される。また対向電極間より排ガスG’が排気される。しかし、ガス供給口352とガス排気口353は固定電極336の間に交互に設けることが好ましい。
【0244】
ハードコート層が形成された基材シートFを、図示されていない元巻きから巻きほぐして搬送されて来るか、または前工程から搬送されて来て、ガイドロール364を経てニップロール365で基材に同伴されて来る空気等を遮断し、ロール回転電極335に接触したまま巻き回しながら角筒型固定電極群336との間に移送し、ロール回転電極(第1電極)335と角筒型固定電極群(第2電極)336との両方から電圧をかけ、対向電極間(放電空間)332で放電プラズマを発生させる。ハードコート層が形成された基材シートFはロール回転電極335に接触したまま巻き回されながらプラズマ状態のガスにより薄膜を形成する。前記基材シートFは、ニップロール366、ガイドロール367を経て、図示していない巻き取り機で巻き取るか、次工程に移送する。
【0245】
薄膜形成中、ロール回転電極(第1電極)335及び角筒型固定電極群(第2電極)336を加熱または冷却するために、電極温度調節手段360で温度を調節した媒体を、送液ポンプPで配管361を経て両電極に送り、電極内側から温度を調節する。ロール回転電極335と固定電極群336はそれぞれ独立に温度調節することができる。なお、368及び369はプラズマ放電処理容器331と外界とを仕切る仕切板である。
【0246】
図11は、図10に示したロール回転電極の導電性の金属質母材とその上に被覆されている誘電体の構造の一例を示す斜視図である。
【0247】
図11において、ロール電極335aは導電性の金属質母材335Aとその上に誘電体335Bが被覆されたものである。内部は中空のジャケットになっていて温度調節用媒体を循環させて温度調節できるようになっている。
【0248】
図12は、角筒型電極の導電性の金属質母材とその上に被覆されている誘電体の構造の一例を示す斜視図である。
【0249】
図12において、角筒型電極336aは、導電性の金属質母材336Aに対し、図11同様の誘電体336Bの被覆を有し、該電極の構造は金属質のパイプになっていて、それがジャケットとなり、放電中の温度調節が行えるようになっている。
【0250】
なお、角筒型固定電極の数は、上記ロール電極の円周より大きな円周上に沿って複数本設置されており、該電極の放電面積はロール回転電極335に対向している全角筒型固定電極面の面積の和で表される。
【0251】
図10に示した角筒型電極336aは、円筒型電極でもよいが、角筒型電極は円筒型電極に比べて、放電範囲(放電面積)を広げる効果があるので、本発明に好ましく用いられる。
【0252】
図11及び12において、ロール電極335a及び角筒型電極336aは、それぞれ導電性の金属質母材335A、336Aの上に誘電体335B、336Bとしてのセラミックスを溶射後、無機化合物の封孔材料を用いて封孔処理したものである。セラミックス誘電体の膜厚は0.1〜5mm、好ましくは1〜3mmである。溶射に用いるセラミックス材としては、アルミナ・窒化珪素等が好ましく用いられるが、この中でもアルミナが加工し易いので、特に好ましく用いられる。また、誘電体層が、ガラスライニングにより無機材料を設けたライニング処理誘電体であってもよい。
【0253】
導電性の金属質母材335A及び336Aとしては、チタン金属またはチタン合金、銀、白金、ステンレススティール、アルミニウム、鉄等の金属等や、鉄とセラミックスとの複合材料またはアルミニウムとセラミックスとの複合材料等を挙げることが出来るが、後述の理由から、チタン金属またはチタン合金が特に好ましい。
【0254】
2個の電極間の距離(電極間隙)は、導電性の金属質母材に設けた誘電体の厚さ、印加電圧の大きさ、プラズマを利用する目的等を考慮して決定されるが、電極の一方に誘電体を設けた場合の誘電体表面と導電性の金属質母材表面の最短距離、上記電極の双方に誘電体を設けた場合の誘電体表面同士の距離としては、いずれの場合も均一な放電を行う観点から0.1nm〜20mmが好ましく、特に好ましくは0.5nm〜2mmである。
【0255】
本発明に有用な導電性の金属質母材及び誘電体についての詳細については後述する。
【0256】
プラズマ放電処理容器331はパイレックス(R)ガラス製の処理容器等が好ましく用いられるが、電極との絶縁がとれれば金属製を用いることも可能である。例えば、アルミニウムまたは、ステンレススティールのフレームの内面にポリイミド樹脂等を張り付けても良く、該金属フレームにセラミックス溶射を行い絶縁性をとってもよい。図9において、平行した両電極の両側面(基材面近くまで)を上記のような材質の物で覆うことが好ましい。
【0257】
本発明の大気圧プラズマ放電処理装置に設置する第1電源(高周波電源)としては、周波数が1〜200kHzのものが好ましく用いられる、
印加電源記号 メーカー 周波数
A1 神鋼電機 3kHz
A2 神鋼電機 5kHz
A3 春日電機 15kHz
A4 神鋼電機 50kHz
A5 ハイデン研究所 100kHz*
A6 パール工業 200kHz
等の市販のものを挙げることが出来、何れも使用することが出来る。なお、*印はハイデン研究所インパルス高周波電源(連続モードで100kHz)である。
【0258】
また、第2電源(高周波電源)としては、周波数800kHz以上のものが好ましく用いられ、
印加電源記号 メーカー 周波数
B1 パール工業 800kHz
B2 パール工業 2MHz
B3 パール工業 13.56MHz
B4 パール工業 27MHz
B5 パール工業 150MHz
等の市販のものを挙げることが出来、何れも好ましく使用出来る。
【0259】
このような電圧を印加して、グロー放電状態を保つことが出来る。
本発明において、対向する電極間に印加する電力は、1W/cm以上の電力(出力密度)を供給することが好ましく、これにより放電ガスを励起してプラズマを発生させ、エネルギーを薄膜形成性ガスに与え薄膜を形成させる。供給する電力は1〜50W/cmが好ましい。なお、放電面積(cm)は、電極において放電が起こる範囲の面積のことを指す。
【0260】
ここで高周波電圧の印加法としては、連続モードと呼ばれる連続サイン波状の連続発振モード0と、パルスモードと呼ばれるON/OFFを断続的に行う断続発振モードのどちらを採用してもよいが、少なくとも第2電極側は連続サイン波の方がより緻密で良質な膜が得られるので好ましい。
【0261】
このような大気圧プラズマによる薄膜形成法に使用する電極は、構造的にも、性能的にも過酷な条件に耐えられるものでなければならない。このような電極としては、金属質母材上に誘電体を被覆したものであることが好ましい。
【0262】
本発明に使用する誘電体被覆電極においては、様々な金属質母材と誘電体との間に特性が合うものが好ましく、その一つの特性として、金属質母材と誘電体との線熱膨張係数の差が10×10−6/℃以下となる組み合わせのものである。好ましくは8×10−6/℃以下、更に好ましくは5×10−6/℃以下、更に好ましくは2×10−6/℃以下である。なお、線熱膨張係数とは、周知の材料特有の物性値である。
【0263】
線熱膨張係数の差が、この範囲にある導電性の金属質母材と誘電体との組み合わせとしては、
Figure 2004203009
等がある。線熱膨張係数の差という観点では、上記(a)または(b)および(e)〜(h)が好ましく、特に、(a)が好ましい。
【0264】
本発明において、金属質母材は、上記の特性からはチタンまたはチタン合金が特に有用である。金属質母材をチタンまたはチタン合金とすることにより、誘電体を上記とすることにより、使用中の電極の劣化、特にひび割れ、剥がれ、脱落等がなく、過酷な条件での長時間の使用に耐えることが出来る。
【0265】
本発明に有用な電極の金属質母材は、チタンを70質量%以上含有するチタン合金またはチタン金属である。本発明において、チタン合金またはチタン金属中のチタンの含有量は、70質量%以上であれば、問題なく使用出来るが、好ましくは80質量%以上のチタンを含有しているものが好ましい。本発明に有用なチタン合金またはチタン金属は、工業用純チタン、耐食性チタン、高力チタン等として一般に使用されているものを用いることが出来る。工業用純チタンとしては、TIA、TIB、TIC、TID等を挙げることが出来、何れも鉄原子、炭素原子、窒素原子、酸素原子、水素原子等を極僅か含有しているもので、チタンの含有量としては、99質量%以上を有している。耐食性チタン合金としては、T15PBを好ましく用いることが出来、上記含有原子の他に鉛を含有しており、チタン含有量としては、98質量%以上である。また、チタン合金としては、鉛を除く上記の原子の他に、アルミニウムを含有し、その他バナジウムや錫を含有しているT64、T325、T525、TA3等を好ましく用いることが出来、これらのチタン含有量としては、85質量%以上を含有しているものである。これらのチタン合金またはチタン金属はステンレススティール、例えばAISI316に比べて、熱膨張係数が1/2程度小さく、金属質母材としてチタン合金またはチタン金属の上に施された後述の誘電体との組み合わせがよく、高温、長時間での使用に耐えることが出来る。
【0266】
一方、誘電体の求められる特性としては、具体的には、比誘電率が6〜45の無機化合物であることが好ましく、また、このような誘電体としては、アルミナ、窒化珪素等のセラミックス、あるいは、ケイ酸塩系ガラス、ホウ酸塩系ガラス等のガラスライニング材等がある。この中では、後述のセラミックスを溶射したものやガラスライニングにより設けたものが好ましい。特にアルミナを溶射して設けた誘電体が好ましい。
【0267】
または、上述のような大電力に耐える仕様の一つとして、誘電体の空隙率が10体積%以下、好ましくは8体積%以下であることで、好ましくは0体積%を越えて5体積%以下である。なお、誘電体の空隙率は、BET吸着法や水銀ポロシメーターにより測定することが出来る。後述の実施例においては、島津製作所製の水銀ポロシメーターにより金属質母材に被覆された誘電体の破片を用い、空隙率を測定する。誘電体が、低い空隙率を有することにより、高耐久性が達成される。このような空隙を有しつつも空隙率が低い誘電体としては、後述の大気プラズマ溶射法等による高密度、高密着のセラミックス溶射被膜等を挙げることが出来る。更に空隙率を下げるためには、封孔処理を行うことが好ましい。
【0268】
上記、大気プラズマ溶射法は、セラミックス等の微粉末、ワイヤ等をプラズマ熱源中に投入し、溶融または半溶融状態の微粒子として被覆対象の金属質母材に吹き付け、皮膜を形成させる技術である。プラズマ熱源とは、分子ガスを高温にし、原子に解離させ、更にエネルギーを与えて電子を放出させた高温のプラズマガスである。このプラズマガスの噴射速度は大きく、従来のアーク溶射やフレーム溶射に比べて、溶射材料が高速で金属質母材に衝突するため、密着強度が高く、高密度な被膜を得ることが出来る。詳しくは、特開2000−301655に記載の高温被曝部材に熱遮蔽皮膜を形成する溶射方法を参照することが出来る。この方法により、上記のような被覆する誘電体(セラミック溶射膜)の空隙率にすることが出来る。
【0269】
また、大電力に耐える別の好ましい仕様としては、誘電体の厚みが0.5〜2mmであることである。この膜厚変動は、5%以下であることが望ましく、好ましくは3%以下、更に好ましくは1%以下である。
【0270】
誘電体の空隙率をより低減させるためには、上記のようにセラミックス等の溶射膜に、更に、無機化合物で封孔処理を行うことが好ましい。前記無機化合物としては、金属酸化物が好ましく、この中では特に酸化ケイ素(SiO)を主成分として含有するものが好ましい。
【0271】
封孔処理の無機化合物は、ゾルゲル反応により硬化して形成したものであることが好ましい。封孔処理の無機化合物が金属酸化物を主成分とするものである場合には、金属アルコキシド等を封孔液として前記セラミック溶射膜上に塗布し、ゾルゲル反応により硬化する。無機化合物がシリカを主成分とするものの場合には、アルコキシシランを封孔液として用いることが好ましい。
【0272】
ここでゾルゲル反応の促進には、エネルギー処理を用いることが好ましい。エネルギー処理としては、熱硬化(好ましくは200℃以下)や、紫外線照射などがある。更に封孔処理の仕方として、封孔液を希釈し、コーティングと硬化を逐次で数回繰り返すと、よりいっそう無機質化が向上し、劣化の無い緻密な電極が出来る。
【0273】
本発明に係る誘電体被覆電極の金属アルコキシド等を封孔液として、セラミックス溶射膜にコーティングした後、ゾルゲル反応で硬化する封孔処理を行う場合、硬化した後の金属酸化物の含有量は60モル%以上であることが好ましい。封孔液の金属アルコキシドとしてアルコキシシランを用いた場合には、硬化後のSiO(xは2以下)含有量が60モル%以上であることが好ましい。硬化後のSiO含有量は、XPS(X線光電子スペクトル)により誘電体層の断層を分析することにより測定できる。
【0274】
本発明の光学フィルムの製造方法に係る電極においては、電極の少なくとも基材と接する側のJIS B 0601で規定される表面粗さの最大高さ(Rmax)が10μm以下になるように調整することが好ましいが、更に好ましくは、8μm以下であり、特に好ましくは、7μm以下に調整することである。このように誘電体被覆電極の誘電体表面を研磨仕上げする等の方法により、誘電体の厚み及び電極間のギャップを一定に保つことが出来、放電状態を安定化出来ること、更に熱収縮差や残留応力による歪やひび割れを無くし、且つ、高精度で、耐久性を大きく向上させることが出来る。誘電体表面の研磨仕上げは、少なくとも基材と接する側の誘電体において行われることが好ましい。
【0275】
本発明に使用する誘電体被覆電極において、大電力に耐える他の好ましい仕様としては、耐熱温度が100℃以上であることである。更に好ましくは120℃以上、特に好ましくは150℃以上である。また上限は500℃である。なお、耐熱温度とは、絶縁破壊が発生せず、正常に放電出来る状態において耐えられる最も高い温度のことを指す。このような耐熱温度は、上記のセラミックス溶射や、泡混入量の異なる層状のガラスライニングで設けた誘電体を適用したり、下記金属質母材と誘電体の線熱膨張係数の差の範囲内の材料を適宜選択する手段を適宜組み合わせることによって達成可能である。
【0276】
《反応ガス》
本発明の金属化合物層の形成に用いる反応ガスについて説明する。
【0277】
薄膜層を形成するための反応ガスは、主に窒素を含むガスである。すなわち、窒素ガスが50%以上で含有することが好ましく、さらに好ましくは70%以上で含有することが好ましく、さらに好ましくは90体積%〜99.99体積%であることが望ましい。反応ガスには窒素のほかに希ガスが含有していてもよい。
【0278】
ここで、希ガスとは、周期表の第18属元素、具体的には、ヘリウム、ネオン、アルゴン、クリプトン、キセノン、ラドン等であり、本発明では、ヘリウム、アルゴン等が窒素に添加されて用いられてもよい。
【0279】
窒素ガスは安定したプラズマ放電を発生させるために用いられ、反応ガスには薄膜を形成するための原料として、反応性ガス(原料ガス)が添加される。該プラズマ中で反応性ガスはイオン化あるいはラジカル化され、基材表面に堆積あるいは付着するなどして薄膜が形成される。
【0280】
更に、反応ガス中に酸素、水素、二酸化炭素、一酸化炭素、二酸化窒素、一酸化窒素、水、過酸化水素、オゾン、メタン、4フッ化メタン等を0.1体積%〜10体積%含有させることにより薄膜層の硬度、密度等の物性を制御することができる。
【0281】
本発明に有用な反応ガスは、様々な物質の原料ガスを添加したものを用いることによって、様々な機能を持った薄膜をセルロースエステルフィルム等の基材上に形成することができる。ここでいう原料ガスとはプラズマ処理により薄膜を形成するためのガスであり、金属酸化物、金属窒化物、金属酸窒化物等の金属化合物層を形成する場合、金属化合物のガスを意味する。
【0282】
本発明に有用な原料ガスとしての有機金属化合物としては、特に限定されないが、Al、As、Au、B、Bi、Sb、Ca、Cd、Cr、Co、Cu、Fe、Ga、Ge、Hg、In、Li、Mg、Mn、Mo、Na、Ni、Pb、Pt、Rh、Se、Si、Sn、Ti、Zr、Y、V、W、Zn,Ta等の金属酸化物を形成するための金属化合物を挙げることができる。
【0283】
例えばTi、Zr、In、Sn、Zn、Ge、Si、Taあるいはその他の金属を含有する有機金属化合物、金属水素化合物、金属ハロゲン化物、金属錯体を用いて、これらの金属酸化物層(ここでいう金属酸化物層には、金属酸化物窒化物層も含む)または金属窒化物層等を形成することができ、これらの層は反射防止層の中屈折率層または高屈折率層としたり、あるいは透明導電層または帯電防止層とすることもできる。
【0284】
また、フッ素含有有機化合物で防汚層や低屈折率層を形成することもでき、珪素化合物でガスバリア層や低屈折率層あるいは防汚層を形成することもできる。本発明は、高、中屈折率層と低屈折率層を交互に多層を積層して形成される反射防止層の形成に特に好ましく用いられる。
【0285】
本発明において、反応性ガスとして有機金属化合物を用いる場合、プラズマ放電処理によりセルロースエステルフィルム等の基材シートの上に均一な薄膜を形成する観点から、反応ガス中の原料ガスとしての金属化合物の含有率は、0.01〜10体積%であることが好ましいが、更に好ましくは、0.1〜5体積%である。
【0286】
(原料ガス)
原料ガスについてさらに詳細に説明する。
【0287】
反射防止層の高屈折率層を形成するには、チタン化合物、ジルコニウム化合物、タンタル化合物が好ましく、具体的には、例えば、テトラジメチルアミノチタンなどの有機アミノ金属化合物、モノチタン、ジチタンなどの金属水素化合物、二塩化チタン、三塩化チタン、四塩化チタンなどの金属ハロゲン化合物、テトラエトキシチタン、テトライソプロポキシチタン、テトラブトキシチタン、テトラエトキシジルコニウム、テトライソプロポキシジルコニウム、テトラブトキシジルコニウム、ペンタイソプロポキシタンタル、ペンタエトキシタンタルなどの金属アルコキシドなどを挙げることができ、これらを用いて金属酸化物層を形成することができる。
【0288】
亜鉛化合物としては、ジンクアセチルアセトナート、ジエチル亜鉛、ジメチル亜鉛などがあげられ、錫化合物としては、テトラエチルスズ、テトラメチルスズ、二酢酸ジ−n−ブチルすず、ビス(2−エチルヘキサン酸)ジブチルすず、二酢酸ジブチルすず、酸化ジブチルすず、二ラウリン酸ジブチルすず、テトラメチルすず、テトラエチルすず、テトラブチルすず、テトラプロピルすず、テトラオクチルすず等の有機錫化合物が好ましく用いられ、インジウム化合物としてはトリエチルインジウム、トリメチルインジウムなどが好ましく用いられる。
【0289】
(フッ素化合物)
大気圧プラズマ処理では原料ガスにフッ素含有有機化合物を用いることでフッ素化合物含有層を形成することもできる。
【0290】
フッ素含有有機化合物としては、フッ化炭素ガス、フッ化炭化水素ガス等が好ましい。
【0291】
具体的には、フッ素含有有機化合物としては、例えば、四フッ化炭素、六フッ化炭素、四フッ化エチレン、六フッ化プロピレン、八フッ化シクロブタン等のフッ化炭素化合物;
二フッ化メタン、四フッ化エタン、四フッ化プロピレン、三フッ化プロピレン、八フッ化シクロブタン等のフッ化炭化水素化合物;
更に、一塩化三フッ化メタン、一塩化二フッ化メタン、二塩化四フッ化シクロブタン等のフッ化炭化水素化合物のハロゲン化物、アルコール、酸、ケトン等の有機化合物のフッ素置換体等を挙げることができる。
【0292】
これらは単独でも混合して用いてもよい。上記のフッ化炭化水素ガスとしては、二フッ化メタン、四フッ化エタン、四フッ化プロピレン、三フッ化プロピレン等の各ガスを挙げることができる。
【0293】
更に、一塩化三フッ化メタン、一塩化二フッ化メタン、二塩化四フッ化シクロブタン等のフッ化炭化水素化合物のハロゲン化物やアルコール、酸、ケトン等の有機化合物のフッ素置換体を用いることができるが、本発明はこれらに限定されない。
【0294】
また、これらの化合物は分子内にエチレン性不飽和基を有していても良い。また、上記の化合物は混合して用いても良い。
【0295】
本発明に有用な反応性ガスにフッ素含有有機化合物を用いる場合、プラズマ放電処理によりセルロースエステルフィルム上に均一な薄膜を形成する観点から、反応ガス中の反応性ガスとしてのフッ素含有有機化合物の含有率は、0.01〜10体積%であることが好ましいく、更に好ましくは、0.1〜5体積%である。
【0296】
また、本発明に好ましく用いられるフッ素含有、有機化合物が常温常圧で気体である場合は、反応性ガスの成分としてそのまま使用できる。
【0297】
また、フッ素含有有機化合物が常温常圧で液体または固体である場合には、気化手段により、例えば加熱、減圧等により気化して使用すればよく、適切な有機溶媒に溶解して用いてもよい。
【0298】
(珪素化合物)
本発明に有用な反応性ガスとしての珪素化合物としては、例えば、ジメチルシラン、テトラメチルシランなどの有機金属化合物、モノシラン、ジシランなどの金属水素化合物、二塩化シラン、三塩化シラン、四フッ化珪素などの金属ハロゲン化合物、テトラメトキシシラン、テトラエトキシシラン、テトラプロポキシシラン、ジメチルジエトキシシラン、メチルトリメトキシシラン、メチルトリエトキシシラン、エチルトリエトキシシラン、などのアルコキシシラン、テトラメチルシラン、ヘキサメチルジシロキサン、オルガノシラン等、3,3,3−トリフルオロメチルトリメトキシシラン等のフルオロアルキルシラン類を用いることが好ましいがこれらに限定されない。
【0299】
また、これらは適宜組み合わせて用いることができる。あるいは別の有機化合物を添加して膜の物性を変化あるいは制御することもできる。
【0300】
また、珪素化合物、チタン化合物、ジルコニウム化合物、タンタル化合物等の金属化合物を放電部へ導入するには、両者は常温常圧で気体、液体または固体いずれの状態であっても使用し得る。
【0301】
気体の場合は、そのまま放電部に導入できるが、液体や固体の場合は、加熱、減圧、超音波照射等の気化手段により気化させて使用することができる。この目的のため、市販の気化器が好ましく用いられる。
【0302】
珪素化合物、チタン化合物等の金属化合物を加熱により気化して用いる場合、テトラエトキシシラン、テトライソプロポキシチタンなどのように常温で液体で、且つ、沸点が200℃以下である金属アルコキシドが本発明の金属酸化物薄膜層の形成する方法に好適である。上記金属アルコキシドは、有機溶媒によって希釈して使用しても良く、有機溶媒としては、メタノール、エタノール、n−ヘキサン、アセトンなどの有機溶媒またはこれらの混合有機溶媒を使用することができる。
【0303】
(金属化合物層の膜厚)
本発明に係る金属化合物層の膜厚としては、1nm〜1000nmの範囲のものが好ましく得られる。
【0304】
このような金属化合物層は、例えば低屈折率層あるいは防眩層と高屈折率層を積層し反射防止層として、或いは透明導電層、帯電防止層とすることができる。
【0305】
本発明において、プラズマ放電装置を複数設けることによって、多層の薄膜を連続的に設けることができ、薄膜のムラもなく多層の積層体を形成することができる。例えば1つの層を形成した後1分以内に次の層を形成することが好ましい。複数の層を1パスで連続的に形成するためには、各層が所定の薄膜形成速度となるように調整されることが必要である。そのため、各層形成後膜厚を測定するか、反射スペクトルを測定し、その結果に基づいて薄膜形成速度をフィードバック制御することが好ましい。これによって、一定の速度で搬送される基材フィルム上に異なる組成あるいは異なる膜厚の薄膜を1パスで連続的に形成することができる。各層の薄膜形成速度を制御する方法としては、特に限定はないが、
放電の印加電圧、電流、周波数、パルス条件等の放電条件、反応ガス中の各成分の比率(窒素濃度、酸素あるいは水素等の添加ガス濃度、種類、原料ガス濃度)、反応ガス供給量、電極間距離、放電部の気圧、基材温度、電極温度、反応ガス温度、放電部の温度、放電面積の変更等があげられるが、これらのみに限定されるものではない。これらの1つ以上の条件を適宜組み合わせることによって、製膜される薄膜の膜質を大きく変えることなく、薄膜形成速度を制御することができる。
【0306】
例えば、セルロースエステルフィルム上に反射防止層を有する光学フィルムを作製する場合、屈折率1.6〜2.3の高屈折率層及び屈折率1.3〜1.5の低屈折率層をセルロースエステルフィルム表面に連続して積層し、効率的に作製することができる。
【0307】
低屈折率層としては、含フッ素有機化合物を含むガスをプラズマ放電処理により形成された含フッ素化合物層、あるいはアルコキシシラン等の有機珪素化合物を用いてプラズマ放電処理により形成された主に酸化ケイ素を有する層が好ましく、高屈折率層としては、有機金属化合物を含むガスをプラズマ放電処理により形成された金属酸化物層、例えば酸化チタン、酸化ジルコニウム、酸化タンタルを主として有する層が好ましい。これらの層は原料ガス内の炭素又は炭素化合物を含有していても良い。
【0308】
本発明はこれらに限定されるものではなく、層構成もこれらに限定されるものではない。例えば、最表面にフッ素含有有機化合物ガス存在下で大気圧もしくはその近傍の圧力下でのプラズマ放電処理して防汚層を設けてもよい。あるいは公知の防汚層、例えばフルオロアルキルシラン等含む組成物を塗設することもできる。
【0309】
上記の方法により、本発明においては、多層の薄膜を積層することができ、各層の膜厚むらもなく、均一な光学フィルムを得ることができる。
【0310】
金属酸化物層等の薄膜の膜厚は、積層体の断面を作製し、透過電子顕微鏡(Transmission Electoron Microscope:以下、TEMと称す)で観察を行うことによって求めることができる。
【0311】
断面の作製は、具体的には積層体を基材と共に電子顕微鏡観察前処理用のエポキシ包埋樹脂に包埋し、ダイヤモンドナイフを装着したウルトラミクロトームを用いて、厚さ約80nmの超薄切片を作製するか、集束イオンビーム(Focused Ion Beam:FIB)加工装置を用いて、積層体表面にGaイオンビームを集束走査し、厚さ約100nmの薄片化した断面を切り出すことで作製することができる。
【0312】
TEMによる観察は倍率として50,000〜500,000倍にて明視野像を観察し、画像はフィルム、イメージングプレート、CCDカメラなどに記録する。
【0313】
TEMの加速電圧としては、80〜400kVが好ましく、特に好ましくは80〜200kVである。
【0314】
その他、電子顕微鏡観察技法、および試料作製技法の詳細については「日本電子顕微鏡学会関東支部編/医学・生物学電子顕微鏡観察法」(丸善)、「日本電子顕微鏡学会関東支部編/電子顕微鏡生物試料作製法」(丸善)、「電子顕微鏡Q&A」(アグネ承風社)をそれぞれ参考にすることができる。
【0315】
適当な媒体に記録されたTEM画像は、画像1枚を少なくとも1024画素×1024画素、好ましくは2048画素×2048画素以上に分解し、コンピュータによる画像処理を行なうことが好ましい。
【0316】
画像処理技術の詳細は「田中弘編 画像処理応用技術(工業調査会)」を参考にでき、画像処理プログラムまたは装置としては上記操作が可能なものであれば特に限定はされないが、一例としてMEDIA CYBERNETICS社(USA)製画像解析ソフトImage−Pro PLUSが挙げられる。
【0317】
画像処理を行なうためには、フィルムに記録されたアナログ画像はスキャナなどでデジタル画像に変換し、シェーディング補正、コントラスト・エッジ強調などを必要に応じ施すことが好ましい。その後、ヒストグラムを作製し、2値化処理によって、積層体界面に相当する箇所を抽出し、界面間の幅(Thickness)を計測する。
【0318】
同様にして少なくとも25箇所以上好ましくは50箇所以上について求めた値から平均膜厚及びその変動を算出することができる。
【0319】
このように、本発明においては様々な機能を有する金属酸化物層を形成した光学フィルムを提供することができる。
【0320】
本発明により、金属化合物層のすじ状の故障が著しく改善され、クラックも少なく耐擦傷性に優れた光学フィルムを提供することができ、また、反射光の色むらが著しく改善された光学フィルムを提供することができた。
【0321】
【実施例】
以下、実施例を挙げて本発明を具体的に説明するが、本発明の実施態様はこれらに限定されるものではない。
【0322】
実施例1
〔延伸セルロースエステルフィルムの作製〕
〔ドープの調製〕
《ドープAの調製》
セルローストリアセテート(アセチル基置換度2.9) 100質量部
トリフェニルホスフェイト 10質量部
ビフェニルジフェニルホスフェイト 2質量部
例示化合物1 (1,3,5−トリアジン化合物) 1質量部
チヌビン326 0.5質量部
アエロジル R972V (二酸化珪素微粒子) 0.15質量部
メチレンクロライド 405質量部
エタノール 45質量部
以上を密閉型の溶解釜に投入し、攪拌しながら60℃で完全に溶解し、冷却後、安積濾紙(株)製の安積濾紙No.244を使用して濾過してドープAとした。
《ドープBの調製》
セルローストリアセテート(アセチル基置換度2.9) 100質量部
トリフェニルホスフェイト 10質量部
ビフェニルジフェニルホスフェイト 2質量部
チヌビン326 0.5質量部
アエロジル R972V (二酸化珪素微粒子) 0.15質量部
メチレンクロライド 405質量部
エタノール 45質量部
以上を密閉型の溶解釜に投入し、攪拌しながら60℃で完全に溶解し、冷却後、安積濾紙(株)製の安積濾紙No.244を使用して濾過してドープBとした。
【0323】
〔セルロースエステルフィルム1〜7及びH1〜3の作製〕
上記で調製したAをステンレスベルト上に流延した。ステンレスベルト上で、溶媒を蒸発させ、ステンレスベルト上からウェブを剥離した。剥離したウェブをテンター乾燥機に導入し、両端をクリップで把持して幅方向に1.05倍延伸しながら70℃で乾燥させ、110℃次いで125℃の各乾燥ゾーンを有するロール乾燥機内に配置された多数のロールを通して搬送させながら乾燥を終了させ膜厚40μmのセルロースエステルフィルムを作製した。このフィルムの両端に幅10mm、高さ5μmのナーリング加工を施して、1350mm幅、巻長は4000mのセルロースエステルフィルムAを得た。
【0324】
ドープAをドープBに変更した以外は同様にしてセルロースエステルフィルムBを作製した。
【0325】
得られたセルロースエステルフィルムA,Bを用いて、下記に従って表記載のハードコート層1A,1B、2、3を所定の膜厚となるように巻き取ることなく続けて形成し、さらにその上に後述の大気圧プラズマ処理によって金属化合物層を連続して積層した。
【0326】
〈ハードコート層1A,1Bの塗設〉
下記のハードコート層塗布組成物を上記で作製したセルロースエステルフィルムB面側にダイによる押し出しコートをし、次いで80℃に設定された乾燥部で乾燥した後、100mJ/cmで紫外線照射し、所定の乾燥膜厚となるように可塑剤を含有するハードコート層1Aを設けた。紫外線照射後、さらにこの上に所定の乾燥膜厚となるようにハードコート層1Bを設けた。
(ハードコート層1A塗布組成物)
ジペンタエリスリトールヘキサアクリレート単量体 60質量部
ジペンタエリスリトールヘキサアクリレート2量体 20質量部
ジペンタエリスリトールヘキサアクリレート3量体以上の成分 20質量部
ジメトキシベンゾフェノン光反応開始剤 4質量部
トリフェニルホスフェイト 1質量部
酢酸エチル 50質量部
メチルエチルケトン 50質量部
イソプロピルアルコール 50質量部
上記塗布組成物を上記の溶媒で適宜希釈して異なる乾燥膜厚のクリアハードコート層1Aを設けた。
(ハードコート層1B塗布組成物)
ジペンタエリスリトールヘキサアクリレート単量体 60質量部
ジペンタエリスリトールヘキサアクリレート2量体 20質量部
ジペンタエリスリトールヘキサアクリレート3量体以上の成分 20質量部
ジメトキシベンゾフェノン光反応開始剤 4質量部
酢酸エチル 50質量部
メチルエチルケトン 50質量部
イソプロピルアルコール 50質量部
上記塗布組成物を上記の溶媒で希釈して異なる乾燥膜厚のクリアハードコート層1Bを設けた。
【0327】
〈ハードコート層3の塗設〉
下記のハードコート層3塗布組成物を上記で作製したセルロースエステルフィルムB面側にダイによる押し出しコートをし、次いで80℃に設定された乾燥部で乾燥した後、120mJ/cmで紫外線照射し、所定膜厚の可塑剤を含有するハードコート層3を設けた。
【0328】
《ハードコート層3塗布組成物》
酢酸エチル 50質量部
メチルエチルケトン 50質量部
イソプロピルアルコール 50質量部
アエロジルR972V(平均粒径16nm) 2質量部
以上を高速攪拌機(TKホモミキサー、特殊機化工業(株)製)で攪拌し、その後衝突型分散機(マントンゴーリン、ゴーリン(株)製)で分散した後、下記の成分を添加した。
【0329】
ジペンタエリスリトールヘキサアクリレート単量体 30質量部
ジペンタエリスリトールヘキサアクリレート2量体 10質量部
ジペンタエリスリトールヘキサアクリレート3量体以上の成分 10質量部
ジメトキシベンゾフェノン光反応開始剤 2質量部
トリフェニルホスフェート 3質量部
〈ハードコート層2の塗設〉
下記のハードコート層2塗布組成物を上記で作製したセルロースエステルフィルムB面側のハードコート層1Aまたはハードコート層3の上に押し出しコートし、次いで80℃に設定された乾燥部で乾燥した後、120mJ/cmで紫外線照射し、所定膜厚のハードコート層2(中心線平均粗さ(Ra)0.2μm)を設けた。
【0330】
《ハードコート層2塗布組成物》
酢酸エチル 50質量部
メチルエチルケトン 50質量部
イソプロピルアルコール 50質量部
サイリシア431(平均粒径2.5μm、(富士シリシア化学(株)製))
2.5質量部
アエロジルR972V(平均粒径16nm) 3質量部
以上を高速攪拌機(TKホモミキサー、特殊機化工業(株)製)で攪拌し、その後衝突型分散機(マントンゴーリン、ゴーリン(株)製)で分散した後、下記の成分を添加した。
【0331】
ジペンタエリスリトールヘキサアクリレート単量体 60質量部
ジペンタエリスリトールヘキサアクリレート2量体 20質量部
ジペンタエリスリトールヘキサアクリレート3量体以上の成分 20質量部
ジメトキシベンゾフェノン光反応開始剤 4質量部
そして大気圧もしくはその近傍の圧力下で反応ガスを用いてプラズマ放電処理による金属化合物層(反射防止層)の形成を行った。
【0332】
《反射防止層の形成》
下記のプラズマ放電処理装置を用いて、大気圧プラズマ放電処理により、上記のセルロースエステルフィルム1〜12上に各々設けられたハードコート層(紫外線硬化樹脂層)上に反射防止層を各々形成した。
【0333】
《プラズマ放電処理装置》
(電極の作製)
図10に示したプラズマ放電処理装置において、誘電体で被覆したロール電極及び同様に誘電体で被覆した複数の角筒型電極のセットを以下のように作製した。
【0334】
第1電極となるロール電極は、冷却水による冷却手段を有するチタン合金T64製ジャケットロール金属質母材に対して、アルミナ溶射膜を被覆し、テトラメトキシシランを酢酸エチルで希釈した溶液を塗布乾燥後、紫外線照射により硬化させ封孔処理を行った。このようにして被覆した誘電体表面を研磨し、平滑にして、Rmax5μmとなるように加工した。最終的な誘電体の膜厚は1mm、誘電体の比誘電率は10であった。更に導電性の金属質母材と誘電体の線熱膨張係数の差は1.7×10−4で、耐熱温度は260℃であった。
【0335】
一方、第2電極の角筒型電極は、中空の角筒型のチタン合金T64に対し、上記同様の誘電体を同条件にて被覆し、対向する角筒型固定電極群とした。この角筒型電極の誘電体については上記ロール電極のものと同じである。
【0336】
この角筒型電極をロール回転電極のまわりに、対向電極間隙を1mmとして25本配置した。角筒型固定電極群の放電総面積は、150cm(幅手方向の長さ)×4cm(搬送方向の長さ)×25本(電極の数)=15000cmであった。
【0337】
対抗電極間より反応ガスの導入と使用済みガスの排気を交互に行った。
プラズマ放電処理装置には、固定電極側に、連続周波数13.56MHz、0.8kV/mmの高周波電圧(パール工業社製高周波電源)を供給し、ロール電極側には、連続周波数100kHz、8kV/mmの高周波電圧(ハイデン研究所製高周波電源)を供給した。また、ロール電極は、ドライブを用いてセルロースエステルフィルムの搬送に同期して回転させた。プラズマ放電処理装置は各金属酸化層ごとに用意され、各層毎に形成する層の膜厚を制御しながら連続的に運転した。
【0338】
なお、固定電極とロール電極の間隙は1mm、反応ガスの圧力は大気圧+1kPaとして行った。プラズマ放電処理に用いた反応ガス(酸化珪素層形成用反応ガス)の組成を以下に記す。尚、反応ガス中の液体成分は気化器によって蒸気とし、加温しながら放電部に供給した。
【0339】
実施例1で作製した、ハードコート層を有するセルロースエステルフィルム上に、下記の反応ガスを用い、図10に記載のプラズマ放電処理装置によりプラズマ処理を行い、ハードコート層側に反射防止層を形成して光学フィルム1〜12を作製した。
《反射防止層の層構成、層の膜厚、反応ガスの種類》
Figure 2004203009
ハードコート層上に、第1酸化チタン層、第1酸化珪素層、第2酸化チタン層、第2酸化珪素層からなる反射防止層を形成し、更に防汚層の順に設けた。
【0340】
《反応ガスの種類》
また、反射防止層の形成に用いた反応ガスを以下に示す。
【0341】
(反応ガスA):酸化チタン層(高屈折率層)形成用
窒素 98.7体積%
水素 1体積%
テトライソプロポキシチタン蒸気 0.3体積%
(反応ガスB):酸化珪素層(低屈折率層1)形成用
窒素 98.7体積%
水素 1体積%
テトラエトキシシラン蒸気 0.3体積%
(反応ガスC):酸化珪素層(低屈折率層2)形成用
窒素 98.7体積%
反応ガス(水素ガス) 1体積%
反応ガス(メチルトリエトキシシラン蒸気) 0.3体積%
また、2層のハードコート層を設ける際、下層のハードコート層を塗設した後一度巻き取った後、再度上層のハードコート層を形成した以外は表1の光学フィルム10と同様にして光学フィルム13を作製した。下層のハードコート層を塗設した後一度巻き取った後、再度上層のハードコート層を形成した以外は光学フィルム11と同様にして光学フィルム14を作製した。連続してハードコート層を形成した光学フィルム10と11は光学フィルム13と14と比較して反射光のむらが低減された。比較の光学フィルム1,12はすじ故障、クラック、密着性、反射光の色むら(ΔE)が劣っていた。
【0342】
以上、実施例1の結果を表1、表2、表3、表4に示す。
【0343】
【表1】
Figure 2004203009
【0344】
【表2】
Figure 2004203009
【0345】
【表3】
Figure 2004203009
【0346】
【表4】
Figure 2004203009
【0347】
実施例2
〔偏光板の作製〕
光学フィルム10,11と13,14について、A面側を60℃の2mol/LのNaOH水溶液に90秒浸漬後、その後常温水で水洗して、80℃で乾燥しそれぞれの片面鹸化処理した光学フィルムを得た。
【0348】
前記光学フィルムの基材フィルムとして用いたセルロースエステルフィルムについても同様に片面鹸化処理を行った。
【0349】
別に120μmの厚さのポリビニルアルコールをヨウ素1質量部、ホウ酸4質量部を含む水溶液100質量部に浸漬し、50℃で4倍に長尺方向に延伸した偏光膜を用意した。この偏光膜の片面に、上記鹸化処理した光学フィルムの鹸化処理面を、完全鹸化型のポリビニルアルコール5質量%水溶液粘着剤で貼り合わせ同様に反対の面には鹸化されたセルロースエステルフィルムを貼り合わせ、偏光板を得た。これらの偏光板に対し保存性の評価を行い、光学フィルム10,11を使った偏光板は光学フィルム13,14を使った偏光板よりも良好な結果を示した。
【0350】
実施例3
〔液晶画像表示装置〕
市販の液晶表示パネル(NEC製 カラー液晶ディスプレイ MultiSync LCD1525J 型名 LA−1529HM)の最表面の偏光板を注意深く剥離した。ここに実施例2で作製した偏光板試料の偏光方向を合わせて液晶表示パネルに張り付けた。強制劣化を行った偏光板試料を用いて、それぞれの液晶表示パネルについて、目視にて視認性を評価し、光学フィルム10,11を用いたものは光学フィルム13,14を用いたものよりも良好な結果を示した。
【0351】
なお、上記評価は次のように行った。
《評価》
作製した低反射積層体のL値、ΔE(色差,反射光むら)、反射率は下記方法で測定した。
【0352】
(L値の測定)
低反射積層体のL値は、色彩色度計CM−2022(ミノルタ(株)製)を用い、SCI(正反射光込み)方式で測定した分光反射率から求めた。サンプルは、測定側の裏面を粗面化処理した後、黒色のスプレーで光吸収処理(370nmから730nmにおける透過率が10%未満)を行い、黒色の台上にて測定した。
【0353】
(ΔE1および平均L値の測定)
作製したサンプルから、1cm間隔で10cm×10cmの範囲で100点のL値を測定し、1cm間隔で隣接する2点間のΔEの最大値ΔE1を求めた。また、測定したL各々の100点平均より、平均L値を求めた。
【0354】
(反射率)
値の測定のために色彩色度計CM−2022(ミノルタ(株)製)を用い、SCI(正反射光込み)方式で測定した450nmから650nmの範囲の分光反射率から、平均値を求めた。
【0355】
(a値とb値の関係)
ΔE1を求めるために、測定した100点のL値のaとbが、下記(式1)の範囲にあるかどうか確認した。
【0356】
式1 b=−1.5×a±5
(色ムラの評価)
値の測定用に作製したサンプルを目視で評価した。評価基準は下記とし5段階で評価し、Aが最も良い。
【0357】
A 反射光の色調変化がほとんど認められない
B 部分的に反射光の色調変化がわずかに認められる
C 部分的に反射光の色調変化が認められる
D 全体的に反射光の色調変化が認められる
E 全体的に反射光の大きな色調変化が認められる
すじ故障
長時間連続的に製膜したサンプルについて、すじ状のむらの有無を目視で評価した。
◎ すじ状のむらは確認できない。
○ わずかにすじ状の故障が認められる。
△ 弱いすじ状の故障が認められる。
× 明らかにすじ状故障が認められる。
【0358】
また、クラック、スチールウール及び総合評価については、
◎ 十分安定している
○ 実用上安定している
△ やや不安定
× 実用不可
とした。
【0359】
【発明の効果】
基材シートの片方の面に、各々の膜厚が0.5μm以上の少なくとも2層からなる活性線硬化樹脂層を有し、少なくとも下層の活性線硬化樹脂層は可塑剤を含有し、上層の活性線硬化樹脂層の上に直接又は他の層を介して主に窒素を含有する大気圧近傍のガス雰囲気下でプラズマ処理によって形成された金属化合物層を有する本発明の光学フィルムは、高温高湿条件下、サイクル処理または長時間処理をおこなっても安定した優れた耐久性能を持ち、低反射率で色むらの低減された性能を示した。また、その光学フィルムを用いて高温高湿条件下でも安定な偏光板、画像表示装置も提供出来るようになった。
【図面の簡単な説明】
【図1】3層構造の基材シートの断面を模式的に示したものである。
【図2】共流延ダイ及び流延して多層構造ウェブ(流延直後はウェブをドープ膜ともいう)を形成したところを表した図である。
【図3】逐次流延ダイ及び流延された多層構造のウェブを表した図である。
【図4】別のタイプの共流延ダイの断面を示した図である。
【図5】溶液流延製膜装置のドープ調製工程を示した図である。
【図6】溶液流延製膜装置の流延工程から乾燥工程までを模式的に示した図である。
【図7】2層構造及び単層構造の基材シートの上に2つのハードコート層を配した光学フィルムの断面を模式的に示したものである。
【図8】基材シートの上に2つのハードコート層を塗設する塗布装置の模式図である。
【図9】本発明に有用なジェット方式の大気圧プラズマ放電処理装置の一例を示した概略図である。
【図10】本発明に有用な対向電極間で基材を処理する方式の大気圧プラズマ放電処理装置の一例を示す概略図である。
【図11】図10に示したロール回転電極の導電性の金属質母材とその上に被覆されている誘電体の構造の一例を示す斜視図である。
【図12】角筒型電極の導電性の金属質母材とその上に被覆されている誘電体の構造の一例を示す斜視図である。
【符号の説明】
10 共流延ダイ
11 口金部分
13、15 表層用スリット
14 基層用スリット
16 金属支持体
17、19 表層用ドープ
18 基層用ドープ
20 多層構造ウェブ
21,23 表層
22 基層
100 セルロースエステル溶液
101 溶解釜
102、105、112、115 送液ポンプ
103 濾過器
104、114 ストックタンク
106、113、116 濾過器
108、117 導管
110 インライン添加液
120 合流管
121 混合機
200 共流延ダイ
201、202、203 導入口
204 金属支持体
205 剥離位置
206 ウェブ
207 テンター装置
208 ロール乾燥装置
210 セルロースエステルフィルム
311 第1電極
312 第2電極
325,326 高周波プローブ
330 プラズマ放電処理装置
401,402 押し出し式塗布装置
403,404 紫外線照射装置
F 基材シート[0001]
TECHNICAL FIELD OF THE INVENTION
The present invention relates to an optical film in which a plurality of hard coat layers are provided on a plastic film, in particular, a cellulose ester film, and a metal compound thin film is formed thereon by plasma treatment under atmospheric pressure or a pressure in the vicinity thereof, and a method for producing the same. Further, the present invention relates to a polarizing plate and a display device produced from these optical films.
[0002]
[Prior art]
In recent years, liquid crystal displays, plasma displays, organic ELs, and the like used for personal computers, word processors, watches, calculators, and the like have been increasingly used in harsh environments. Therefore, a polarizing plate, a protective film for a polarizing plate, a retardation film, an antireflection film, an antistatic film, a transparent conductive film, a front conductive filter for a plasma display panel, an inorganic EL panel or an organic EL panel used for a display device such as a liquid crystal display. Also for optical films such as front films for use, it is naturally required that the characteristics do not change even under severe environments, for example, durability such as no deterioration under high temperature and high humidity and excellent dimensional stability. .
[0003]
Conventionally, a method for forming such a highly functional thin film is a coating film curing method represented by coating, or a dry thin film forming method using a vacuum such as a sputtering method, a vacuum deposition method, or an ion plating method. Was made by
[0004]
The dry thin film formation method using vacuum is a preferable method for forming a high-performance thin film because a high-precision thin film can be formed. However, the vacuum device used for the dry thin film formation method, when the substrate to be processed is large, the device becomes extremely large, the price becomes expensive, and enormous time is spent on vacuum evacuation, so that productivity cannot be increased. Demerits are great.
[0005]
As a method of overcoming the disadvantage of low productivity by using a vacuum device, as a method of discharging under an atmospheric pressure or a pressure close to the atmospheric pressure, exciting a reactive gas by plasma, and forming a thin film on a substrate, The atmospheric pressure plasma method is known.
[0006]
Conventionally, cellulose triacetate (hereinafter sometimes abbreviated as TAC) film has been used as a substrate on which a high-performance thin film is mounted because of its advantages such as good light transmittance and small birefringence. Was.
[0007]
On the other hand, a polarizing plate used for a display device is made by laminating a polarizing film protective film, which is a TAC film, with a polarizing film. And the durability due to exposure to high temperature and high humidity inside the vehicle as in car navigation. Further, a similar deterioration phenomenon over time is observed in a display device which is generally used. Accordingly, the protective film for a polarizing plate is naturally required to have good moisture resistance and heat resistance such as not deteriorating under high temperature and high humidity and excellent in dimensional stability. In the protective film for a polarizing plate of a TAC film, a plasticizer such as a phosphate ester is contained in the TAC film in order to impart appropriate flexibility to the film. However, when a polarizing plate using such a polarizing plate protective film is used under high temperature and high humidity, cracks may occur in the thin film, the polarizing plate protective film may be peeled off from the polarizing film, or the polarizing plate protective film may be used. Problems such as coloring of the film may occur.
[0008]
An optical film in which a high-performance thin film is added to such a TAC film is also affected by some effect, and the thin film often deteriorates with time.
[0009]
Among them, Patent Literature 1 discloses a technique in which atmospheric pressure plasma treatment is performed on triacetyl cellulose by atmospheric pressure plasma by applying two frequencies.
[0010]
Here, a method of generating a pulse plasma in which a stable discharge state is realized by applying a high-frequency AC pulse wave using a high-frequency power supply under atmospheric pressure conditions has been proposed.
[0011]
This is a method in which a glow discharge is generated by placing a solid dielectric on at least one opposing surface of an opposing electrode under a pressure near atmospheric pressure and applying a pulsed electric field between the opposing electrodes. A glow discharge plasma generation method characterized in that a plasma is generated by applying a high-frequency AC pulse wave, and in particular, a high-frequency AC pulse wave is applied at the start of a discharge, and then a high-frequency AC pulse wave is applied. Although this is a method of generating discharge plasma, the obtained optical film cannot be sufficiently stabilized due to durability and the like.
[0012]
Patent Literature 2 also discloses a method of performing atmospheric pressure plasma treatment on triacetyl cellulose. A thin film is continuously formed on a surface of a film substrate having hygroscopicity such as TAC by using normal pressure plasma. In forming the base film, wrinkles are prevented from being generated in the base film, but it is not sufficient.
[0013]
That is, under a pressure close to the atmospheric pressure, a discharge plasma is generated by applying a pulse voltage between the opposed electrodes while passing the film base F between the opposed electrodes, and the discharge plasma is generated using the discharged plasma. In the method of continuously forming a thin film on the surface of the semiconductor device, the electric field strength between the opposing electrodes is 1 in a gas atmosphere comprising 0.01 to 5% by volume of a metal element-containing alkoxide and 50 to 99.99% by volume of argon gas. By applying a pulse voltage so as to be ~ 90 kV / cm to form a thin film, and controlling the temperature of the film substrate F during the film formation to 100 ° C or less, the film substrate in the plasma discharge space is formed. Although fluctuations in temperature (moisture content) are suppressed, a sufficient effect has not been obtained.
[0014]
Further, Patent Document 3 discloses that a metal compound layer is formed by an atmospheric pressure plasma treatment, and describes that atmospheric pressure plasma mainly containing nitrogen is used for the metal compound layer.
[0015]
Patent Document 4 discloses a plastic film in which a hard coat composed of two layers is applied.
[0016]
[Patent Document 1]
JP 2002-110397 A
[0017]
[Patent Document 2]
JP 2002-26632 A
[0018]
[Patent Document 3]
JP-A-11-181573
[0019]
[Patent Document 4]
JP 2000-52472 A
[0020]
[Problems to be solved by the invention]
As described above, the atmospheric pressure plasma treatment can form a functional film at a lower cost than a method using a vacuum process. However, if a rare gas such as helium is used as a reaction gas, the merit that the cost can be reduced is lost. For this reason, a plasma treatment method in a nitrogen atmosphere has been proposed. However, plasma treatment in a nitrogen atmosphere is less likely to cause a stable plasma discharge than helium, resulting in poor film quality. It is difficult to obtain a stable film, and a streak-like failure is liable to occur.
[0021]
The present invention is intended to reduce such streak-like failures and to propose an optical film having a uniform metal compound layer and a method of manufacturing the optical film. Provides an optical film with excellent durability and a uniform metal compound layer formed, especially an optical film with reduced color unevenness of reflected light, and enables significant cost reduction without the need for a vacuum process It is an object of the present invention to establish a manufacturing method described above and to provide a polarizing plate and a display device using such an optical film.
[0022]
[Means for Solving the Problems]
This object is achieved by any of the following technical means (1) to (7).
[0023]
(1) At least one surface of a plastic substrate sheet has at least two active ray-curable resin layers each having a thickness of 0.5 μm or more, and at least a lower active ray-curable resin layer contains a plasticizer. It has a metal compound layer formed by a plasma treatment under a gas atmosphere near the atmospheric pressure containing nitrogen mainly directly or through another layer on the upper active ray curable resin layer. Optical film.
[0024]
(2) The optical film according to (1), wherein the optical film contains a compound having three or more aromatic rings in a molecule.
[0025]
(3) At least one surface of the plastic base sheet is formed with an active ray-curable resin layer having the performance of at least two hard coat layers each having a thickness of 0.5 μm or more, and further directly thereon. Alternatively, a method for producing an optical film, characterized in that a metal compound layer is formed by plasma treatment under a gas atmosphere near atmospheric pressure mainly containing nitrogen via another layer.
[0026]
(4) A gas containing nitrogen as a main component is supplied between at least two electrodes facing each other in the plasma processing, and a high-frequency voltage is applied between the first electrode and the second electrode to thereby form the gas. And exposing the substrate sheet on which the active ray-curable resin layer is applied to the excited gas to form a metal compound layer on the active ray-curable resin layer applied to the substrate sheet. , The high frequency voltage has a first frequency ω1And the first frequency ω1Higher second frequency ω2The method for producing an optical film according to the item (3), comprising:
[0027]
(5) After forming an actinic ray-curable resin layer containing a plasticizer as the hard coat layer, a second actinic ray-curable resin layer is provided without winding, and further directly or through another layer. The optical film according to (3) or (4), wherein two or more metal compound layers are continuously formed by a plasma treatment in a gas atmosphere near the atmospheric pressure mainly containing nitrogen. Production method.
[0028]
(6) A polarizing plate comprising the optical film according to (1) or (2).
[0029]
(7) A display device comprising (1) the optical film according to item (2).
[0030]
Hereinafter, the present invention will be described in more detail.
Examples of the plastic base sheet used in the present invention include polyester such as polyethylene terephthalate, polycarbonate, cyclic polyolefin, polysulfone, polyacrylate, cellulose ester, norbornene-based resin (for example, Arton (manufactured by JSR), Zeonex, Zeonoa (Nihon Zeon) And the like, but not particularly limited thereto. Among them, cellulose esters (for example, KC4UX2MW, KC8UX2MW, KC8UN, KC5UN, KC4UY, KC12UR manufactured by Konica Corporation) are preferably used.
[0031]
In the following description, the base sheet is formed using cellulose ester.
In the present invention, as described below, the dope preparation step is divided into a cellulose ester solution preparation step and an in-line additive liquid preparation step, and it is preferable to combine and mix these in-line to prepare a dope. Therefore, in the present invention, a dope in a state of being introduced into a casting die described below is referred to as a dope, that is, a liquid before the merging, that is, a liquid containing a cellulose ester serving as a substrate is a cellulose ester solution, a plasticizer or UV. A liquid containing fine particles such as an agent and a matting agent is referred to as an in-line additive liquid.
[0032]
[Film of base sheet]
One example of the base sheet F used in the present invention is one in which the layer structure of the cellulose ester film has one base layer and is most commonly used, and another example has a multilayer structure, and has one layer structure. It may have a base layer and at least one surface layer, the number of layers may be two or more, and one formed surface layer or base layer may be composed of a plurality of layers.
[0033]
FIG. 1 (a) schematically shows a cross section of a film having a single-layer structure, and FIG. 1 (b) schematically shows a cross section of a film having a three-layer structure. In the drawings, 21 and 23 indicate surface layers and 22 indicates a base layer. .
[0034]
(Co-casting and sequential casting)
The cellulose ester film having a multilayer structure used in the present invention is obtained by laminating a dope in multiple layers by co-casting or sequential casting in a solution casting film forming process.
[0035]
FIG. 2 is a view showing a co-casting die and a state where a multilayer structure web is formed by casting (the web may be also referred to as a doped film immediately after casting). In the co-casting, as shown in FIG. 2, a plurality of (three in FIG. 2) surface slits 13 and 15 and a base layer slit 14 are provided in a base portion 11 of a co-casting die 10, and a metal support is provided. A dope 17 for the surface layer, a dope 18 for the base layer, and a dope 19 for the surface layer are simultaneously cast from the respective slits onto the web 16 to form a web as a base material sheet F having a multilayer structure of the surface layer 21 / base layer 22 / surface layer 23. 20 are formed.
[0036]
FIG. 3 is a view showing a sequential casting die and a web having a multilayer structure that has been cast. In the sequential casting, as shown in FIG. 3, a plurality (three in FIG. 3) of the surface casting dies 30, the base layer dies 31, and the surface casting dies 32 are placed in different places above the metal support 16. First, a surface dope 33 as one surface layer is cast from the surface die 30 to form a surface dope film 36 on the metal support 16, and then a base layer dope 34 is A base layer dope film 37 is formed on the surface layer dope film 36 from 31, and a surface dope 35 is cast from the next surface die 32 to form a surface dope film 38, thereby forming a surface layer / base layer / surface layer. A multi-layered web 39 is formed as the base sheet F to be formed.
[0037]
FIG. 4 is a diagram showing a cross section of another type of co-casting die. In the co-casting die 50 where three layers join in the main body, a base layer dope 56 and surface dopes 55 and 57 are introduced into a base layer slit 52 and surface layer slits 51 and 53, respectively. Are joined at the joining slit 58, form a laminar flow, pass through the slit 54, and are cast on the metal support 16 in three layers of surface layer / base layer / surface layer.
[0038]
Preferably, the surface layer of the multi-layered web as shown in FIGS. 2, 3 and 4 is wider than the base layer, and the base web is cast so that the surface web wraps around.
[0039]
In addition, in order to produce a substrate sheet having a single-layer structure, only one layer can be cast using any one slit in the die to produce a substrate sheet.
[0040]
(Solution casting method)
The cellulose ester film of the present invention is formed by a solution casting method. Here, the solution casting film forming method according to the present invention will be described with reference to FIG.
[0041]
FIG. 5 is a diagram schematically showing a dope preparation step and a casting step of the solution casting film forming apparatus according to the present invention. In the following steps, typical steps will be described by taking two-layer co-casting as an example.
[0042]
(1) Cellulose ester solution preparation step:
This is a step of forming a cellulose ester solution 100 by dissolving additives such as a cellulose ester and a plasticizer in a dissolving vessel 101 with stirring in an organic solvent mainly containing a good solvent for the cellulose ester described below. Dissolution is carried out at normal pressure, below the boiling point of the main solvent, at high temperature above the boiling point of the main solvent, at high temperature, at high temperature, at cooling, and at high pressure. Although there are various dissolution methods, a high-temperature dissolution method is preferably used in the present invention. After dissolution, the cellulose ester solution 100 is filtered by a liquid sending pump 102 with a filter 103 (filter press type), left in a stock tank 104 for defoaming, and a liquid sending pump 105 (pressure type fixed gear pump) for casting. The solution is transported by a conduit 108 so as to be mixed with an in-line additive liquid 110 such as a matting agent dispersion liquid or an ultraviolet absorbent additive liquid via a filter 106. When the dope used in the base layer or the surface layer does not contain an additive such as a matting agent or an ultraviolet absorber, it is directly sent to a casting die after passing through the filter 106.
[0043]
For filtration, the cellulose ester solution is filtered using a suitable filter medium such as filter paper for a filter press. As the filtering material in the present invention, it is preferable that the absolute filtering accuracy is small in order to remove insolubles and the like, but if the absolute filtering accuracy is too small, there is a problem that clogging of the filtering material is likely to occur. A filter medium having an accuracy of 8 μm or less is preferable, a filter medium in a range of 1 to 8 μm is more preferable, and a filter medium in a range of 3 to 6 μm is further preferable. As the filter paper, for example, the commercially available product No. No. of Azumi Filter Paper Co., Ltd. 244, 277 and the like can be mentioned, and are preferably used. The material of the filter medium for the further filtration is not particularly limited, and a normal filter medium can be used. However, a filter medium made of plastic such as polypropylene or Teflon (R) or a metal filter medium such as stainless steel may cause fibers to fall off. Preferred. Filtration can be carried out by a usual method, but a method of filtering under heating, while heating or keeping at a temperature not lower than the boiling point of the organic solvent to be used at normal pressure and at a temperature in which the organic solvent does not boil, is a filtration material. The increase in the differential pressure before and after (hereinafter sometimes referred to as filtration pressure) is small, which is preferable. The preferred temperature range depends on the organic solvent used, but is preferably 45 to 120 ° C, more preferably 45 to 70 ° C, and still more preferably 45 to 55 ° C. The smaller the filtration pressure is, the more preferably it is 0.3 to 1.6 MPa, more preferably it is 0.3 to 1.2 MPa, and even more preferably it is 0.3 to 1.0 MPa. Note that an ultraviolet absorber may be added to the cellulose ester solution in the melting vessel 101 in advance.
[0044]
As the compound having three or more aromatic rings in the molecule, a compound having a triphenylene ring or a 1,3,5-triazine compound shown in the following chemical formula 1 is preferable.
[0045]
Embedded image
Figure 2004203009
[0046]
One of the specific examples of the additive is a compound having a triphenylene ring, and among them, a compound represented by the following general formula (I) is preferable.
[0047]
Embedded image
Figure 2004203009
[0048]
In the general formula (I), R1, R2, R3, R4, R5And R6Is a hydrogen atom, a halogen atom, nitro, sulfo, aliphatic group, aromatic group, heterocyclic group, -OR11, -SR12, -CO-RThirteen, -O-CO-R14, -CO-ORFifteen, -O-CO-OR16, -NR17R18, -CO-NR19R20, -NR21-CO-R22, -O-CO-NR23R24, -SiR25R26R27, -O-SiR28R29R30, -S-CO-R31, -O-SO2-R32, -SO-R33, -NR34-CO-OR35, -SO2-R36Or -NR37-CO-NR38R39,
R11, R12, RThirteen, R14, RFifteen, R16, R17, R18, R19, R20, R21, R22, R23, R24, R25, R26, R27, R28, R29, R30, R31, R32, R33, R34, R35, R36, R37, R38And R39Is a hydrogen atom, an aliphatic group, an aromatic group or a heterocyclic group. Also, R1And R2, R3And R4Or R5And R6May combine with each other to form a ring.
[0049]
R1, R2, R3, R4, R5And R6Is -OR11, -SR12, -O-CO-R14, -O-CO-OR16, -NR17R18, -NR21-CO-R22Or -O-CO-NR23R24Preferably, -OR11, -SR12, -O-CO-R14, -O-CO-OR16Or -O-CO-NR23R24And more preferably -OR.11Or -O-CO-R14More preferably, -O-CO-R14Is most preferred.
[0050]
R11, R12, RThirteen, R14, RFifteen, R16, R17, R18, R19, R20, R21, R22, R23, R24, R25, R26, R27, R28, R29, R30, R31, R32, R33, R34, R35, R36, R37, R38And R39Is preferably a hydrogen atom, an aliphatic group or an aromatic group. -O-CO-R14R14Is most preferably an aromatic group.
[0051]
In the general formula (I), R1, R2, R3, R4, R5And R6Are preferably the same group.
[0052]
Examples of the aliphatic group include an alkyl group, an alkenyl group, an alkynyl group, a substituted alkyl group, a substituted alkenyl group and a substituted alkynyl group.
[0053]
The alkyl group may be cyclic (for example, a cycloalkyl group or the like), and the alkyl group may be branched. The alkyl group preferably has 1 to 30 carbon atoms, more preferably 1 to 20 carbon atoms, and most preferably 1 to 10 carbon atoms.
[0054]
Specific examples of the alkyl group include groups such as methyl, ethyl, i-propyl, butyl, i-butyl, s-butyl, t-butyl, t-pentyl, hexyl, octyl, t-octyl, dodecyl, and tetracosyl Is mentioned.
[0055]
The alkenyl group may be cyclic (cycloalkenyl group), and the alkenyl group may be branched. Further, the alkenyl group may have two or more double bonds.
[0056]
The alkenyl group preferably has 2 to 30 carbon atoms, more preferably 2 to 20 carbon atoms, and most preferably 2 to 10 carbon atoms.
[0057]
Specific examples of the alkenyl group include vinyl, allyl and 3-heptenyl. The alkynyl group may be cyclic (cycloalkynyl group), and the alkynyl group may have a branch.
[0058]
Further, the alkynyl group may have two or more triple bonds. The alkynyl group preferably has 2 to 30 carbon atoms, more preferably 2 to 20 carbon atoms, and most preferably 2 to 10 carbon atoms.
[0059]
Specific examples of the alkynyl group include groups such as ethynyl, 2-propynyl, 1-pentynyl, and 2,4-octadynyl.
[0060]
Specific examples of the substituent of the substituted alkyl group, the substituted alkenyl group and the substituted alkynyl group include, for example, a halogen atom, nitro, sulfo, aromatic group, heterocyclic group, -OR.41, -SR42, -CO-R43, -O-CO-R44, -CO-OR45, -O-CO-OR46, -NR47R48, -CO-NR49R50, -NR51-CO-R52, -O-CO-NR53R54, -SiR55R56R57R58Or -O-SiR59R60R61R62And the like.
[0061]
R41, R42, R43, R44, R45, R46, R47, R48, R49, R50, R51, R52, R53, R54, R55, R56, R57, R58, R59, R60, R61Or R62Is a hydrogen atom, an aliphatic group, an aromatic group or a heterocyclic group. The alkyl part of the substituted alkyl group is the same as the above-mentioned alkyl group.
[0062]
Specific examples of the substituted alkyl group include benzyl, phenethyl, 2-methoxyethyl, ethoxymethyl, 2- (2-methoxyethoxy) ethyl, 2-hydroxyethyl, hydroxymethyl, 2-carboxyethyl, carboxymethyl, ethoxycarbonylmethyl , 4-acryloyloxybutyl, trichloromethyl or perfluoropentyl. The alkenyl part of the substituted alkenyl group is the same as the above alkenyl group. Specific examples of the substituted alkenyl group include, for example, styryl and 4-methoxystyryl.
[0063]
The alkynyl part of the substituted alkynyl group is the same as the above alkynyl group. Specific examples of the substituted alkynyl group include groups such as 4-butoxyphenylethynyl, 4-propylphenylethynyl, and trimethylsilylethynyl.
[0064]
In the present invention, the aromatic group means an aryl group and a substituted aryl group.
The number of carbon atoms of the aryl group is preferably from 6 to 30, more preferably from 6 to 20, and most preferably from 6 to 10.
[0065]
Specific examples of the aryl group include, for example, phenyl, 1-naphthyl and 2-naphthyl.
[0066]
Specific examples of the substituent of the substituted aryl group include, for example, a halogen atom, a nitro group, a sulfo group, an aliphatic group, an aromatic group, a heterocyclic group, -OR.71, -SR72, -CO-R73, -O-CO-R74, -CO-OR75, -O-CO-OR76, -NR77R78, -CO-NR79R80, -NR81-CO-R82, -O-CO-NR83R84, -SiR85R86R87R88Or -O-SiR89R90R91R92And the like.
[0067]
R71, R72, R73, R74, R75, R76, R77, R78, R79, R80, R81, R82, R83, R84, R85, R86, R87, R88, R89, R90, R91And R92Is a hydrogen atom, an aliphatic group, an aromatic group or a heterocyclic group.
[0068]
The aryl part of the substituted aryl group has the same meaning as the above aryl group.
Specific examples of the substituted aryl group include p-biphenylyl, 4-phenylethynylphenyl, 2-methoxyphenyl, 3-methoxyphenyl, 4-methoxyphenyl, 2-ethoxyphenyl, 3-ethoxyphenyl, 4-ethoxyphenyl, -Propoxyphenyl, 3-propoxyphenyl, 4-propoxyphenyl, 2-butoxyphenyl, 3-butoxyphenyl, 4-butoxyphenyl, 2-hexyloxyphenyl, 3-hexyloxyphenyl, 4-hexyloxyphenyl, 2-octyl Oxyphenyl, 3-octyloxyphenyl, 4-octyloxyphenyl, 2-dodecyloxyphenyl, 3-dodecyloxyphenyl, 4-dodecyloxyphenyl, 2-tetracosyloxyphenyl, 3-tetracosyloxyphenyl, -Tetracosyloxyphenyl, 3,4-dimethoxyphenyl, 3,4-diethoxyphenyl, 3,4-dihexyloxyphenyl, 2,4-dimethoxyphenyl, 2,4-diethoxyphenyl, 2,4-dihexyl Oxyphenyl, 3,5-dimethoxyphenyl, 3,5-dimethoxyphenyl, 3,5-dihexyloxyphenyl, 3,4,5-trimethoxyphenyl, 3,4,5-triethoxyphenyl, 3,4,5 -Trihexyloxyphenyl, 2,4,6-trimethoxyphenyl, 2,4,6-triethoxyphenyl, 2,4,6-trihexyloxyphenyl, 2-fluorophenyl, 3-fluorophenyl, 4-fluoro Phenyl, 2-chlorophenyl, 3-chlorophenyl, 4-chlorophenyl, 2-bromophenyl, 3 Bromophenyl, 4-bromophenyl, 3,4-difluorophenyl, 3,4-dichlorophenyl, 3,4-dibromophenyl, 2,4-difluorophenyl, 2,4-dichlorophenyl, 2,4-dibromophenyl, 3, 5-difluorophenyl, 3,5-dichlorophenyl, 3,5-dibromophenyl, 3,4,5-trifluorophenyl, 3,4,5-trichlorophenyl, 3,4,5-tribromophenyl, 2,4 , 6-Trifluorophenyl, 2,4,6-trichlorophenyl, 2,4,6-tribromophenyl, pentafluorophenyl, pentachlorophenyl, pentabromophenyl, 2-iodophenyl, 3-iodophenyl, 4-iodo Phenyl, 2-formylphenyl, 3-formylphenyl, 4-formylphenyl, 2-benzoylphenyl, 3-benzoylphenyl, 4-benzoylphenyl, 2-carboxyphenyl, 3-carboxyphenyl, 4-carboxyphenyl, o-tolyl, m-tolyl, p-tolyl, 2-ethylphenyl, 3-ethyl Phenyl, 4-ethylphenyl, 2- (2-methoxyethoxy) phenyl, 3- (2-methoxyethoxy) phenyl, 4- (2-methoxyethoxy) phenyl, 2-ethoxycarbonylphenyl, 3-ethoxycarbonylphenyl, -Ethoxycarbonylphenyl, 2-benzoyloxyphenyl, 3-benzoyloxyphenyl, 4-benzoyloxyphenyl and the like.
[0069]
In the present invention, the heterocyclic group may have a substituent. The heterocycle in the heterocyclic group is preferably a 5- or 6-membered ring. An aliphatic ring, an aromatic ring, or another heterocyclic ring may be condensed to the heterocyclic ring in the heterocyclic group. Examples of the hetero atom in the heterocyclic ring include atoms such as B, N, O, S, Se, and Te.
[0070]
Specific examples of the heterocyclic ring in the heterocyclic group include, for example, a pyrrolidine ring, a morpholine ring, a 2-bora-1,3-dioxolane ring, and a 1,3-thiazolidine ring.
[0071]
Specific examples of the unsaturated heterocyclic ring in the unsaturated heterocyclic group, for example, imidazole ring, thiazole ring, benzothiazole ring, benzoxazole ring, benzotriazole ring, benzoselenazole ring, pyridine ring, pyrimidine ring or quinoline ring And the like.
[0072]
Specific examples of the substituent of the heterocyclic group are the same as the specific examples of the substituent of the substituted aryl group.
[0073]
The molecular weight of the compound having a triphenylene ring is preferably from 300 to 2,000. The boiling point of the compound is preferably 260 ° C. or higher. The boiling point can be measured using a commercially available measuring device (for example, TG / DTA100, manufactured by Seiko Instruments Inc.). Hereinafter, specific examples of the compound having a triphenylene ring will be described.
[0074]
In addition, a plurality of Rs shown below mean the same group.
[0075]
Embedded image
Figure 2004203009
[0076]
(1) Fluoro
(2) Chloro
(3) Bromo
(4) Formyl
(5) Benzoyl
(6) carboxyl
(7) Butylamino
(8) Dibenzylamino
(9) Trimethylsilyloxy
(10) 1-pentynyl
(11) ethoxycarbonyl
(12) 2-hydroxyethoxycarbonyl
(13) phenoxycarbonyl
(14) N-phenylcarbamoyl
(15) N, N-diethylcarbamoyl
(16) 4-methoxybenzoyloxy
(17) N-phenylcarbamoyloxy
(18) Hexyloxy
(19) 4-hexyloxybenzoyloxy
(20) Ethoxy
(21) Benzoyloxy
(22) m-dodecyloxyphenylthio
(23) t-octylthio
(24) p-fluorobenzoylthio
(25) isobutyrylthio
(26) p-methylbenzenesulfinyl
(27) ethanesulfinyl
(28) benzenesulfonyl
(29) Methanesulfonyl
(30) 2-methoxyethoxy
(31) Propoxy
(32) 2-hydroxyethoxy
(33) 2-carboxyethoxy
(34) 3-heptenyloxy
(35) 2-phenylethoxy
(36) Trichloromethoxy
(37) 2-propynyloxy
(38) 2,4-octadiynyloxy
(39) Perfluoropentyloxy
(40) ethoxycarbonylmethoxy
(41) p-methoxyphenoxy
(42) m-ethoxyphenoxy
(43) o-chlorophenoxy
(44) m-dodecyloxyphenoxy
(45) 4-pyridyloxy
(46) Pentafluorobenzoyloxy
(47) p-hexyloxybenzoyloxy
(48) 1-naphthoyloxy
(49) 2-Naphthoyloxy
(50) 5-imidazolecarbonyloxy
(51) o-phenoxycarbonylbenzoyloxy
(52) m- (2-methoxyethoxy) benzoyloxy
(53) o-carboxybenzoyloxy
(54) p-formylbenzoyloxy
(55) m-ethoxycarbonylbenzoyloxy
(56) p-pivaloylbenzoyloxy
(57) propionyloxy
(58) phenylacetoxy
(59) Cinnamoyloxy
(60) hydroxyacetoxy
(61) ethoxycarbonylacetoxy
(62) m-butoxyphenylpropioyloxy
(63) Propioloyloxy
(64) trimethylsilylpropioyloxy
(65) 4-octenoyloxy
(66) 3-hydroxypropionyloxy
(67) 2-methoxyethoxyacetoxy
(68) Perfluorobutyryloxy
(69) methanesulfonyloxy
(70) p-toluenesulfonyloxy
(71) Triethylsilyl
(72) m-butoxyphenoxycarbonylamino
(73) Hexyl
(74) phenyl
(75) 4-pyridyl
(76) benzyloxycarbonyloxy
(77) m-chlorobenzamide
(78) 4-methylanilino
[0077]
Embedded image
Figure 2004203009
[0078]
(79) Nitro
(80) Sulfo
(81) Formyl
(82) carboxyl
(83) methoxycarbonyl
(84) benzyloxycarbonyl
(85) phenoxycarbonyl
[0079]
Embedded image
Figure 2004203009
[0080]
(86) Butoxy
(87) Hexyloxy
(88) Dodecyloxy
(89) Hexanoyloxy
(90) Carboxymethoxy
[0081]
Embedded image
Figure 2004203009
[0082]
Embedded image
Figure 2004203009
[0083]
Embedded image
Figure 2004203009
[0084]
Embedded image
Figure 2004203009
[0085]
Embedded image
Figure 2004203009
[0086]
Embedded image
Figure 2004203009
[0087]
As the discotic compound, a compound having a 1,3,5-triazine ring or a compound having a porphyrin skeleton can be preferably used.
[0088]
Among the compounds having a 1,3,5-triazine ring, a compound represented by the following general formula (III) is preferable.
[0089]
Embedded image
Figure 2004203009
[0090]
In the general formula (III), X1Is a single bond, -NR4-, -O- or -S-; X2Is a single bond, -NR5-, -O- or -S-; X3Is a single bond, -NR6-, -O- or -S-; R1, R2And R3Is an alkyl, alkenyl, aryl or heterocyclic group; and R4, R5And R6Is a hydrogen atom, an alkyl group, an alkenyl group, an aryl group or a heterocyclic group. The compound represented by the general formula (I) is particularly preferably a melamine compound.
[0091]
In the melamine compound, in the general formula (I), X1, X2And X3Are respectively -NR4-, -NR5-And -NR6-Or X1, X2And X3Is a single bond, and R1, R2And R3Is a heterocyclic group having a free valence at the nitrogen atom. -X1-R1, -X2-R2And -X3-R3Are preferably the same substituent. R1, R2And R3Is particularly preferably an aryl group. R4, R5And R6Is particularly preferably a hydrogen atom.
[0092]
The alkyl group is preferably a chain alkyl group rather than a cyclic alkyl group. A linear alkyl group is more preferable than a branched alkyl group.
[0093]
The number of carbon atoms of the alkyl group is preferably 1 to 30, more preferably 1 to 20, still more preferably 1 to 10, further preferably 1 to 8, and 1 to 8. Most preferably, it is 6. The alkyl group may have a substituent.
[0094]
Specific examples of the substituent include a halogen atom, an alkoxy group (for example, each group such as methoxy, ethoxy, and epoxyethyloxy) and an acyloxy group (for example, acryloyloxy and methacryloyloxy). The alkenyl group is preferably a chain alkenyl group rather than a cyclic alkenyl group. A linear alkenyl group is preferable to a branched alkenyl group. The number of carbon atoms of the alkenyl group is preferably 2 to 30, more preferably 2 to 20, still more preferably 2 to 10, further preferably 2 to 8, and 2 to 8. Most preferably, it is 6. The alkenyl group may have a substituent.
[0095]
Specific examples of the substituent include a halogen atom, an alkoxy group (for example, each group such as methoxy, ethoxy, and epoxyethyloxy) and an acyloxy group (for example, each group such as acryloyloxy and methacryloyloxy).
[0096]
The aryl group is preferably a phenyl group or a naphthyl group, and particularly preferably a phenyl group. The aryl group may have a substituent.
[0097]
Specific examples of the substituent include, for example, halogen atom, hydroxyl, cyano, nitro, carboxyl, alkyl group, alkenyl group, aryl group, alkoxy group, alkenyloxy group, aryloxy group, acyloxy group, alkoxycarbonyl group, alkenyloxy Carbonyl group, aryloxycarbonyl group, sulfamoyl, alkyl-substituted sulfamoyl group, alkenyl-substituted sulfamoyl group, aryl-substituted sulfamoyl group, sulfonamide group, carbamoyl, alkyl-substituted carmoyl group, alkenyl-substituted carbamoyl group, aryl-substituted carbamoyl group, amide group, alkylthio And alkenylthio, arylthio and acyl groups. The alkyl group has the same meaning as the above-described alkyl group.
[0098]
The alkyl group of an alkoxy group, an acyloxy group, an alkoxycarbonyl group, an alkyl-substituted sulfamoyl group, a sulfonamide group, an alkyl-substituted carbamoyl group, an amide group, an alkylthio group and an acyl group have the same meaning as the above-mentioned alkyl group.
[0099]
The alkenyl group has the same meaning as the above-described alkenyl group.
The alkenyl group of the alkenyloxy group, the acyloxy group, the alkenyloxycarbonyl group, the alkenyl-substituted sulfamoyl group, the sulfonamide group, the alkenyl-substituted carbamoyl group, the amide group, the alkenylthio group and the acyl group is also the same as the above-mentioned alkenyl group.
[0100]
Specific examples of the aryl group include, for example, phenyl, α-naphthyl, β-naphthyl, 4-methoxyphenyl, 3,4-diethoxyphenyl, 4-octyloxyphenyl, and 4-dodecyloxyphenyl. No.
[0101]
Examples of the aryloxy group, acyloxy group, aryloxycarbonyl group, aryl-substituted sulfamoyl group, sulfonamide group, aryl-substituted carbamoyl group, amide group, arylthio group and acyl group are the same as the above-mentioned aryl group.
[0102]
X1, X2Or X3Is preferably -NR-, -O- or -S-, the heterocyclic group preferably has aromaticity.
[0103]
The heterocyclic ring in the heterocyclic group having aromaticity is generally an unsaturated heterocyclic ring, preferably a heterocyclic ring having the largest number of double bonds. The heterocycle is preferably a 5-, 6- or 7-membered ring, more preferably a 5- or 6-membered ring, and most preferably a 6-membered ring.
[0104]
The hetero atom in the heterocyclic ring is preferably each atom such as N, S or O, and particularly preferably N atom.
[0105]
As the heterocyclic ring having aromaticity, a pyridine ring (each group such as 2-pyridyl or 4-pyridyl) is particularly preferable. The heterocyclic group may have a substituent. Examples of the substituent of the heterocyclic group are the same as the examples of the substituent of the aryl moiety.
[0106]
X1, X2Or X3When is a single bond, the heterocyclic group is preferably a heterocyclic group having a free valence at a nitrogen atom. The heterocyclic group having a free valence at the nitrogen atom is preferably a 5-, 6-, or 7-membered ring, more preferably a 5- or 6-membered ring, and more preferably a 5-membered ring. Is most preferred. The heterocyclic group may have a plurality of nitrogen atoms.
[0107]
Further, the hetero atom in the heterocyclic group may have a hetero atom (for example, an O atom or an S atom) other than a nitrogen atom. The heterocyclic group may have a substituent. Specific examples of the substituent of the heterocyclic group are the same as the specific examples of the substituent of the aryl moiety.
[0108]
Hereinafter, specific examples of the heterocyclic group having a free valence at the nitrogen atom are shown.
[0109]
Embedded image
Figure 2004203009
[0110]
Embedded image
Figure 2004203009
[0111]
The molecular weight of the compound having a 1,3,5-triazine ring is preferably from 300 to 2,000. The boiling point of the compound is preferably 260 ° C. or higher. The boiling point can be measured using a commercially available measuring device (for example, TG / DTA100, manufactured by Seiko Instruments Inc.).
[0112]
Hereinafter, specific examples of the compound having a 1,3,5-triazine ring are shown.
Note that a plurality of Rs shown below represent the same group.
[0113]
Embedded image
Figure 2004203009
[0114]
(1) Butyl
(2) 2-methoxy-2-ethoxyethyl
(3) 5-undecenyl
(4) phenyl
(5) 4-ethoxycarbonylphenyl
(6) 4-butoxyphenyl
(7) p-biphenylyl
(8) 4-pyridyl
(9) 2-naphthyl
(10) 2-methylphenyl
(11) 3,4-dimethoxyphenyl
(12) 2-furyl
[0115]
Embedded image
Figure 2004203009
[0116]
Embedded image
Figure 2004203009
[0117]
(14) phenyl
(15) 3-ethoxycarbonylphenyl
(16) 3-butoxyphenyl
(17) m-biphenylyl
(18) 3-phenylthiophenyl
(19) 3-chlorophenyl
(20) 3-benzoylphenyl
(21) 3-acetoxyphenyl
(22) 3-benzoyloxyphenyl
(23) 3-phenoxycarbonylphenyl
(24) 3-methoxyphenyl
(25) 3-anilinophenyl
(26) 3-isobutyrylaminophenyl
(27) 3-phenoxycarbonylaminophenyl
(28) 3- (3-ethylureido) phenyl
(29) 3- (3,3-diethylureido) phenyl
(30) 3-methylphenyl
(31) 3-phenoxyphenyl
(32) 3-hydroxyphenyl
(33) 4-ethoxycarbonylphenyl
(34) 4-butoxyphenyl
(35) p-biphenylyl
(36) 4-phenylthiophenyl
(37) 4-chlorophenyl
(38) 4-benzoylphenyl
(39) 4-acetoxyphenyl
(40) 4-benzoyloxyphenyl
(41) 4-phenoxycarbonylphenyl
(42) 4-methoxyphenyl
(43) 4-anilinophenyl
(44) 4-isobutyrylaminophenyl
(45) 4-phenoxycarbonylaminophenyl
(46) 4- (3-ethylureido) phenyl
(47) 4- (3,3-diethylureido) phenyl
(48) 4-methylphenyl
(49) 4-phenoxyphenyl
(50) 4-hydroxyphenyl
(51) 3,4-diethoxycarbonylphenyl
(52) 3,4-dibutoxyphenyl
(53) 3,4-diphenylphenyl
(54) 3,4-diphenylthiophenyl
(55) 3,4-dichlorophenyl
(56) 3,4-dibenzoylphenyl
(57) 3,4-diacetoxyphenyl
(58) 3,4-dibenzoyloxyphenyl
(59) 3,4-diphenoxycarbonylphenyl
(60) 3,4-dimethoxyphenyl
(61) 3,4-dianilinophenyl
(62) 3,4-dimethylphenyl
(63) 3,4-diphenoxyphenyl
(64) 3,4-dihydroxyphenyl
(65) 2-naphthyl
(66) 3,4,5-triethoxycarbonylphenyl
(67) 3,4,5-tributoxyphenyl
(68) 3,4,5-triphenylphenyl
(69) 3,4,5-triphenylthiophenyl
(70) 3,4,5-trichlorophenyl
(71) 3,4,5-tribenzoylphenyl
(72) 3,4,5-triacetoxyphenyl
(73) 3,4,5-tribenzoyloxyphenyl
(74) 3,4,5-triphenoxycarbonylphenyl
(75) 3,4,5-trimethoxyphenyl
(76) 3,4,5-trianilinophenyl
(77) 3,4,5-trimethylphenyl
(78) 3,4,5-triphenoxyphenyl
(79) 3,4,5-trihydroxyphenyl
[0118]
Embedded image
Figure 2004203009
[0119]
(80) phenyl
(81) 3-ethoxycarbonylphenyl
(82) 3-butoxyphenyl
(83) m-biphenylyl
(84) 3-phenylthiophenyl
(85) 3-chlorophenyl
(86) 3-benzoylphenyl
(87) 3-acetoxyphenyl
(88) 3-benzoyloxyphenyl
(89) 3-phenoxycarbonylphenyl
(90) 3-methoxyphenyl
(91) 3-anilinophenyl
(92) 3-isobutyrylaminophenyl
(93) 3-phenoxycarbonylaminophenyl
(94) 3- (3-ethylureido) phenyl
(95) 3- (3,3-diethylureido) phenyl
(96) 3-methylphenyl
(97) 3-phenoxyphenyl
(98) 3-hydroxyphenyl
(99) 4-ethoxycarbonylphenyl
(100) 4-butoxyphenyl
(101) p-biphenylyl
(102) 4-phenylthiophenyl
(103) 4-chlorophenyl
(104) 4-benzoylphenyl
(105) 4-acetoxyphenyl
(106) 4-benzoyloxyphenyl
(107) 4-phenoxycarbonylphenyl
(108) 4-methoxyphenyl
(109) 4-anilinophenyl
(110) 4-isobutyrylaminophenyl
(111) 4-phenoxycarbonylaminophenyl
(112) 4- (3-ethylureido) phenyl
(113) 4- (3,3-diethylureido) phenyl
(114) 4-methylphenyl
(115) 4-phenoxyphenyl
(116) 4-hydroxyphenyl
(117) 3,4-diethoxycarbonylphenyl
(118) 3,4-dibutoxyphenyl
(119) 3,4-diphenylphenyl
(120) 3,4-diphenylthiophenyl
(121) 3,4-dichlorophenyl
(122) 3,4-dibenzoylphenyl
(123) 3,4-diacetoxyphenyl
(124) 3,4-dibenzoyloxyphenyl
(125) 3,4-diphenoxycarbonylphenyl
(126) 3,4-dimethoxyphenyl
(127) 3,4-dianilinophenyl
(128) 3,4-dimethylphenyl
(129) 3,4-diphenoxyphenyl
(130) 3,4-dihydroxyphenyl
(131) 2-naphthyl
(132) 3,4,5-triethoxycarbonylphenyl
(133) 3,4,5-Tributoxyphenyl
(134) 3,4,5-triphenylphenyl
(135) 3,4,5-triphenylthiophenyl
(136) 3,4,5-trichlorophenyl
(137) 3,4,5-tribenzoylphenyl
(138) 3,4,5-triacetoxyphenyl
(139) 3,4,5-tribenzoyloxyphenyl
(140) 3,4,5-Triphenoxycarbonylphenyl
(141) 3,4,5-trimethoxyphenyl
(142) 3,4,5-trianilinophenyl
(143) 3,4,5-trimethylphenyl
(144) 3,4,5-triphenoxyphenyl
(145) 3,4,5-trihydroxyphenyl
[0120]
Embedded image
Figure 2004203009
[0121]
(146) phenyl
(147) 4-ethoxycarbonylphenyl
(148) 4-butoxyphenyl
(149) p-biphenylyl
(150) 4-phenylthiophenyl
(151) 4-chlorophenyl
(152) 4-benzoylphenyl
(153) 4-acetoxyphenyl
(154) 4-benzoyloxyphenyl
(155) 4-phenoxycarbonylphenyl
(156) 4-methoxyphenyl
(157) 4-anilinophenyl
(158) 4-isobutyrylaminophenyl
(159) 4-phenoxycarbonylaminophenyl
(160) 4- (3-ethylureido) phenyl
(161) 4- (3,3-diethylureido) phenyl
(162) 4-methylphenyl
(163) 4-phenoxyphenyl
(164) 4-hydroxyphenyl
[0122]
Embedded image
Figure 2004203009
[0123]
(165) phenyl
(166) 4-ethoxycarbonylphenyl
(167) 4-butoxyphenyl
(168) p-biphenylyl
(169) 4-phenylthiophenyl
(170) 4-chlorophenyl
(171) 4-benzoylphenyl
(172) 4-acetoxyphenyl
(173) 4-benzoyloxyphenyl
(174) 4-phenoxycarbonylphenyl
(175) 4-methoxyphenyl
(176) 4-anilinophenyl
(177) 4-isobutyrylaminophenyl
(178) 4-phenoxycarbonylaminophenyl
(179) 4- (3-ethylureido) phenyl
(180) 4- (3,3-Diethylureido) phenyl
(181) 4-methylphenyl
(182) 4-phenoxyphenyl
(183) 4-hydroxyphenyl
[0124]
Embedded image
Figure 2004203009
[0125]
(184) phenyl
(185) 4-ethoxycarbonylphenyl
(186) 4-butoxyphenyl
(187) p-biphenylyl
(188) 4-phenylthiophenyl
(189) 4-chlorophenyl
(190) 4-benzoylphenyl
(191) 4-acetoxyphenyl
(192) 4-benzoyloxyphenyl
(193) 4-phenoxycarbonylphenyl
(194) 4-methoxyphenyl
(195) 4-anilinophenyl
(196) 4-isobutyrylaminophenyl
(197) 4-phenoxycarbonylaminophenyl
(198) 4- (3-ethylureido) phenyl
(199) 4- (3,3-diethylureido) phenyl
(200) 4-methylphenyl
(201) 4-phenoxyphenyl
(202) 4-hydroxyphenyl
[0126]
Embedded image
Figure 2004203009
[0127]
(203) phenyl
(204) 4-ethoxycarbonylphenyl
(205) 4-butoxyphenyl
(206) p-biphenylyl
(207) 4-phenylthiophenyl
(208) 4-chlorophenyl
(209) 4-benzoylphenyl
(210) 4-acetoxyphenyl
(211) 4-benzoyloxyphenyl
(212) 4-phenoxycarbonylphenyl
(213) 4-methoxyphenyl
(214) 4-anilinophenyl
(215) 4-isobutyrylaminophenyl
(216) 4-phenoxycarbonylaminophenyl
(217) 4- (3-ethylureido) phenyl
(218) 4- (3,3-diethylureido) phenyl
(219) 4-methylphenyl
(220) 4-phenoxyphenyl
(221) 4-hydroxyphenyl
[0128]
Embedded image
Figure 2004203009
[0129]
(222) phenyl
(223) 4-butylphenyl
(224) 4- (2-methoxy-2-ethoxyethyl) phenyl
(225) 4- (5-Nonenyl) phenyl
(226) p-biphenylyl
(227) 4-ethoxycarbonylphenyl
(228) 4-butoxyphenyl
(229) 4-methylphenyl
(230) 4-chlorophenyl
(231) 4-phenylthiophenyl
(232) 4-benzoylphenyl
(233) 4-acetoxyphenyl
(234) 4-benzoyloxyphenyl
(235) 4-phenoxycarbonylphenyl
(236) 4-methoxyphenyl
(237) 4-anilinophenyl
(238) 4-isobutyrylaminophenyl
(239) 4-phenoxycarbonylaminophenyl
(240) 4- (3-ethylureido) phenyl
(241) 4- (3,3-diethylureido) phenyl
(242) 4-phenoxyphenyl
(243) 4-hydroxyphenyl
(244) 3-butylphenyl
(245) 3- (2-methoxy-2-ethoxyethyl) phenyl
(246) 3- (5-Nonenyl) phenyl
(247) m-biphenylyl
(248) 3-ethoxycarbonylphenyl
(249) 3-butoxyphenyl
(250) 3-methylphenyl
(251) 3-chlorophenyl
(252) 3-phenylthiophenyl
(253) 3-benzoylphenyl
(254) 3-acetoxyphenyl
(255) 3-benzoyloxyphenyl
(256) 3-phenoxycarbonylphenyl
(257) 3-methoxyphenyl
(258) 3-anilinophenyl
(259) 3-isobutyrylaminophenyl
(260) 3-phenoxycarbonylaminophenyl
(261) 3- (3-ethylureido) phenyl
(262) 3- (3,3-diethylureido) phenyl
(263) 3-phenoxyphenyl
(264) 3-hydroxyphenyl
(265) 2-butylphenyl
(266) 2- (2-methoxy-2-ethoxyethyl) phenyl
(267) 2- (5-nonenyl) phenyl
(268) o-Biphenylyl
(269) 2-ethoxycarbonylphenyl
(270) 2-butoxyphenyl
(271) 2-methylphenyl
(272) 2-chlorophenyl
(273) 2-phenylthiophenyl
(274) 2-benzoylphenyl
(275) 2-acetoxyphenyl
(276) 2-benzoyloxyphenyl
(277) 2-phenoxycarbonylphenyl
(278) 2-methoxyphenyl
(279) 2-anilinophenyl
(280) 2-isobutyrylaminophenyl
(281) 2-phenoxycarbonylaminophenyl
(282) 2- (3-ethylureido) phenyl
(283) 2- (3,3-diethylureido) phenyl
(284) 2-phenoxyphenyl
(285) 2-hydroxyphenyl
(286) 3,4-dibutylphenyl
(287) 3,4-di (2-methoxy-2-ethoxyethyl) phenyl
(288) 3,4-diphenylphenyl
(289) 3,4-diethoxycarbonylphenyl
(290) 3,4-didodecyloxyphenyl
(291) 3,4-dimethylphenyl
(292) 3,4-dichlorophenyl
(293) 3,4-dibenzoylphenyl
(294) 3,4-diacetoxyphenyl
(295) 3,4-dimethoxyphenyl
(296) 3,4-di-N-methylaminophenyl
(297) 3,4-diisobutyrylaminophenyl
(298) 3,4-diphenoxyphenyl
(299) 3,4-dihydroxyphenyl
(300) 3,5-dibutylphenyl
(301) 3,5-di (2-methoxy-2-ethoxyethyl) phenyl
(302) 3,5-diphenylphenyl
(303) 3,5-diethoxycarbonylphenyl
(304) 3,5-didodecyloxyphenyl
(305) 3,5-dimethylphenyl
(306) 3,5-dichlorophenyl
(307) 3,5-dibenzoylphenyl
(308) 3,5-diacetoxyphenyl
(309) 3,5-dimethoxyphenyl
(310) 3,5-di-N-methylaminophenyl
(311) 3,5-diisobutyrylaminophenyl
(312) 3,5-diphenoxyphenyl
(313) 3,5-dihydroxyphenyl
(314) 2,4-dibutylphenyl
(315) 2,4-di (2-methoxy-2-ethoxyethyl) phenyl
(316) 2,4-diphenylphenyl
(317) 2,4-diethoxycarbonylphenyl
(318) 2,4-didodecyloxyphenyl
(319) 2,4-dimethylphenyl
(320) 2,4-dichlorophenyl
(321) 2,4-dibenzoylphenyl
(322) 2,4-diacetoxyphenyl
(323) 2,4-dimethoxyphenyl
(324) 2,4-di-N-methylaminophenyl
(325) 2,4-diisobutyrylaminophenyl
(326) 2,4-diphenoxyphenyl
(327) 2,4-dihydroxyphenyl
(328) 2,3-dibutylphenyl
(329) 2,3-di (2-methoxy-2-ethoxyethyl) phenyl
(330) 2,3-diphenylphenyl
(331) 2,3-diethoxycarbonylphenyl
(332) 2,3-didodecyloxyphenyl
(333) 2,3-dimethylphenyl
(334) 2,3-dichlorophenyl
(335) 2,3-dibenzoylphenyl
(336) 2,3-diacetoxyphenyl
(337) 2,3-dimethoxyphenyl
(338) 2,3-di-N-methylaminophenyl
(339) 2,3-diisobutyrylaminophenyl
(340) 2,3-diphenoxyphenyl
(341) 2,3-dihydroxyphenyl
(342) 2,6-dibutylphenyl
(343) 2,6-di (2-methoxy-2-ethoxyethyl) phenyl
(344) 2,6-diphenylphenyl
(345) 2,6-diethoxycarbonylphenyl
(346) 2,6-didodecyloxyphenyl
(347) 2,6-dimethylphenyl
(348) 2,6-dichlorophenyl
(349) 2,6-dibenzoylphenyl
(350) 2,6-diacetoxyphenyl
(351) 2,6-dimethoxyphenyl
(352) 2,6-di-N-methylaminophenyl
(353) 2,6-diisobutyrylaminophenyl
(354) 2,6-diphenoxyphenyl
(355) 2,6-dihydroxyphenyl
(356) 3,4,5-tributylphenyl
(357) 3,4,5-tri (2-methoxy-2-ethoxyethyl) phenyl
(358) 3,4,5-triphenylphenyl
(359) 3,4,5-triethoxycarbonylphenyl
(360) 3,4,5-tridodecyloxyphenyl
(361) 3,4,5-trimethylphenyl
(362) 3,4,5-trichlorophenyl
(363) 3,4,5-tribenzoylphenyl
(364) 3,4,5-triacetoxyphenyl
(365) 3,4,5-trimethoxyphenyl
(366) 3,4,5-tri-N-methylaminophenyl
(367) 3,4,5-triisobutyrylaminophenyl
(368) 3,4,5-Triphenoxyphenyl
(369) 3,4,5-trihydroxyphenyl
(370) 2,4,6-tributylphenyl
(371) 2,4,6-tri (2-methoxy-2-ethoxyethyl) phenyl
(372) 2,4,6-triphenylphenyl
(373) 2,4,6-triethoxycarbonylphenyl
(374) 2,4,6-tridodecyloxyphenyl
(375) 2,4,6-trimethylphenyl
(376) 2,4,6-trichlorophenyl
(377) 2,4,6-tribenzoylphenyl
(378) 2,4,6-triacetoxyphenyl (379) 2,4,6-trimethoxyphenyl
(380) 2,4,6-tri-N-methylaminophenyl
(381) 2,4,6-triisobutyrylaminophenyl
(382) 2,4,6-triphenoxyphenyl (383) 2,4,6-trihydroxyphenyl
(384) pentafluorophenyl
(385) pentachlorophenyl
(386) pentamethoxyphenyl
(387) 6-N-methylsulfamoyl-8-methoxy-2-naphthyl
(388) 5-N-methylsulfamoyl-2-naphthyl
(389) 6-N-phenylsulfamoyl-2-naphthyl
(390) 5-ethoxy-7-N-methylsulfamoyl-2-naphthyl
(391) 3-methoxy-2-naphthyl
(392) 1-ethoxy-2-naphthyl
(393) 6-N-phenylsulfamoyl-8-methoxy-2-naphthyl
(394) 5-methoxy-7-N-phenylsulfamoyl-2-naphthyl
(395) 1- (4-methylphenyl) -2-naphthyl
(396) 6,8-di-N-methylsulfamoyl-2-naphthyl
(397) 6-N-2-acetoxyethylsulfamoyl-8-methoxy-2-naphthyl
(398) 5-acetoxy-7-N-phenylsulfamoyl-2-naphthyl
(399) 3-benzoyloxy-2-naphthyl
(400) 5-acetylamino-1-naphthyl
(401) 2-Methoxy-1-naphthyl (402) 4-phenoxy-1-naphthyl
(403) 5-N-methylsulfamoyl-1-naphthyl
(404) 3-N-methylcarbamoyl-4-hydroxy-1-naphthyl
(405) 5-methoxy-6-N-ethylsulfamoyl-1-naphthyl
(406) 7-tetradecyloxy-1-naphthyl
(407) 4- (4-methylphenoxy) -1-naphthyl
(408) 6-N-methylsulfamoyl-1-naphthyl
(409) 3-N, N-dimethylcarbamoyl-4-methoxy-1-naphthyl
(410) 5-methoxy-6-N-benzylsulfamoyl-1-naphthyl
(411) 3,6-di-N-phenylsulfamoyl-1-naphthyl
(412) Methyl
(413) Ethyl
(414) Butyl
(415) Octyl
(416) Dodecyl
(417) 2-butoxy-2-ethoxyethyl
(418) Benzyl
(419) 4-methoxybenzyl
[0130]
Embedded image
Figure 2004203009
[0131]
(424) methyl
(425) phenyl
(426) Butyl
[0132]
Embedded image
Figure 2004203009
[0133]
(430) methyl
(431) Ethyl
(432) butyl
(433) Octyl
(434) Dodecyl
(435) 2-butoxy 2-ethoxyethyl
(436) benzyl
(437) 4-methoxybenzyl
[0134]
Embedded image
Figure 2004203009
[0135]
Embedded image
Figure 2004203009
[0136]
In the present invention, a melamine polymer may be used as the compound having a 1,3,5-triazine ring. The melamine polymer is preferably synthesized by a polymerization reaction of a melamine compound represented by the following general formula (IV) with a carbonyl compound.
[0137]
Embedded image
Figure 2004203009
[0138]
In the above synthesis reaction scheme, R11, R12, RThirteen, R14, RFifteenAnd R16Is a hydrogen atom, an alkyl group, an alkenyl group, an aryl group or a heterocyclic group.
[0139]
The above-mentioned alkyl group, alkenyl group, aryl group, heterocyclic group and their substituents have the same meanings as those described in the general formula (I) and their substituents.
[0140]
The polymerization reaction between the melamine compound and the carbonyl compound is the same as in a method for synthesizing a normal melamine resin (for example, a melamine formaldehyde resin). Alternatively, a commercially available melamine polymer (melamine resin) may be used.
[0141]
The molecular weight of the melamine polymer is preferably from 2,000 to 400,000. Specific examples of the repeating unit of the melamine polymer are shown below.
[0142]
Embedded image
Figure 2004203009
[0143]
MP-1: RThirteen, R14, RFifteen, R16: CH2OH
MP-2: RThirteen, R14, RFifteen, R16: CH2OCH3
MP-3: RThirteen, R14, RFifteen, R16:CH2OiC4H9
MP-4: RThirteen, R14, RFifteen, R16: CH2On-C4H9
MP-5: RThirteen, R14, RFifteen, R16: CH2NHCOCH = CH2
MP-6: RThirteen, R14, RFifteen, R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-7: RThirteen, R14, RFifteen: CH2OH; R16: CH2OCH3
MP-8: RThirteen, R14, R16: CH2OH; RFifteen: CH2OCH3
MP-9: RThirteen, R14: CH2OH; RFifteen, R16: CH2OCH3
MP-10: RThirteen, R16: CH2OH; R14, RFifteen: CH2OCH3
MP-11: RThirteen: CH2OH; R14, RFifteen, R16: CH2OCH3
MP-12: RThirteen, R14, R16: CH2OCH3RFifteen: CH2OH
MP-13: RThirteen, R16: CH2OCH3R14, RFifteen: CH2OH
MP-14: RThirteen, R14, RFifteen: CH2OH; R16: CH2OiC4H9
MP-15: RThirteen, R14, R16: CH2OH; RFifteen: CH2OiC4H9
MP-16: RThirteen, R14: CH2OH; RFifteen, R16: CH2OiC4H9
MP-17: RThirteen, R16: CH2OH; R14, RFifteen: CH2OiC4H9
MP-18: RThirteen: CH2OH; R14, RFifteen, R16: CH2OiC4H9
MP-19: RThirteen, R14, R16: CH2OiC4H9RFifteen: CH2OH
MP-20: RThirteen, R16: CH2OiC4H9R14, RFifteen: CH2OH
MP-21: RThirteen, R14, RFifteen: CH2OH; R16: CH2On-C4H9
MP-22: RThirteen, R14, R16: CH2OH; RFifteen: CH2On-C4H9
MP-23: RThirteen, R14: CH2OH; RFifteen, R16: CH2On-C4H9
MP-24: RThirteen, R16: CH2OH; R14, RFifteen: CH2On-C4H9
MP-25: RThirteen: CH2OH; R14, RFifteen, R16: CH2O-N-C4H9
MP-26: RThirteen, R14, R16: CH2On-C4H9RFifteen: CH2OH
MP-27: RThirteen, R16: CH2On-C4H9R14, RFifteen: CH2OH
MP-28: RThirteen, R14: CH2OH; RFifteen: CH2OCH3R16: CH2On-C4H9
MP-29: RThirteen, R14: CH2OH; RFifteen: CH2On-C4H9R16: CH2OCH3
MP-30: RThirteen, R16: CH2OH; R14: CH2OCH3RFifteen: CH2On-C4H9
MP-31: RThirteen: CH2OH; R14, RFifteen: CH2OCH3R16: CH2On-C4H9
MP-32: RThirteen: CH2OH; R14, R16: CH2OCH3RFifteen: CH2On-C4H9
MP-33: RThirteen: CH2OH; R14: CH2OCH3RFifteen, R16: CH2On-C4H9
MP-34: RThirteen: CH2OH; R14, RFifteen: CH2On-C4H9R16: CH2OCH3
MP-35: RThirteen, R14: CH2OCH3RFifteen: CH2OH; R16: CH2On-C4H9
MP-36: RThirteen, R16: CH2OCH3R14: CH2OH; RFifteen: CH2On-C4H9
MP-37: RThirteen: CH2OCH3R14, RFifteen: CH2OH; R16: CH2On-C4H9
MP-38: RThirteen, R16: CH2On-C4H9R14: CH2OCH3RFifteen: CH2OH
MP-39: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2On-C4H9; R16: CH2NHCOCH = CH2
MP-40: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCOCH = CH2R16: CH2On-C4H9
MP-41: RThirteen: CH2OH; R14: CH2On-C4H9RFifteen: CH2NHCOCH = CH2R16: CH2OCH3
MP-42: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2On-C4H9R16:CH2NHCOCH = CH2
MP-43: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCOCH = CH2R16: CH2On-C4H9
MP-44: RThirteen: CH2On-C4H9R14: CH2OCH3RFifteen: CH2OH; R16: CH2NHCOCH = CH2
MP-45: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R16: CH2NHCOCH = CH2
MP-46: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCOCH = CH2R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-47: RThirteen: CH2OH; R14: CH2NHCO (CH2)7CH = CH (CH2)7CH3RFifteen: CH2NHCOCH = CH2R16: CH2OCH3
MP-48: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R16: CH2NHCOCH = CH2
MP-49: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCOCH = CH2R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-50: RThirteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R14: CH2OCH3RFifteen: CH2OH; R16: CH2NHCOCH = CH2
[0144]
Embedded image
Figure 2004203009
[0145]
MP-51: RThirteen, R14, RFifteen, R16: CH2OH
MP-52: RThirteen, R14, RFifteen, R16: CH2OCH3
MP-53: RThirteen, R14, RFifteen, R16: CH2OiC4H9
MP-54: RThirteen, R14, RFifteen, R16: CH2On-C4H9
MP-55: RThirteen, R14, RFifteen, R16: CH2NHCOCH = CH2
MP-56: RThirteen, R14, RFifteen, R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-57: RThirteen, R14, RFifteen: CH2OH; R16: CH2OCH3
MP-58: RThirteen, R14, R16: CH2OH; RFifteen: CH2OCH3
MP-59: RThirteen, R14: CH2OH; RFifteen, R16: CH2OCH3
MP-60: RThirteen, R16: CH2OH; R14, RFifteen: CH2OCH3
MP-61: RThirteen: CH2OH; R14, RFifteen, R16: CH2OCH3
MP-62: RThirteen, R14, R16: CH2OCH3RFifteen: CH2OH
MP-63: RThirteen, R16: CH2OCH3R14, RFifteen: CH2OH
MP-64: RThirteen, R14, RFifteen: CH2OH; R16: CH2OiC4H9
MP-65: RThirteen, R14, R16: CH2OH; RFifteen: CH2OiC4H9
MP-66: RThirteen, R14: CH2OH; RFifteen, R16: CH2OiC4H9
MP-67: RThirteen, R16: CH2OH; R14, RFifteen: CH2OiC4H9
MP-68: RThirteen: CH2OH; R14, RFifteen, R16: CH2OiC4H9
MP-69: RThirteen, R14, R16: CH2OiC4H9RFifteen: CH2OH
MP-70: RThirteen, R16: CH2OiC4H9R14, RFifteen: CH2OH
MP-71: RThirteen, R14, RFifteen: CH2OH; R16: CH2On-C4H9
MP-72: RThirteen, R14, R16: CH2OH; RFifteen: CH2On-C4H9
MP-73: RThirteen, R14: CH2OH; RFifteen, R16: CH2On-C4H9
MP-74: RThirteen, R16: CH2OH; R14, RFifteen: CH2On-C4H9
MP-75: RThirteen: CH2OH; R14, RFifteen, R16: CH2On-C4H9
MP-76: RThirteen, R14, R16: CH2On-C4H9RFifteen: CH2OH
MP-77: RThirteen, R16: CH2On-C4H9R14, RFifteen: CH2OH
MP-78: RThirteen, R14: CH2OH; RFifteen: CH2OCH3R16: CH2On-C4H9
MP-79: RThirteen, R14: CH2OH; RFifteen: CH2On-C4H9R16: CH2OCH3
MP-80: RThirteen, R16: CH2OH; R14: CH2OCH3RFifteen: CH2On-C4H9
MP-81: RThirteen: CH2OH; R14, RFifteen: CH2OCH3R16: CH2On-C4H9
MP-82: RThirteen: CH2OH; R14, R16: CH2OCH3RFifteen: CH2On-C4H9
MP-83: RThirteen: CH2OH; R14: CH2OCH3RFifteen, R16: CH2On-C4H9
MP-84: RThirteen: CH2OH; R14, RFifteen: CH2On-C4H9R16: CH2OCH3
MP-85: RThirteen, R14: CH2OCH3RFifteen: CH2OH; R16: CH2On-C4H9
MP-86: RThirteen, R16: CH2OCH3R14: CH2OH; RFifteen: CH2On-C4H9
MP-87: RThirteen: CH2OCH3R14, RFifteen: CH2OH; R16: CH2On-C4H9
MP-88: RThirteen, R16: CH2On-C4H9R14: CH2OCH3RFifteen: CH2OH
MP-89: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2On-C4H9R16: CH2NHCOCH = CH2
MP-90: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCOCH = CH2R16: CH2On-C4H9
MP-91: RThirteen: CH2OH; R14: CH2On-C4H9RFifteen: CH2NHCOCH = CH2R16: CH2OCH3
MP-92: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2On-C4H9R16: CH2NHCOCH = CH2
MP-93: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCOCH = CH2R16: CH2On-C4H9
MP-94: RThirteen: CH2On-C4H9R14: CH2OCH3RFifteen: CH2OH; R16: CH2NHCOCH = CH2
MP-95: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R16: CH2NHCOCH = CH2
MP-96: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCOCH = CH2R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-97: RThirteen: CH2OH; R14: CH2NHCO (CH2)7CH = CH (CH2)7CH3RFifteen: CH2NHCOCH = CH2R16: CH2OCH3
MP-98: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R16: CH2NHCOCH = CH2
MP-99: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCOCH = CH2R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-100: RThirteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R14: CH2OCH3RFifteen: CH2OH; R16: CH2NHCOCH = CH2
[0146]
Embedded image
Figure 2004203009
[0147]
MP-101: RThirteen, R14, RFifteen, R16: CH2OH
MP-102: RThirteen, R14, RFifteen, R16: CH2OCH3
MP-103: RThirteen, R14, RFifteen, R16: CH2OiC4H9
MP-104: RThirteen, R14, RFifteen, R16: CH2On-C4H9
MP-105: RThirteen, R14, RFifteen, R16: CH2NHCOCH = CH2
MP-106: RThirteen, R14, RFifteen, R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-107: RThirteen, R14, RFifteen: CH2OH; R16: CH2OCH3
MP-108: RThirteen, R14, R16: CH2OH; RFifteen: CH2OCH3
MP-109: RThirteen, R14: CH2OH; RFifteen, R16: CH2OCH3
MP-110: RThirteen, R16: CH2OH; R14, RFifteen: CH2OCH3
MP-111: RThirteen: CH2OH; R14, RFifteen, R16: CH2OCH3
MP-112: RThirteen, R14, R16: CH2OCH3RFifteen: CH2OH
MP-113: RThirteen, R16: CH2OCH3R14, RFifteen: CH2OH
MP-114: RThirteen, R14, RFifteen: CH2OH; R16: CH2OiC4H9
MP-115: RThirteen, R14, R16: CH2OH; RFifteen: CH2OiC4H9
MP-116: RThirteen, R14: CH2OH; RFifteen, R16: CH2OiC4H9
MP-117: RThirteen, R16: CH2OH; R14, RFifteen: CH2OiC4H9
MP-118: RThirteen: CH2OH; R14, RFifteen, R16: CH2OiC4H9
MP-119: RThirteen, R14, R16: CH2OiC4H9RFifteen: CH2OH
MP-120: RThirteen, R16: CH2OiC4H9R14, RFifteen: CH2OH
MP-121: RThirteen, R14, RFifteen: CH2OH; R16: CH2On-C4H9
MP-122: RThirteen, R14, R16: CH2OH; RFifteen: CH2On-C4H9
MP-123: RThirteen, R14: CH2OH; RFifteen, R16: CH2On-C4H9
MP-124: RThirteen, R16: CH2OH; R14, RFifteen: CH2On-C4H9
MP-125: RThirteen: CH2OH; R14, RFifteen, R16: CH2On-C4H9
MP-126: RThirteen, R14, R16: CH2On-C4H9RFifteen: CH2OH
MP-127: RThirteen, R16: CH2On-C4H9R14, RFifteen: CH2OH
MP-128: RThirteen, R14: CH2OH; RFifteen: CH2OCH3R16: CH2On-C4H9
MP-129: RThirteen, R14: CH2OH; RFifteen: CH2On-C4H9R16: CH2OCH3
MP-130: RThirteen, R16: CH2OH; R14: CH2OCH3RFifteen: CH2On-C4H9
MP-131: RThirteen: CH2OH; R14, RFifteen: CH2OCH3R16: CH2On-C4H9
MP-132: RThirteen: CH2OH; R14, R16: CH2OCH3RFifteen: CH2On-C4H9
MP-133: RThirteen: CH2OH; R14: CH2OCH3RFifteen, R16: CH2On-C4H9
MP-134: RThirteen: CH2OH; R14, RFifteen: CH2On-C4H9R16: CH2OCH3
MP-135: RThirteen, R14: CH2OCH3RFifteen: CH2OH; R16: CH2On-C4H9
MP-136: RThirteen, R16: CH2OCH3R14: CH2OH; RFifteen: CH2On-C4H9
MP-137: RThirteen: CH2OCH3R14, RFifteen: CH2OH; R16: CH2On-C4H9
MP-138: RThirteen, R16: CH2On-C4H9R14: CH2OCH3RFifteen: CH2OH
MP-139: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2On-C4H9R16: CH2NHCOCH = CH2
MP-140: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCOCH = CH2R16: CH2On-C4H9
MP-141: RThirteen: CH2OH; R14: CH2On-C4H9RFifteen: CH2NHCOCH = CH2R16: CH2OCH3
MP-142: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2On-C4H9R16: CH2NHCOCH = CH2
MP-143: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCOCH = CH2R16: CH2On-C4H9
MP-144: RThirteen: CH2On-C4H9R14: CH2OCH3RFifteen: CH2OH; R16: CH2NHCOCH = CH2
MP-145: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R16: CH2NHCOCH = CH2
MP-146: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCOCH = CH2R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-147: RThirteen: CH2OH; R14: CH2NHCO (CH2)7CH = CH (CH2)7CH3RFifteen: CH2NHCOCH = CH2R16: CH2OCH3
MP-148: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R16: CH2NHCOCH = CH2
MP-149: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCOCH = CH2R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-150: RThirteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R14: CH2OCH3RFifteen: CH2OH; R16: CH2NHCOCH = CH2
[0148]
Embedded image
Figure 2004203009
[0149]
MP-151: RThirteen, R14, RFifteen, R16:CH2OH
MP-152: RThirteen, R14, RFifteen, R16: CH2OCH3
MP-153: RThirteen, R14, RFifteen, R16: CH2OiC4H9
MP-154: RThirteen, R14, RFifteen, R16: CH2On-C4H9
MP-155: RThirteen, R14, RFifteen, R16: CH2NHCOCH = CH2
MP-156: RThirteen, R14, RFifteen, R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-157: RThirteen, R14, RFifteen: CH2OH; R16: CH2OCH3
MP-158: RThirteen, R14, R16: CH2OH; RFifteen: CH2OCH3
MP-159: RThirteen, R14: CH2OH; RFifteen, R16: CH2OCH3
MP-160: RThirteen, R16: CH2OH; R14, RFifteen: CH2OCH3
MP-161: RThirteen: CH2OH; R14, RFifteen, R16: CH2OCH3
MP-162: RThirteen, R14, R16: CH2OCH3RFifteen: CH2OH
MP-163: RThirteen, R16: CH2OCH3R14, RFifteen: CH2OH
MP-164: RThirteen, R14, RFifteen: CH2OH; R16: CH2OiC4H9
MP-165: RThirteen, R14, R16: CH2OH; RFifteen: CH2OiC4H9
MP-166: RThirteen, R14: CH2OH; RFifteen, R16: CH2OiC4H9
MP-167: RThirteen, R16: CH2OH; R14, RFifteen: CH2OiC4H9
MP-168: RThirteen: CH2OH; R14, RFifteen, R16: CH2OiC4H9
MP-169: RThirteen, R14, R16: CH2OiC4H9RFifteen: CH2OH
MP-170: RThirteen, R16: CH2OiC4H9R14, RFifteen: CH2OH
MP-171: RThirteen, R14, RFifteen: CH2OH; R16: CH2On-C4H9
MP-172: RThirteen, R14, R16: CH2OH; RFifteen: CH2On-C4H9
MP-173: RThirteen, R14: CH2OH; RFifteen, R16: CH2On-C4H9
MP-174: RThirteen, R16: CH2OH; R14, RFifteen: CH2On-C4H9
MP-175: RThirteen: CH2OH; R14, RFifteen, R16: CH2On-C4H9
MP-176: RThirteen, R14, R16: CH2On-C4H9RFifteen: CH2OH
MP-177: RThirteen, R16: CH2On-C4H9R14, RFifteen: CH2OH
MP-178: RThirteen, R14: CH2OH; RFifteen: CH2OCH3R16: CH2On-C4H9
MP-179: RThirteen, R14: CH2OH; RFifteen: CH2On-C4H9R16: CH2OCH3
MP-180: RThirteen, R16: CH2OH; R14: CH2OCH3RFifteen: CH2On-C4H9
MP-181: RThirteen: CH2OH; R14, RFifteen: CH2OCH3R16: CH2On-C4H9
MP-182: RThirteen: CH2OH; R14, R16: CH2OCH3RFifteen: CH2On-C4H9
MP-183: RThirteen: CH2OH; R14: CH2OCH3RFifteen, R16: CH2On-C4H9
MP-184: RThirteen: CH2OH; R14, RFifteen: CH2On-C4H9R16: CH2OCH3
MP-185: RThirteen, R14: CH2OCH3RFifteen: CH2OH; R16: CH2O-N-C4H9
MP-186: RThirteen, R16: CH2OCH3R14: CH2OH; RFifteen: CH2On-C4H9
MP-187: RThirteen: CH2OCH3R14, RFifteen: CH2OH; R16: CH2On-C4H9
MP-188: RThirteen, R16: CH2On-C4H9R14: CH2OCH3R1 5: CH2OH
MP-189: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2On-C4H9R16: CH2NHCOCH = CH2
MP-190: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCOCH = CH2R16: CH2On-C4H9
MP-191: RThirteen: CH2OH; R14: CH2On-C4H9RFifteen: CH2NHCOCH = CH2R16: CH2OCH3
MP-192: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2On-C4H9R16: CH2NHCOCH = CH2
MP-193: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCOCH = CH2R16: CH2On-C4H9
MP-194: RThirteen: CH2On-C4H9R14: CH2OCH3RFifteen: CH2OH; R16: CH2NHCOCH = CH2
MP-195: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R16: CH2NHCOCH = CH2
MP-196: RThirteen: CH2OH; R14: CH2OCH3RFifteen: CH2NHCOCH = CH2R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-197: RThirteen: CH2OH; R14: CH2NHCO (CH2)7CH = CH (CH2)7CH3RFifteen: CH2NHCOCH = CH2R16: CH2OCH3
MP-198: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R16: CH2NHCOCH = CH2
MP-199: RThirteen: CH2OCH3R14: CH2OH; RFifteen: CH2NHCOCH = CH2R16: CH2NHCO (CH2)7CH = CH (CH2)7CH3
MP-200: RThirteen: CH2NHCO (CH2)7CH = CH (CH2)7CH3R14: CH2OCH3RFifteen: CH2OH; R16: CH2NHCOCH = CH2
In the present invention, a copolymer obtained by combining two or more kinds of the above repeating units may be used. Two or more homopolymers or copolymers may be used in combination.
[0150]
Further, two or more compounds having a 1,3,5-triazine ring may be used in combination. Two or more discotic compounds (for example, a compound having a 1,3,5-triazine ring and a compound having a porphyrin skeleton) may be used in combination.
[0151]
In addition, specific examples of the additives other than those described above of the present invention will be described below.
[0152]
Embedded image
Figure 2004203009
[0153]
Embedded image
Figure 2004203009
[0154]
Embedded image
Figure 2004203009
[0155]
Embedded image
Figure 2004203009
[0156]
Embedded image
Figure 2004203009
[0157]
Embedded image
Figure 2004203009
[0158]
Embedded image
Figure 2004203009
[0159]
In the dope, additives other than those described above, an antioxidant, a dye, a fluorescent brightener (for example, those described in Japanese Patent Application No. 2002-123821) and the like can be added.
[0160]
(2) -1 In-line additive liquid (mainly containing ultraviolet absorber) preparation process
The description will be made as an in-line additive liquid containing an ultraviolet absorber. The method for preparing an organic solvent such as a lower alcohol used for a cellulose ester solution, a resin described below, and an ultraviolet absorber-containing in-line additive liquid containing as needed is a method that can be sufficiently uniformly prepared in the liquid. Although not particularly limited, the following method is preferable.
[0161]
An organic solvent, an ultraviolet absorber, and a resin described below are added to the dissolving vessel 111 as needed, and the mixture is stirred and dissolved to form a resin solution. The solution is sent to a filter 113 by a solution sending pump 112 to remove aggregates and form an in-line additive solution 110 (a similar operation may be repeated several times to circulate). Then, the in-line additive liquid is transferred from the switching valve 119 to the stock tank 114, and after standing still defoaming, the liquid is transferred by the liquid feed pump 115 (for example, a pressurized fixed quantity gear pump), filtered by the filter 116 and transferred by the conduit 117.
[0162]
The organic solvent used is preferably the organic solvent used for the dope, but is not particularly limited. Examples of the lower alcohols used for the dope include methyl alcohol, ethyl alcohol, propyl alcohol, isopropyl alcohol, butyl alcohol, etc., and ethanol is particularly preferable.
[0163]
If necessary, a resin having good compatibility with the cellulose ester can be added to the liquid for adding an ultraviolet absorber. As the resin having good compatibility with the cellulose ester, a cellulose ester used for the dope may be used, but the resin described in Japanese Patent Application No. 2001-184450 can be preferably used because it is hardly clogged at the time of filtration of the dispersion. For example, Actflow series resins commercially available from Soken Chemical Co., Ltd. can be preferably used.
[0164]
After filtration in the final filter 116, the in-line additive liquid is preferably transferred by a conduit without stagnating in a stock tank or the like and without passing through a liquid feed pump. It is merged with the ester solution 100 by a merge pipe 120. This is preferable because there is no stagnation of both liquids and no new aggregates are generated by the liquid feed pump. These filtrations are located immediately before the in-line mixer. For example, large aggregates generated from the path due to replacement of the filter medium, etc. are reliably removed from the fine particle dispersion liquid being sent by a single filtration to relatively large foreign substances. It is preferable to use a metal filter having the above-mentioned absolute filtration accuracy and a metal filter having organic solvent resistance which can be used for a long time. As the filter medium, metal, particularly stainless steel, is preferable from the viewpoint of durability. It is preferable to have a porosity of 60 to 80% from the viewpoint of clogging. Therefore, it is most preferable to filter with a metal filter medium having an absolute filtration accuracy of 30 to 60 μm and a porosity of 60 to 80%, thereby reliably removing coarse foreign substances over a long period of time. Is preferred. Examples of a metal filter medium having an absolute filtration accuracy of 30 to 60 μm and a porosity of 60 to 80% include, for example, NF-10, NF-12, and NF-13 of Finepore NF series manufactured by Nippon Seisen Co., Ltd. And any of them is preferably used.
[0165]
(2) -2 In-line additive liquid (mainly containing fine particle dispersion) preparation process
Description will be made as an in-line additive liquid containing a fine particle dispersion. An organic solvent such as a lower alcohol used for a cellulose ester solution, a method for preparing a fine particle agent dispersion containing a resin described below and a matting agent fine particle described below is a method capable of sufficiently dispersing uniformly in the liquid. Although not particularly limited, the following method is preferable.
[0166]
An organic solvent and a resin described below are added to the dissolving vessel 111A, and the mixture is stirred and dissolved to form a resin solution. Fine particles of the matting agent or a fine particle dispersion are added to the resin solution, and a dispersing machine such as a manton-goreen or a sand mill (shown in the figure). ) And sent to a filter 113A by a liquid sending pump 112A to remove aggregates to obtain an in-line additive liquid 110A (a similar operation may be repeated several times to circulate). Then, the in-line additive liquid is transferred from the switching valve 119A to the stock tank 114A, and after standing still and defoamed, transferred by the liquid feed pump 115A (for example, a pressurized fixed quantity gear pump), filtered by the filter 116A, and transferred by the conduit 117A. In addition, you may add an ultraviolet absorber to an in-line additive liquid beforehand in the dissolution pot 111A.
[0167]
As a method for preparing the dispersion liquid of the fine particles according to the present invention, for example, the following three types can be mentioned.
[0168]
(Preparation method A)
After stirring and mixing the organic solvent and the fine particles, the mixture is dispersed with a disperser. This is used as a dispersion of fine particles.
[0169]
(Preparation method B)
After stirring and mixing the organic solvent and the fine particles, the mixture is dispersed with a disperser to obtain a dispersion liquid of the fine particles. Separately, a small amount of a resin (a resin having a good dispersibility to fine particles and giving a proper viscosity to the liquid and being compatible with a cellulose ester, or a cellulose ester) is added to an organic solvent, and the resin solution obtained by stirring and dissolving is added. prepare. The above-mentioned fine particle dispersion is added thereto, stirred and sufficiently dispersed to obtain a fine particle dispersion.
[0170]
(Preparation method C)
A small amount of resin (a resin having good dispersibility with respect to fine particles and compatible with cellulose ester or cellulose ester) is added to the organic solvent, and the mixture is stirred and dissolved. Fine particles are added thereto and sufficiently dispersed by a disperser to obtain a dispersion liquid of the fine particles.
[0171]
Preparation method A is excellent in dispersibility of silicon dioxide fine particles, and preparation method C is excellent in that silicon dioxide fine particles are hard to re-aggregate. Preparation method B is a preferable preparation method that is excellent in both the dispersibility of the silicon dioxide fine particles and the difficulty of re-aggregation of the silicon dioxide fine particles.
[0172]
The in-line additive solution containing the dispersion liquid of the fine particles dispersed and prepared by the preparation methods A to C is added to the cellulose ester solution and stirred to form a dope. The in-line additive solution and the cellulose ester solution are combined in the in-line, and the in-line mixer is used. It is preferable that the dope is sufficiently mixed.
[0173]
In the above-mentioned preparation method, the concentration of silicon dioxide when the silicon dioxide fine particles are mixed and dispersed in an organic solvent is preferably 5 to 30% by mass, more preferably 10 to 25% by mass, and still more preferably 15 to 20% by mass. The higher the dispersion concentration, the lower the liquid turbidity with respect to the amount added, and the resulting film has a low haze and is preferably free of aggregates.
[0174]
The organic solvent used is preferably the organic solvent used for the dope, but is not particularly limited. Examples of the lower alcohols used for the dope include methyl alcohol, ethyl alcohol, propyl alcohol, isopropyl alcohol, butyl alcohol, etc., and ethanol is particularly preferable.
[0175]
As a resin that helps dispersibility of fine particles, improves dispersibility, and has good compatibility with cellulose ester, a cellulose ester used for dope may be used. However, the resin described in Japanese Patent Application No. 2001-184450 may be used for dispersion filtration. At this time, it can be preferably used because it is hardly clogged. For example, Actflow series resins commercially available from Soken Chemical Co., Ltd. can be preferably used.
[0176]
(Dispersion equipment)
An ordinary disperser can be used as the disperser for dispersing the fine particles. Dispersers can be broadly divided into media dispersers and medialess dispersers. For dispersing silicon dioxide fine particles, a medialess disperser is preferred because it has a low haze. Examples of the media dispersing machine include a ball mill, a sand mill, and a dyno mill. Examples of the medialess disperser include an ultrasonic type, a centrifugal type, and a high-pressure type. In the present invention, a high-pressure disperser is preferable. The high-pressure dispersing device is a device that creates a special condition such as a high shear or a high pressure state by allowing a composition in which fine particles and a solvent are mixed to pass through a thin tube at a high speed.
[0177]
In the case of processing with a high-pressure dispersion device, for example, it is preferable that the maximum pressure condition inside the device is 10 MPa or more in a thin tube having a tube diameter of 1 to 2000 μm. More preferably, it is 20 MPa or more. In this case, it is preferable that the maximum arrival speed reaches 100 m / sec or more, and the heat transfer speed reaches 420 kJ / hour or more. The high-pressure dispersing apparatus as described above includes an ultrahigh-pressure homogenizer (trade name: Microfluidizer) manufactured by Microfluidics Corporation and a nanomizer manufactured by Nanomizer. UHN-01 manufactured by Waki Machine Co., Ltd. can be mentioned.
[0178]
After filtration in the final filter 116A, the in-line additive liquid is preferably transferred by a conduit without being stagnated in a stock tank or the like and without passing through a liquid feed pump. The solution is combined with the ester solution 100A in the joining pipe 120A and supplied to the die while being mixed in the mixer 121. This is preferable because there is no stagnation of both liquids and no new aggregates are generated by the liquid feed pump. These filtrations are located immediately before the in-line mixer. For example, large aggregates generated from the path due to replacement of the filter medium, etc. are reliably removed from the fine particle dispersion liquid being sent by a single filtration to relatively large foreign substances. It is preferable to use a metal filter having the above-mentioned absolute filtration accuracy and a metal filter having organic solvent resistance which can be used for a long time. As the filter medium, metal, particularly stainless steel, is preferable from the viewpoint of durability. It is preferable to have a porosity of 60 to 80% from the viewpoint of clogging. Therefore, it is most preferable to filter with a metal filter medium having an absolute filtration accuracy of 30 to 60 μm and a porosity of 60 to 80%, thereby reliably removing coarse foreign substances over a long period of time. Is preferred. Examples of a metal filter medium having an absolute filtration accuracy of 30 to 60 μm and a porosity of 60 to 80% include, for example, NF-10, NF-12, and NF-13 of Finepore NF series manufactured by Nippon Seisen Co., Ltd. And any of them is preferably used.
[0179]
<< Additive used in cellulose ester film and actinic radiation curable resin layer as lower hard coat layer >>
The additive of the cellulose ester film used in the present invention will be described.
[0180]
(Plasticizer)
The plasticizer is not particularly limited, but a phosphate ester plasticizer, a phthalate ester plasticizer, a trimellitate ester plasticizer, a pyromellitic acid plasticizer, a glycolate plasticizer, a citrate ester plasticizer Agents, polyester plasticizers and the like.
[0181]
Phosphate esters include
For example, triphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, octyl diphenyl phosphate, diphenyl biphenyl phosphate, trioctyl phosphate, tributyl phosphate and the like;
As phthalate esters,
For example, diethyl phthalate, dimethoxyethyl phthalate, dimethyl phthalate, dioctyl phthalate, dibutyl phthalate, di-2-ethylhexyl phthalate, butylbenzyl phthalate, dicyclohexyl phthalate, dibenzyl phthalate and the like;
Examples of the trimellitic acid-based plasticizer include tributyl trimellitate, triphenyl trimellitate, triethyl trimellitate, and the like;
As pyromellitic ester plasticizers,
For example, tetrabutyl pyromellitate, tetraphenyl pyromellitate, tetraethyl pyromellitate, and the like;
As glycerin esters,
For example, triacetin, tributyrin and the like;
Examples of glycolic acid esters include ethyl phthalyl ethyl glycolate, methyl phthalyl ethyl glycolate, butyl phthalyl butyl glycolate and the like;
Examples of other carboxylic acid esters include polyhydric alcohol esters such as butyl oleate, methylacetyl ricinoleate, dibutyl sebacate, various trimellitate esters, trimethylolpropane tribenzoate, and trimethylolpropane tetrabenzoate. Can be. Among these, a phosphate plasticizer or a glycolate plasticizer is preferable.
[0182]
It is preferable to use these plasticizers alone or in combination.
The amount of the plasticizer used is preferably 1% by mass to 30% by mass based on the cellulose ester in view of film performance, processability and the like.
[0183]
Further, the in-line additive can be selected from the above-mentioned chemical formulas 2 to 39 and the ultraviolet absorber.
[0184]
(3) Dope preparation process:
The cellulose ester solution 100 and the in-line additive liquid 110 are transferred by liquid sending pumps 105 and 115, respectively, are transferred through conduits 108 and 117 filtered by filters 106 and 116, and are combined by a joining pipe 120. Since the combined liquids are transported in a layered form in the conduit, they are difficult to mix as they are. Therefore, in the present invention, after the two liquids are merged, they are transferred to the next step (4) while being sufficiently mixed by a mixer 121 such as an in-line mixer. As the in-line mixer that can be used in the present invention, for example, a static mixer SWJ (Toray static type in-tube mixer Hi-Mixer, manufactured by Toray Engineering) is preferable. When an in-line mixer is used, it can be applied to a dope in which a cellulose ester is concentrated and dissolved under high pressure.
[0185]
The above-mentioned dope preparation step is for preparing a dope containing fine particles, which is introduced into a layer containing fine particles, for example, a slit for a surface layer of a co-casting die. As a matter of course, for the dope of the layer containing no fine particles, an in-line additive liquid preparation step including a dispersion of the fine particles is preferably used, but an ultraviolet absorber may be added in-line instead of the fine particles. The number of such dope preparation steps, such as the type of cellulose ester, the concentration, the presence or absence of fine particles, the concentration of fine particles, the presence or absence of organic compound additives, the concentration of organic compounds, etc. Can be provided). In the co-casting die described later, the dope prepared by changing the components according to the purpose is supplied to each slit. The viscosity of the dope used for the base layer is preferably 50 to 10,000 Pa · s (at 35 ° C.), and particularly preferably 50 to 1,000 Pa · s. The viscosity of the dope used for the surface layer is preferably from 0.1 to 5,000 Pa · s, more preferably from 5 to 1,000 Pa · s, still more preferably from 10 to 500 Pa · s, particularly preferably from 10 to 500 Pa · s. 5050 Pa · s. In the present invention, the viscosity of the dope for the surface layer is preferably lower than that of the dope for the base layer.
[0186]
The dope preparation step 150 described in FIG. 5 is referred to as a preparation step A. For example, when the dope prepared in the preparation step A is a dope for a base layer, the dope is introduced into the inlet 202 of the base layer of the co-casting die 200, The respective dopes from the preparation step B and a similar preparation step C (not shown) are respectively introduced into the surface dope introduction ports 201 and 203 of the co-casting die 200 and subjected to co-casting. The dope preparation steps B and C may be the same as the dope preparation step A, or may be sent separately from one dope preparation step if the composition of the surface layer dope C is the same.
[0187]
FIG. 6 is a view showing steps after casting of the solution casting film forming apparatus according to the present invention. Hereinafter, an example of the production of the cellulose ester film according to the present invention will be described with reference to FIG.
[0188]
(4) Co-casting process:
As described above, the dopes prepared in the dope preparation steps B, A, and C are mixed and prepared by respective in-line mixers, and each dope is introduced into the co-casting die 200 through the inlets 201, 202, and 203, respectively. In a step of co-casting, for example, three layers of dope from a co-casting die 200 to a casting position on an endless metal support 204, for example, a stainless steel belt or a rotating metal drum, which is transferred to a metal support 204. is there. It is desirable that the surface of the metal support 204 be a mirror surface. The co-casting die 200 (for example, a pressure-type co-casting die) is preferable because three slit shapes in the die portion can be prepared and the film thickness can be easily made uniform. Examples of the co-casting die 200 include a coat hanger die and a T die, all of which are preferably used. In the case of sequential casting, two or more doping amounts are provided on the metal support 204 to supply a doping amount of two or more types to form a multilayer doped film.
[0189]
(5) Solvent evaporation step:
For example, a web 206 having a three-layer structure (the web is referred to as a dope film after casting the dope on the metal support) 206 is heated or cooled on the metal support 204 to form the web 206 from the metal support 204. This is a step of evaporating the solvent until the solvent can be peeled off. In order to evaporate the solvent, there are a method of blowing air to the web 206 and / or a method of transferring heat from the back surface of the metal support 204 by liquid or gas, a method of transferring heat from the front and back by radiant heat, and the like. The method is preferred because of its high drying efficiency. A method of combining them is also preferable. In the case of backside liquid heat transfer, it is preferable to heat the web at a temperature not higher than the boiling point of the main solvent of the organic solvent used in the dope or the organic solvent having the lowest boiling point. The surface temperature of the metal support for casting is 10 to 55 ° C., the temperature of the solution is 25 to 60 ° C., and the temperature of the solution is preferably equal to or higher than the temperature of the support, preferably 5 ° C. or higher. More preferably, the temperature is set at The higher the temperature of the solution and the temperature of the support, the higher the drying rate of the solvent can be. Therefore, if the temperature is too high, foaming or flatness may be deteriorated. The more preferred range of the temperature of the support depends on the organic solvent used, but it is preferably 20 to 55 ° C, and the more preferred range of the solution temperature is 35 to 45 ° C.
[0190]
(6) Peeling process:
In this step, the web 206 from which the solvent has evaporated on the metal support 204 is peeled off at a peeling position 205. The peeled web 206 is sent to the next step (7). If the residual solvent amount (the formula described below) of the web 206 at the time of peeling is too large, it is difficult to peel off. On the contrary, if it is dried too much on the metal support 204 and peeled off, it becomes difficult to peel off. A part of 206 is peeled off. In the present invention, when the thin web is peeled off from the metal support, it is preferable to peel the thin web with a force of 170 N / m or less from the lowest peelable tension as the peeling tension in order to prevent deterioration and flatness of the flatness. Forces within 140 N / m are more preferred.
[0191]
Gel casting (gel casting) is a method for increasing the film forming speed (the film forming speed can be increased because the film is separated while the residual solvent amount is as large as possible). Examples of the method include a method in which a poor solvent for the cellulose ester is added to the dope, gelling is performed after casting the dope, and a method in which the temperature of the metal support is lowered to gelate. By gelling on the metal support 204 to increase the strength of the film at the time of peeling, the peeling can be accelerated and the film forming speed can be increased. Drying of the web 206 on the metal support 204 can be peeled in the range of 5 to 150% by mass depending on the strength of the conditions, the length of the metal support 204, and the like, but peels off when the residual solvent amount is larger. In this case, if the web 206 is too soft, the flatness at the time of peeling may be impaired, or a fray or vertical streak may easily occur due to the peeling tension, and the amount of the residual solvent for peeling can be determined in consideration of economic speed and quality. Therefore, in the present invention, the temperature at the peeling position on the metal support 204 is preferably 10 to 40 ° C., more preferably 12 to 30 ° C., and the residual solvent amount of the web 206 at the peeling position is 10 to 120 ° C. It is preferable to set it as mass%.
[0192]
In order to maintain good flatness of the cellulose ester film at the time of production, the amount of the residual solvent when peeling from the metal support is preferably 10 to 150% by mass, more preferably 80 to 150% by mass. And more preferably 100 to 130% by mass. The ratio of the good solvent contained in the residual organic solvent of the web at the time of peeling is preferably 30 to 90%, more preferably 50 to 85%, and particularly preferably 60 to 80%.
[0193]
In the present invention, the amount of the residual solvent can be represented by the following equation.
Residual solvent amount (% by mass) = {(M−N) / N} × 100
Here, M is the mass of the web at any time, and the ratio of the components volatilized by drying can be determined by gas chromatography. N is the mass when the M was dried at 110 ° C. for 3 hours. The measurement is performed by gas chromatography with a headspace sampler connected. In the present invention, the measurement was performed under the following measurement conditions using a gas chromatography 5890 SERISII manufactured by Hewlett-Packard and a headspace sampler HP7694.
[0194]
Headspace sampler heating conditions: 120 ° C, 20 minutes
GC introduction temperature: 150 ° C
Temperature rise: 40 ° C, 5 minutes hold → 100 ° C (8 ° C / min)
Column: DB-WAX manufactured by J & W (inner diameter 0.32 mm, length 30 m).
[0195]
In the present invention, the drying time on the metal support of the web from casting to peeling of the dope is preferably within 120 seconds, more preferably 30 to 120 seconds, and further preferably 30 to 90 seconds. . The surface properties of the peeled web in this range are good, and when the metal compound thin film described below is applied to the dried cellulose ester film, the flatness is excellent, and there is no crack when repeatedly exposed to high temperature and high humidity conditions. An excellent optical film can be obtained.
[0196]
7) Drying process:
After the peeling, the web 206 is generally formed by using a roll drying device 208 that alternately transports the web 206 through rolls 209 arranged in zigzag and / or a tenter device 207 that transports the web 206 by clipping both ends of the web 206 with clips. dry. In FIG. 6, a roll drying device 208 is disposed after the tenter device 207. In general, hot air is blown to both sides of the web as a drying means, but there is also a method of heating by applying a microwave instead of the wind. Too fast drying tends to impair the flatness of the finished film. The drying temperature is generally in the range of 40 to 250 ° C, preferably at 110 to 160 ° C. The drying temperature, the amount of drying air, and the drying time vary depending on the solvent used, and the drying conditions may be appropriately selected according to the type and combination of the solvents used. Reference numeral 210 denotes a roll of the completed cellulose ester film. In the drying step of the cellulose ester film, the amount of the residual solvent is preferably adjusted to 1% by mass or less, and more preferably to 0.1% by mass or less and wound up.
[0197]
Although the above-described base sheet F has the base layer 22 and the surface layers 21 and 23 on both sides, it is also possible to manufacture the base sheet 22 alone or the base layer 22 and any surface layer. It works. FIGS. 7A, 7B, and 7C are schematic cross-sectional views of the optical film of the present invention prepared using such a base sheet.
[0198]
《Hard coat layer》
The hard coat layer (active ray curable resin layer) used in the present invention and applied on the base sheet will be described.
[0199]
The optical film of the present invention is characterized in that a metal compound layer is formed directly or via another layer on a cellulose ester film, as shown in FIGS. 7 (a), (b) and (c). It is more preferable to form via a hard coat layer (active ray curable resin layer) or another layer. As shown in the schematic diagram of FIG. 8, the application of the hard coat layer can be performed by two extrusion-type coating devices 401 and 402 arranged at different positions.
[0200]
The hard coat layer (active ray curable resin layer) may have various functions, and for example, may be an antiglare layer or a clear hard coat layer. The hard coat layer (active ray-curable resin layer) is preferably a layer formed by polymerizing a component containing at least one ethylenically unsaturated monomer.
[0201]
As a resin layer formed by polymerizing a component containing an ethylenically unsaturated monomer, a layer formed by curing an active ray-curable resin or a thermosetting resin is preferably used. It is a resin layer.
[0202]
Here, the actinic ray-curable resin layer refers to a layer mainly composed of a resin which is cured through a crosslinking reaction or the like by irradiation with actinic rays such as ultraviolet rays or electron beams.
[0203]
Typical examples of the actinic radiation curable resin include an ultraviolet curable resin and an electron beam curable resin, but a resin which is cured by irradiation with actinic rays other than ultraviolet rays and electron beams may be used.
[0204]
Examples of the ultraviolet-curable resin include an ultraviolet-curable acrylic urethane-based resin, an ultraviolet-curable polyester acrylate-based resin, an ultraviolet-curable epoxy acrylate-based resin, an ultraviolet-curable polyol acrylate-based resin, and an ultraviolet-curable epoxy resin. Can be.
[0205]
Specific examples include, for example, trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, and alkyl-modified dipentaerythritol pentaacrylate.
[0206]
As the UV-curable acrylic urethane resin, generally, a product obtained by reacting an isocyanate monomer or a prepolymer with a polyester polyol is further added with 2-hydroxyethyl acrylate and 2-hydroxyethyl methacrylate (hereinafter, acrylate includes methacrylate). And acrylate-based monomers having a hydroxyl group, such as 2-hydroxypropyl acrylate, which are easily formed. Examples of such a compound include those described in JP-A-59-151110. Can be used.
[0207]
Examples of the UV-curable polyester acrylate resin include those easily formed by reacting 2-hydroxyethyl acrylate and 2-hydroxy acrylate monomers with a polyester polyol, and disclosed in JP-A-59-151112. Can be used.
[0208]
Specific examples of the ultraviolet-curable epoxy acrylate-based resin include those formed by making epoxy acrylate an oligomer, adding a reactive diluent and a photoreaction initiator thereto, and reacting the oligomer. No. 105738 can be used.
[0209]
Specific examples of these photoreaction initiators include benzoin and derivatives, acetophenone, benzophenone, hydroxybenzophenone, Michler's ketone, α-amyloxime ester, thioxanthone, and the like, and derivatives thereof. You may use together with a photosensitizer.
[0210]
The photoinitiator described above can also be used as a photosensitizer. When an epoxy acrylate photoreactive agent is used, a sensitizer such as n-butylamine, triethylamine, and tri-n-butylphosphine can be used.
[0211]
Examples of the resin monomer include, as one monomer having one unsaturated double bond, general monomers such as methyl acrylate, ethyl acrylate, butyl acrylate, benzyl acrylate, cyclohexyl acrylate, vinyl acetate, and styrene. Further, monomers having two or more unsaturated double bonds include ethylene glycol diacrylate, propylene glycol diacrylate, divinylbenzene, 1,4-cyclohexane diacrylate, 1,4-cyclohexyldimethyl adiacrylate, and the above-mentioned trimethylolpropane. Examples thereof include triacrylate and pentaerythritol tetraacrylic ester.
[0212]
As the ultraviolet curable resin that can be used in the present invention, for example, Adeka Optomer KR / BY series: KR-400, KR-410, KR-550, KR-566, KR-567, BY-320B (Asahi Denka ( Koeihard A-101-KK, A-101-WS, C-302, C-401-N, C-501, M-101, M-102, T-102, D-102, NS -101, FT-102Q8, MAG-1-P20, AG-106, M-101-C (manufactured by Koei Chemical Co., Ltd.); Seika Beam PHC2210 (S), PHC X-9 (K-3), PHC2213, DP -10, DP-20, DP-30, P1000, P1100, P1200, P1300, P1400, P1500, P1600, SCR900 (Dainichi Chemical Industries KRM7033, KRM7039, KRM7130, KRM7131, UVECRYL29201, UVECRYL29202 (manufactured by Daicel UCB) Ltd .; RC-5015, RC-5016, RC-5020, RC-5031, RC-5100, RC-5102. , RC-5120, RC-5122, RC-5152, RC-5171, RC-5180, RC-5181 (manufactured by Dainippon Ink and Chemicals, Inc.); 340 Clear (China Paint Co., Ltd.); Sunrad H-601, RC-750, RC-700, RC-600, RC-501, RC-611, RC-612 (Sanyo Chemical Industry Co., Ltd.); SP -1509, SP-1507 (manufactured by Showa Polymer Co., Ltd.); RCC-15C (manufactured by Grace Japan), Aronix M-6100, M-8030, M-8060 (manufactured by Toagosei Co., Ltd.), etc. Can be appropriately selected from commercially available products.
[0213]
As described above, the ultraviolet ray curable resin layer has been particularly described, but the same effect can be obtained with other active ray resin layers.
[0214]
These actinic ray-curable resin layers can be applied by a known method.
As a light source for forming a cured film layer of the ultraviolet curable resin by a photocuring reaction, any light source that generates ultraviolet light can be used without limitation. For example, a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a carbon arc lamp, a metal halide lamp, a xenon lamp, and the like can be used. Irradiation conditions differ depending on each lamp, but the irradiation light amount is 20 to 10000 mJ / cm.2About 50 to 2000 mJ / cm.2It is. In the region from the near ultraviolet region to the visible light region, it can be efficiently formed by using a sensitizer having an absorption maximum in that region.
[0215]
As the organic solvent of the UV curable resin layer composition coating liquid, for example, hydrocarbons, alcohols, ketones, esters, glycol ethers, and other organic solvents are appropriately selected or mixed and used. it can. 5% by mass or more, more preferably 5 to 80%, of propylene glycol monoalkyl ether (1 to 4 carbon atoms in the alkyl group) or propylene glycol monoalkyl ether acetate (1 to 4 carbon atoms in the alkyl group). It is preferable to use the above-mentioned organic solvent containing the above-mentioned organic solvent by mass.
[0216]
As a method for applying the ultraviolet curable resin composition coating solution, the above-described extrusion type coating devices 401 and 402 shown in FIG. 8 can be used, but an appropriate coating amount is 0.1 to 30 μm as a wet film thickness. Preferably, it is 0.5 to 15 μm.
[0217]
The UV-curable resin composition to be applied is preferably irradiated with UV light by UV irradiation devices 403 and 404 during or after coating and drying, as shown in FIG. 5 minutes is preferable, and 0.1 second to 10 seconds is more preferable from the viewpoint of the curing efficiency of the ultraviolet curable resin, the working efficiency, and the productivity.
[0218]
To the cured resin layer thus obtained, in order to prevent blocking, to enhance abrasion resistance or the like, or to impart antiglare properties, it is possible to add fine particles of an inorganic compound or an organic compound. The type is almost the same as the above-mentioned fine particles of the matting agent.
[0219]
The average particle size of these fine particle powders is preferably from 0.005 μm to 5 μm, and particularly preferably from 0.01 to 1 μm. It is preferable that two or more kinds of particles having different particle diameters and different materials (refractive index) are contained.
[0220]
The ratio of the ultraviolet curable resin composition to the fine particle powder is preferably 0.1 to 10 parts by mass based on 100 parts by mass of the resin composition.
[0221]
The ultraviolet curable resin layer may be a clear hard coat layer having a center line average roughness (Ra) defined by JIS B 0601 of 1 to 50 nm or an antiglare layer having a Ra of 0.1 to 1 μm. Good.
[0222]
The ultraviolet curing resin layer is formed by coating two or more layers. Thereby, a hard coat layer having more excellent hardness and friction resistance can be formed. The hard coat layer preferably has a pencil hardness of 2H or more, particularly preferably 3H to 6H. Further, if necessary, a hard coat layer can be applied to both surfaces of the cellulose ester film.
[0223]
Fine particles may be added to the upper ultraviolet curable resin layer for imparting antiglare properties, or fine particles may be added to both layers.
[0224]
The additive of the active ray resin layer of the hard coat layer will be described.
The amount of the plasticizer contained in the lower hard coat layer is preferably 0.5 to 12% by mass, particularly preferably 1 to 10% by mass. The plasticizer can be added in advance to the hard coat coating solution. Alternatively, a plasticizer is applied to the surface of the plastic substrate in advance by applying, spraying, or other method, and then the lower active ray-curable resin layer is applied thereon, so that the lower active ray-curable resin layer contains the plasticizer. Can be contained. The upper active ray-curable resin layer preferably does not contain a plasticizer, but may contain some plasticizer eluted from the lower layer. As the plasticizer, a plasticizer such as a cellulose ester which can be added to a base sheet is preferably used.
[0225]
In the present invention, when forming the two hard coat layers, the second layer is also continuously formed without winding after completion of the coating of the first layer, thereby reducing the unevenness of the metal compound layer formed thereon. Thus, the color unevenness of the reflected light can be further reduced.
[0226]
When two hard coat layers are continuously formed, it is preferable that the lower hard coat layer is irradiated with ultraviolet rays after application and drying to be in a half-cured state, and the upper hard coat layer is formed thereon.
[0227]
Furthermore, in the present invention, a method of forming a metal compound layer on the hard coat layer by plasma discharge treatment is particularly preferably used.
[0228]
Hereinafter, a method of forming a metal compound layer by a plasma discharge process will be described with reference to FIGS.
[0229]
FIG. 9 is a schematic view showing an example of a jet type atmospheric pressure plasma discharge processing apparatus useful for the present invention.
[0230]
The jet type atmospheric pressure plasma discharge processing apparatus is not shown in FIG. 9 (illustrated in FIG. 11 to be described later) in addition to the plasma discharge processing apparatus and the voltage applying means having two power supplies. And an apparatus having an electrode temperature adjusting means.
[0231]
The plasma discharge processing device 310 has a counter electrode composed of a first electrode 311 and a second electrode 312, and a first power source 321 from the first electrode 311 between the counter electrodes. Frequency ω1High frequency voltage V1Is applied, and the second frequency ω from the second power source 322 is applied from the second electrode 312.2High frequency voltage V2Is applied. The first power supply 321 has a higher frequency voltage (V) than the second power supply 322.1> V2) May be applied, and the first frequency ω of the first power supply 321 may be used.1And the second frequency ω of the second power source 3222The relationship is ω12It is.
[0232]
The current I from the first power supply 321 is provided between the first electrode 311 and the first power supply 321.1The first filter 323 is installed so that the current flows toward the first electrode 311, and the current I1From the second power supply 322.2Is designed to make it easier to pass to the ground side.
[0233]
The current I from the second power source 322 is provided between the second electrode 312 and the second power source 322.2The second filter 324 is provided so that the current flows toward the second electrode 312.2From the first power supply 321.1To the earth side.
[0234]
Gas G is introduced from a gas supply means into a space 313 between the opposing electrodes (discharge space) between the first electrode 311 and the second electrode 312, and a high-frequency voltage is applied to the first electrode 311 and the second electrode 312 to generate a discharge. Then, the gas G is brought into a plasma state, and is blown in a jet shape below the counter electrode (below the paper surface) to form a thin film near the processing position 314 on the hard coat layer applied to the base sheet F. Depending on the temperature of the substrate sheet F during the plasma discharge treatment, the physical properties and composition of the obtained thin film may change, and it is desirable to appropriately control the change. As a temperature control medium, an insulating material such as distilled water or oil is preferably used. During the plasma discharge treatment, it is desired to uniformly adjust the temperature of the surface of the electrode and the temperature of the surface of the substrate sheet so as to minimize the unevenness of the substrate temperature in the width direction or the longitudinal direction.
[0235]
FIG. 9 shows a measuring instrument used for measuring the high-frequency voltage (applied voltage) and the discharge starting voltage described above. 325 and 326 are high frequency probes, and 327 and 328 are oscilloscopes.
[0236]
By arranging a plurality of the jet-type atmospheric pressure plasma discharge processing devices in series and arranging them in series, it is possible to continuously perform high-speed processing. If each device jets a different gas, it is possible to form a laminated thin film having different layers.
[0237]
FIG. 10 is a schematic view showing an example of another atmospheric pressure plasma discharge processing apparatus useful for the present invention.
[0238]
This atmospheric pressure plasma discharge processing apparatus has at least a plasma discharge processing apparatus 330, a voltage applying unit 340 having two power supplies, a gas supply unit 350, and an electrode temperature adjusting unit 360.
[0239]
Between the counter electrode (discharge space) 332 between the roll rotating electrode (first electrode) 335 and the rectangular cylindrical fixed electrode group (second electrode) 336, a metal compound thin film is formed on the base sheet F by plasma discharge treatment. can do.
[0240]
The roll rotating electrode (first electrode) 335 receives the frequency ω from the first power source 341.1High frequency voltage V1And a square cylindrical fixed electrode group (second electrode) 336 from the second power source 342 to the frequency ω.2High frequency voltage V2Can be applied.
[0241]
The current I from the first power supply 341 is supplied between the roll rotating electrode (first electrode) 335 and the first power supply 341.2A first filter 343 is provided so that the current flows toward the roll rotating electrode (first electrode) 335.1From the second power source 342.2To the earth side. In addition, a current I from the second power source is supplied between the square cylindrical fixed electrode group (second electrode) 336 and the second power source 342.2The second filter 344 is provided so that the current flows toward the second electrode.2From the first power supply 341.1To the earth side.
[0242]
The roll rotation electrode 335 may be used as a second electrode, and the rectangular cylindrical fixed electrode group 336 may be used as a first electrode. In any case, a first power supply is connected to the first electrode, and a second power supply is connected to the second electrode. The first power supply has a higher frequency voltage (V) than the second power supply.1> V2) Can be applied, and the frequency is ω12It has the ability to become.
[0243]
The gas G generated by the gas supply device 351 of the gas supply means 350 is supplied from the space between the fixed electrodes 336 to the space between the opposed electrodes 332 from the air supply port 352 by controlling the flow rate. Exhaust gas G 'is exhausted from between the opposed electrodes. However, the gas supply ports 352 and the gas exhaust ports 353 are preferably provided alternately between the fixed electrodes 336.
[0244]
The base sheet F on which the hard coat layer is formed is unwound from an original winding (not shown) and conveyed, or is conveyed from a previous process, and is passed through a guide roll 364 to a nip roll 365 to be applied to the base material. The entrained air and the like are cut off and transferred between the rectangular cylindrical fixed electrode group 336 while being wound while being in contact with the roll rotary electrode 335, and the roll rotary electrode (first electrode) 335 and the rectangular cylindrical fixed electrode A voltage is applied from both the group (second electrode) 336 and discharge plasma is generated between the counter electrodes (discharge space) 332. The base sheet F on which the hard coat layer is formed forms a thin film with a gas in a plasma state while being wound while being in contact with the roll rotating electrode 335. The base sheet F passes through a nip roll 366 and a guide roll 367 and is wound by a winder (not shown) or transferred to the next step.
[0245]
During the formation of the thin film, the medium whose temperature has been adjusted by the electrode temperature adjusting means 360 in order to heat or cool the roll rotating electrode (first electrode) 335 and the rectangular cylindrical fixed electrode group (second electrode) 336 is supplied by a liquid feed pump. P sends to both electrodes via a pipe 361 and adjusts the temperature from the inside of the electrodes. The temperature of the roll rotating electrode 335 and the fixed electrode group 336 can be independently adjusted. Note that reference numerals 368 and 369 denote partition plates that partition the plasma discharge processing container 331 from the outside.
[0246]
FIG. 11 is a perspective view showing an example of the structure of the conductive metal base material of the roll rotating electrode shown in FIG. 10 and the dielectric material coated thereon.
[0247]
In FIG. 11, a roll electrode 335a has a conductive metal base material 335A and a dielectric 335B coated thereon. The inside is a hollow jacket that allows temperature adjustment by circulating a temperature adjustment medium.
[0248]
FIG. 12 is a perspective view showing an example of the structure of a conductive metallic base material of a rectangular cylindrical electrode and a dielectric material coated thereon.
[0249]
In FIG. 12, a rectangular cylindrical electrode 336a has a coating of a dielectric 336B similar to that of FIG. 11 on a conductive metal base material 336A, and the structure of the electrode is a metal pipe. Is a jacket so that temperature control during discharge can be performed.
[0250]
The number of the rectangular cylindrical fixed electrodes is plural along the circumference larger than the circumference of the roll electrode, and the discharge area of the electrode is a full-width cylindrical type electrode facing the roll rotating electrode 335. It is expressed as the sum of the areas of the fixed electrode surfaces.
[0251]
The prismatic electrode 336a shown in FIG. 10 may be a cylindrical electrode, but the prismatic electrode 336a is preferably used in the present invention because it has an effect of expanding the discharge range (discharge area) as compared with the cylindrical electrode. .
[0252]
11 and 12, a roll electrode 335a and a rectangular cylindrical electrode 336a are formed by spraying ceramics as dielectrics 335B and 336B on conductive metallic base materials 335A and 336A, respectively, and then using a sealing material of an inorganic compound. It was used for sealing. The thickness of the ceramic dielectric is 0.1 to 5 mm, preferably 1 to 3 mm. As the ceramic material used for thermal spraying, alumina, silicon nitride, or the like is preferably used. Among them, alumina is particularly preferably used because alumina is easily processed. Further, the dielectric layer may be a lining treated dielectric provided with an inorganic material by glass lining.
[0253]
Examples of the conductive metallic base materials 335A and 336A include metals such as titanium metal or titanium alloy, silver, platinum, stainless steel, aluminum, and iron, a composite material of iron and ceramics, or a composite material of aluminum and ceramics. Etc., but titanium metal or a titanium alloy is particularly preferred for the reasons described below.
[0254]
The distance between the two electrodes (electrode gap) is determined in consideration of the thickness of the dielectric provided on the conductive metal base material, the magnitude of the applied voltage, the purpose of utilizing the plasma, and the like. The shortest distance between the dielectric surface when a dielectric is provided on one of the electrodes and the surface of the conductive metal base material, and the distance between the dielectric surfaces when the dielectric is provided on both of the electrodes, Also in this case, the thickness is preferably 0.1 nm to 20 mm, particularly preferably 0.5 nm to 2 mm, from the viewpoint of performing uniform discharge.
[0255]
The details of the conductive metallic base material and the dielectric material useful in the present invention will be described later.
[0256]
As the plasma discharge processing container 331, a processing container made of Pyrex (R) glass or the like is preferably used, but a metal container can be used as long as insulation from the electrodes can be obtained. For example, a polyimide resin or the like may be attached to the inner surface of an aluminum or stainless steel frame, and the metal frame may be sprayed with ceramics to obtain insulation. In FIG. 9, it is preferable to cover both side surfaces (up to near the base material surface) of both parallel electrodes with the above-mentioned material.
[0257]
As the first power supply (high-frequency power supply) installed in the atmospheric pressure plasma discharge treatment apparatus of the present invention, a power supply having a frequency of 1 to 200 kHz is preferably used.
Applied power supply symbol Manufacturer Frequency
A1 Shinko Electric 3kHz
A2 Shinko Electric 5kHz
A3 Kasuga Electric 15kHz
A4 Shinko Electric 50kHz
A5 Heiden Institute 100kHz *
A6 Pearl Industry 200kHz
And the like, and any of them can be used. In addition, * mark is a HEIDEN laboratory impulse high frequency power supply (100 kHz in continuous mode).
[0258]
As the second power supply (high-frequency power supply), a power supply having a frequency of 800 kHz or more is preferably used.
Applied power supply symbol Manufacturer Frequency
B1 Pearl Industry 800kHz
B2 Pearl Industry 2MHz
B3 Pearl Industry 13.56MHz
B4 Pearl Industry 27MHz
B5 Pearl Industry 150MHz
And the like, and any of them can be preferably used.
[0259]
By applying such a voltage, a glow discharge state can be maintained.
In the present invention, the power applied between the opposing electrodes is 1 W / cm2It is preferable to supply the above-mentioned electric power (output density), whereby the discharge gas is excited to generate plasma, and energy is given to the thin film forming gas to form a thin film. The power to be supplied is 1 to 50 W / cm2Is preferred. The discharge area (cm2) Refers to the area of the range in which discharge occurs in the electrode.
[0260]
Here, as a method of applying the high-frequency voltage, either a continuous sine wave continuous oscillation mode 0 called a continuous mode or an intermittent oscillation mode in which ON / OFF is intermittently called a pulse mode may be adopted. On the second electrode side, a continuous sine wave is preferable because a denser and higher quality film can be obtained.
[0261]
Electrodes used in such a thin film formation method using atmospheric pressure plasma must be able to withstand severe conditions in terms of structure and performance. Such an electrode is preferably a metal base material coated with a dielectric.
[0262]
In the dielectric-coated electrode used in the present invention, it is preferable that the characteristics match between various metallic base materials and the dielectric. One of the characteristics is the linear thermal expansion between the metallic base material and the dielectric. The coefficient difference is 10 × 10-6/ ° C or lower. Preferably 8 × 10-6/ ° C or lower, more preferably 5 × 10-6/ ° C or lower, more preferably 2 × 10-6/ ° C or lower. The linear thermal expansion coefficient is a physical property value of a known material.
[0263]
The difference between the coefficients of linear thermal expansion is as follows:
Figure 2004203009
Etc. From the viewpoint of the difference in linear thermal expansion coefficient, the above (a) or (b) and (e) to (h) are preferable, and (a) is particularly preferable.
[0264]
In the present invention, titanium or a titanium alloy is particularly useful as the metallic base material from the above characteristics. By using titanium or titanium alloy as the metallic base material, and by setting the dielectric material to the above, there is no deterioration of the electrode during use, especially cracking, peeling, falling off, etc., and it is used for a long time under severe conditions Can withstand.
[0265]
The metallic base material of the electrode useful in the present invention is a titanium alloy or titanium metal containing 70% by mass or more of titanium. In the present invention, the content of titanium in the titanium alloy or titanium metal can be used without any problem as long as it is 70% by mass or more, but preferably contains 80% by mass or more of titanium. As the titanium alloy or titanium metal useful in the present invention, those generally used as industrial pure titanium, corrosion-resistant titanium, high-strength titanium and the like can be used. Examples of industrial pure titanium include TIA, TIB, TIC, TID, etc., all of which contain very little iron atom, carbon atom, nitrogen atom, oxygen atom, hydrogen atom and the like. The content is 99% by mass or more. As the corrosion-resistant titanium alloy, T15PB can be preferably used, which contains lead in addition to the above contained atoms, and has a titanium content of 98% by mass or more. As the titanium alloy, in addition to the above-mentioned atoms except for lead, T64, T325, T525, TA3, and the like containing aluminum and containing vanadium and tin can be preferably used. The amount is 85% by mass or more. These titanium alloys or titanium metals have a coefficient of thermal expansion smaller than that of stainless steel, for example, AISI 316, by about 1/2, and are combined with a later-described dielectric applied on the titanium alloy or titanium metal as a metallic base material. It can withstand high temperature and long time use.
[0266]
On the other hand, the properties required of the dielectric are, specifically, preferably an inorganic compound having a relative dielectric constant of 6 to 45. Examples of such a dielectric include ceramics such as alumina and silicon nitride. Alternatively, there are glass lining materials such as silicate glass and borate glass. Among these, those obtained by spraying ceramics described later and those provided by glass lining are preferable. In particular, a dielectric provided by spraying alumina is preferable.
[0267]
Alternatively, as one of the specifications that can withstand the large power as described above, the porosity of the dielectric is 10% by volume or less, preferably 8% by volume or less, preferably more than 0% by volume and 5% by volume or less. It is. The porosity of the dielectric can be measured by a BET adsorption method or a mercury porosimeter. In the examples described later, the porosity is measured using a piece of a dielectric material coated on a metallic base material using a mercury porosimeter manufactured by Shimadzu Corporation. High durability is achieved by the dielectric having a low porosity. Examples of the dielectric having such voids and low porosity include a ceramic sprayed coating having a high density and a high adhesion by an atmospheric plasma spraying method described later. In order to further reduce the porosity, it is preferable to perform a sealing treatment.
[0268]
The above-described atmospheric plasma spraying method is a technique in which fine powders such as ceramics, wires, and the like are charged into a plasma heat source, and are sprayed as fine particles in a molten or semi-molten state on a metal base material to be coated to form a film. The plasma heat source is a high-temperature plasma gas in which a molecular gas is heated to a high temperature, dissociated into atoms, and further applied with energy to emit electrons. This plasma gas is sprayed at a high speed, and the sprayed material collides with the metal base material at a higher speed than conventional arc spraying or flame spraying, so that a high adhesion strength and a high-density coating can be obtained. For details, reference can be made to the thermal spraying method for forming a heat shielding film on a high-temperature exposed member described in JP-A-2000-301655. According to this method, the porosity of the dielectric material (ceramic sprayed film) to be coated as described above can be obtained.
[0269]
Another preferable specification that can withstand high power is that the thickness of the dielectric is 0.5 to 2 mm. This variation in film thickness is desirably 5% or less, preferably 3% or less, and more preferably 1% or less.
[0270]
In order to further reduce the porosity of the dielectric, it is preferable that the sprayed film of ceramic or the like is further subjected to sealing treatment with an inorganic compound as described above. As the inorganic compound, metal oxides are preferable, and among them, silicon oxide (SiO 2) is particularly preferable.x) Is preferable.
[0271]
It is preferable that the inorganic compound for the pore-sealing treatment is formed by curing by a sol-gel reaction. In the case where the inorganic compound for the sealing treatment contains a metal oxide as a main component, a metal alkoxide or the like is applied as a sealing liquid on the ceramic sprayed film and cured by a sol-gel reaction. When the inorganic compound is mainly composed of silica, it is preferable to use alkoxysilane as the sealing liquid.
[0272]
Here, it is preferable to use energy treatment to promote the sol-gel reaction. Examples of the energy treatment include thermal curing (preferably 200 ° C. or lower) and ultraviolet irradiation. Further, as a sealing treatment method, when the sealing liquid is diluted and coating and curing are repeated several times sequentially, the mineralization is further improved, and a dense electrode without deterioration can be obtained.
[0273]
In the case where a sealing treatment is performed by coating a ceramic sprayed film with a metal alkoxide or the like of the dielectric coated electrode according to the present invention as a sealing liquid and then performing a sealing treatment by a sol-gel reaction, the content of the cured metal oxide is 60%. It is preferably at least mol%. When alkoxysilane is used as the metal alkoxide of the sealing liquid, the cured SiO 2x(X is 2 or less) The content is preferably 60 mol% or more. SiO after curingxThe content can be measured by analyzing a slice of the dielectric layer by XPS (X-ray photoelectron spectrum).
[0274]
In the electrode according to the method for producing an optical film of the present invention, the electrode is adjusted so that the maximum height (Rmax) of the surface roughness defined by JIS B0601 at least on the side in contact with the substrate is 10 μm or less. Is preferably, but more preferably 8 μm or less, and particularly preferably adjusted to 7 μm or less. In this way, the thickness of the dielectric and the gap between the electrodes can be kept constant by the method of polishing and finishing the dielectric surface of the dielectric coated electrode, and the discharge state can be stabilized. Distortion and cracks due to residual stress can be eliminated, and high accuracy and durability can be greatly improved. The polishing finish of the dielectric surface is preferably performed at least on the dielectric in contact with the base material.
[0275]
Another preferable specification of the dielectric-coated electrode used in the present invention that withstands large power is that the heat-resistant temperature is 100 ° C. or higher. It is more preferably at least 120 ° C, particularly preferably at least 150 ° C. The upper limit is 500 ° C. Note that the heat-resistant temperature refers to the highest temperature that can withstand a state in which dielectric breakdown does not occur and discharge can be performed normally. Such a heat-resistant temperature is within the range of the above-described ceramic thermal spraying, a dielectric provided with a layered glass lining having a different amount of bubbles mixed therein, or a difference in a linear thermal expansion coefficient between the metal base material and the dielectric described below. It can be achieved by appropriately combining means for appropriately selecting the above materials.
[0276]
《Reactive gas》
The reaction gas used for forming the metal compound layer of the present invention will be described.
[0277]
The reaction gas for forming the thin film layer is a gas mainly containing nitrogen. That is, the content of nitrogen gas is preferably 50% or more, more preferably 70% or more, and even more preferably 90% to 99.99% by volume. The reaction gas may contain a rare gas in addition to nitrogen.
[0278]
Here, the rare gas is an element belonging to Group 18 of the periodic table, specifically, helium, neon, argon, krypton, xenon, radon, or the like. In the present invention, helium, argon, or the like is added to nitrogen. May be used.
[0279]
Nitrogen gas is used to generate a stable plasma discharge, and a reactive gas (raw material gas) is added to the reactive gas as a raw material for forming a thin film. The reactive gas is ionized or radicalized in the plasma, and forms a thin film by depositing or adhering to the surface of the substrate.
[0280]
Further, the reaction gas contains 0.1% to 10% by volume of oxygen, hydrogen, carbon dioxide, carbon monoxide, nitrogen dioxide, nitrogen monoxide, water, hydrogen peroxide, ozone, methane, tetrafluoromethane and the like. By doing so, physical properties such as hardness and density of the thin film layer can be controlled.
[0281]
By using a reaction gas useful in the present invention to which a source gas of various substances is added, thin films having various functions can be formed on a substrate such as a cellulose ester film. The source gas referred to here is a gas for forming a thin film by a plasma treatment, and means a gas of a metal compound when a metal compound layer such as a metal oxide, a metal nitride, or a metal oxynitride is formed.
[0282]
The organometallic compound as a source gas useful in the present invention is not particularly limited, but Al, As, Au, B, Bi, Sb, Ca, Cd, Cr, Co, Cu, Fe, Ga, Ge, Hg, Metals for forming metal oxides such as In, Li, Mg, Mn, Mo, Na, Ni, Pb, Pt, Rh, Se, Si, Sn, Ti, Zr, Y, V, W, Zn, Ta Compounds can be mentioned.
[0283]
For example, using an organic metal compound, a metal hydride, a metal halide, or a metal complex containing Ti, Zr, In, Sn, Zn, Ge, Si, Ta, or another metal, these metal oxide layers (here, The metal oxide layer may include a metal oxide nitride layer), a metal nitride layer, or the like, and these layers may be a medium refractive index layer or a high refractive index layer of an antireflection layer, Alternatively, it can be a transparent conductive layer or an antistatic layer.
[0284]
Further, the antifouling layer and the low-refractive-index layer can be formed with a fluorine-containing organic compound, and the gas barrier layer, the low-refractive-index layer and the antifouling layer can be formed with a silicon compound. The present invention is particularly preferably used for forming an antireflection layer formed by alternately stacking high and medium refractive index layers and low refractive index layers.
[0285]
In the present invention, when an organometallic compound is used as the reactive gas, from the viewpoint of forming a uniform thin film on a base sheet such as a cellulose ester film by plasma discharge treatment, the metal compound as a source gas in the reaction gas is used. The content is preferably from 0.01 to 10% by volume, and more preferably from 0.1 to 5% by volume.
[0286]
(Source gas)
The source gas will be described in more detail.
[0287]
In order to form a high refractive index layer of the antireflection layer, a titanium compound, a zirconium compound, and a tantalum compound are preferable. Specifically, for example, an organic amino metal compound such as tetradimethylaminotitanium, and a metal such as monotitanium and dititanium Hydrogen compounds, metal halides such as titanium dichloride, titanium trichloride, titanium tetrachloride, tetraethoxytitanium, tetraisopropoxytitanium, tetrabutoxytitanium, tetraethoxyzirconium, tetraisopropoxyzirconium, tetrabutoxyzirconium, pentaisopropoxytantalum And a metal alkoxide such as pentaethoxy tantalum, and the like, and a metal oxide layer can be formed using these.
[0288]
Examples of the zinc compound include zinc acetylacetonate, diethyl zinc, and dimethyl zinc. Examples of the tin compound include tetraethyltin, tetramethyltin, di-n-butyltin diacetate, and dibutyl bis (2-ethylhexanoate). Organotin compounds such as tin, dibutyltin diacetate, dibutyltin oxide, dibutyltin dilaurate, tetramethyltin, tetraethyltin, tetrabutyltin, tetrapropyltin, and tetraoctyltin are preferably used, and the indium compound is triethylindium. And trimethylindium are preferably used.
[0289]
(Fluorine compound)
In the atmospheric pressure plasma treatment, a fluorine compound-containing layer can be formed by using a fluorine-containing organic compound as a source gas.
[0290]
As the fluorine-containing organic compound, a fluorocarbon gas, a fluorohydrocarbon gas, or the like is preferable.
[0291]
Specifically, examples of the fluorine-containing organic compound include carbon fluoride compounds such as carbon tetrafluoride, carbon hexafluoride, ethylene tetrafluoride, hexafluoropropylene, and cyclobutane octafluoride;
Fluorohydrocarbon compounds such as methane difluoride, ethane tetrafluoride, propylene tetrafluoride, propylene trifluoride, and cyclobutane octafluoride;
Further, mention may be made of halides of fluorinated hydrocarbon compounds such as methane monochloride trifluoride, methane monochloride difluoromethane and cyclobutane dichloride, and fluorine-substituted organic compounds such as alcohols, acids and ketones. Can be.
[0292]
These may be used alone or as a mixture. Examples of the fluorinated hydrocarbon gas include methane difluoride, ethane tetrafluoride, propylene tetrafluoride, and propylene trifluoride.
[0293]
Further, it is possible to use a fluoride of a hydrocarbon compound such as trifluoromethane trifluoride, methane dichloride methane, or cyclobutane difluoride or a fluorine-substituted organic compound such as alcohol, acid or ketone. Although possible, the present invention is not limited to these.
[0294]
Further, these compounds may have an ethylenically unsaturated group in the molecule. Further, the above compounds may be used as a mixture.
[0295]
When a fluorine-containing organic compound is used as the reactive gas useful in the present invention, from the viewpoint of forming a uniform thin film on the cellulose ester film by plasma discharge treatment, the fluorine-containing organic compound is contained as a reactive gas in the reaction gas. The ratio is preferably from 0.01 to 10% by volume, and more preferably from 0.1 to 5% by volume.
[0296]
When the fluorine-containing organic compound preferably used in the present invention is a gas at normal temperature and normal pressure, it can be used as it is as a reactive gas component.
[0297]
Further, when the fluorine-containing organic compound is a liquid or solid at normal temperature and normal pressure, it may be used by evaporating it by a vaporizing means, for example, heating, reducing pressure, or the like, or may be used by dissolving in an appropriate organic solvent .
[0298]
(Silicon compound)
Examples of the silicon compound as a reactive gas useful in the present invention include, for example, dimethylsilane, organometallic compounds such as tetramethylsilane, metal hydrogen compounds such as monosilane and disilane, silane dichloride, silane trichloride, and silicon tetrafluoride. Metal silanes such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, dimethyldiethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, etc., alkoxysilane, tetramethylsilane, hexamethyldiamine It is preferable to use fluoroalkylsilanes such as 3,3,3-trifluoromethyltrimethoxysilane such as siloxane and organosilane, but not limited thereto.
[0299]
These can be used in appropriate combination. Alternatively, the properties of the film can be changed or controlled by adding another organic compound.
[0300]
In order to introduce a metal compound such as a silicon compound, a titanium compound, a zirconium compound, and a tantalum compound into the discharge portion, both of them can be used in a gas, liquid or solid state at normal temperature and normal pressure.
[0301]
In the case of gas, it can be directly introduced into the discharge section, but in the case of liquid or solid, it can be used after being vaporized by vaporizing means such as heating, decompression, and ultrasonic irradiation. Commercial vaporizers are preferably used for this purpose.
[0302]
When a metal compound such as a silicon compound and a titanium compound is vaporized by heating and used, a metal alkoxide which is liquid at ordinary temperature, such as tetraethoxysilane and tetraisopropoxytitanium, and has a boiling point of 200 ° C. or less is used in the present invention. It is suitable for a method of forming a metal oxide thin film layer. The metal alkoxide may be used after being diluted with an organic solvent. As the organic solvent, an organic solvent such as methanol, ethanol, n-hexane, acetone or a mixed organic solvent thereof can be used.
[0303]
(Thickness of metal compound layer)
The thickness of the metal compound layer according to the present invention is preferably in the range of 1 nm to 1000 nm.
[0304]
Such a metal compound layer can be, for example, a low refractive index layer or an antiglare layer and a high refractive index layer laminated to form an antireflection layer, or a transparent conductive layer or an antistatic layer.
[0305]
In the present invention, by providing a plurality of plasma discharge devices, a multilayer thin film can be continuously provided, and a multilayer laminate can be formed without unevenness of the thin film. For example, it is preferable to form the next layer within one minute after forming one layer. In order to form a plurality of layers continuously in one pass, it is necessary to adjust each layer to a predetermined thin film forming speed. Therefore, it is preferable to measure the film thickness after forming each layer or measure the reflection spectrum, and to perform feedback control of the thin film formation speed based on the result. Thus, thin films having different compositions or different thicknesses can be continuously formed in one pass on the base film conveyed at a constant speed. Although there is no particular limitation on the method of controlling the thin film formation rate of each layer,
Discharge conditions such as applied voltage, current, frequency and pulse conditions of discharge, ratio of each component in the reaction gas (addition gas concentration, type, source gas concentration such as nitrogen concentration, oxygen or hydrogen), reaction gas supply amount, electrode Examples include, but are not limited to, the distance between the electrodes, the pressure of the discharge unit, the temperature of the substrate, the temperature of the electrode, the temperature of the reaction gas, the temperature of the discharge unit, and the change of the discharge area. By appropriately combining one or more of these conditions, the thin film formation speed can be controlled without greatly changing the quality of the thin film to be formed.
[0306]
For example, when producing an optical film having an antireflection layer on a cellulose ester film, a high refractive index layer having a refractive index of 1.6 to 2.3 and a low refractive index layer having a refractive index of 1.3 to 1.5 are formed of cellulose. It can be continuously laminated on the surface of the ester film and efficiently produced.
[0307]
As the low refractive index layer, a fluorine-containing compound layer formed by plasma discharge treatment of a gas containing a fluorine-containing organic compound, or silicon oxide formed mainly by plasma discharge treatment using an organosilicon compound such as alkoxysilane is used. Preferably, the high refractive index layer is a metal oxide layer formed by plasma discharge treatment of a gas containing an organometallic compound, for example, a layer mainly containing titanium oxide, zirconium oxide, and tantalum oxide. These layers may contain carbon or carbon compounds in the source gas.
[0308]
The present invention is not limited to these, and the layer configuration is not limited to these. For example, an antifouling layer may be provided on the outermost surface by performing a plasma discharge treatment at atmospheric pressure or a pressure near the atmospheric pressure in the presence of a fluorine-containing organic compound gas. Alternatively, a known antifouling layer, for example, a composition containing a fluoroalkylsilane or the like can be applied.
[0309]
According to the method described above, in the present invention, a multilayer thin film can be laminated, and a uniform optical film can be obtained without unevenness in the thickness of each layer.
[0310]
The thickness of the thin film such as a metal oxide layer can be determined by preparing a cross section of the stacked body and observing it with a transmission electron microscope (hereinafter, referred to as a TEM).
[0311]
The cross section was prepared by embedding the laminated body together with the base material in an epoxy-embedded resin for pre-processing by electron microscopic observation, and using an ultramicrotome equipped with a diamond knife, an ultra-thin section of about 80 nm in thickness. Or by using a focused ion beam (FIB) processing device to focus and scan the surface of the laminate with a Ga ion beam and cut out a thinned cross section having a thickness of about 100 nm. it can.
[0312]
Observation by TEM involves observing a bright field image at a magnification of 50,000 to 500,000, and recording the image on a film, imaging plate, CCD camera, or the like.
[0313]
The acceleration voltage of the TEM is preferably from 80 to 400 kV, particularly preferably from 80 to 200 kV.
[0314]
For details on electron microscopy techniques and sample preparation techniques, see "The Electron Microscopy Society of Japan, Kanto Chapter / Medical and Biological Electron Microscopy" (Maruzen), "The Japan Electron Microscopy Society of Kanto Chapter," Electron Microscopy Biological Specimens Preparation method ”(Maruzen) and“ Electron microscope Q & A ”(Agne Shofusha) can be referred to respectively.
[0315]
Regarding the TEM image recorded on an appropriate medium, it is preferable that one image is decomposed into at least 1024 pixels × 1024 pixels, preferably 2048 pixels × 2048 pixels or more, and image processing is performed by a computer.
[0316]
The details of the image processing technology can be referred to “Hiroshi Tanaka, Image Processing Application Technology (Industry Research Committee)”. The image processing program or device is not particularly limited as long as it can perform the above operations. Image analysis software Image-Pro PLUS manufactured by CYBERNETICS (USA).
[0317]
In order to perform image processing, it is preferable that an analog image recorded on a film is converted into a digital image by a scanner or the like, and shading correction, contrast / edge enhancement, and the like are performed as necessary. Thereafter, a histogram is prepared, a portion corresponding to the interface of the stacked body is extracted by a binarization process, and a width (Thickness) between the interfaces is measured.
[0318]
Similarly, the average film thickness and its variation can be calculated from the values obtained for at least 25 or more, preferably 50 or more.
[0319]
As described above, in the present invention, an optical film on which metal oxide layers having various functions are formed can be provided.
[0320]
According to the present invention, streak-like failure of the metal compound layer is remarkably improved, an optical film with less cracks and excellent scratch resistance can be provided, and an optical film with significantly improved color unevenness of reflected light can be provided. Could be provided.
[0321]
【Example】
Hereinafter, the present invention will be described specifically with reference to examples, but embodiments of the present invention are not limited thereto.
[0322]
Example 1
(Preparation of stretched cellulose ester film)
(Preparation of dope)
<< Preparation of Dope A >>
100 parts by mass of cellulose triacetate (degree of acetyl group substitution: 2.9)
Triphenyl phosphate 10 parts by mass
Biphenyl diphenyl phosphate 2 parts by mass
Exemplified compound 1 (1,3,5-triazine compound) 1 part by mass
Tinuvin 326 0.5 parts by mass
Aerosil R972V (silicon dioxide fine particles) 0.15 parts by mass
Methylene chloride 405 parts by mass
45 parts by mass of ethanol
The above was charged into a closed dissolving pot, completely dissolved at 60 ° C. while stirring, cooled, and then cooled by Azumi Filter Paper No. 244 was used to obtain dope A.
<< Preparation of dope B >>
100 parts by mass of cellulose triacetate (degree of acetyl group substitution: 2.9)
Triphenyl phosphate 10 parts by mass
Biphenyl diphenyl phosphate 2 parts by mass
Tinuvin 326 0.5 parts by mass
Aerosil R972V (silicon dioxide fine particles) 0.15 parts by mass
Methylene chloride 405 parts by mass
45 parts by mass of ethanol
The above was charged into a closed dissolving pot, completely dissolved at 60 ° C. while stirring, cooled, and then cooled by Azumi Filter Paper No. 244 was used to obtain dope B.
[0323]
[Production of cellulose ester films 1 to 7 and H1 to 3]
A prepared above was cast on a stainless steel belt. The solvent was evaporated on the stainless belt, and the web was peeled off from the stainless belt. The exfoliated web is introduced into a tenter dryer, gripped at both ends with clips, dried at 70 ° C. while stretching 1.05 times in the width direction, and placed in a roll dryer having respective drying zones at 110 ° C. and then 125 ° C. The drying was completed while being conveyed through a large number of rolls, and a cellulose ester film having a thickness of 40 μm was produced. A knurling process having a width of 10 mm and a height of 5 μm was performed on both ends of the film to obtain a cellulose ester film A having a width of 1350 mm and a winding length of 4000 m.
[0324]
A cellulose ester film B was produced in the same manner except that dope A was changed to dope B.
[0325]
Using the obtained cellulose ester films A and B, the hard coat layers 1A, 1B, 2, and 3 shown in the table are continuously formed without winding up to a predetermined film thickness as described below, and further formed thereon. The metal compound layer was continuously laminated by the atmospheric pressure plasma treatment described later.
[0326]
<Coating of hard coat layers 1A and 1B>
The following hard coat layer coating composition was extrusion-coated with a die on the surface of the cellulose ester film B prepared above, and then dried in a drying unit set at 80 ° C., and then 100 mJ / cm.2And a hard coat layer 1A containing a plasticizer was provided so as to have a predetermined dry film thickness. After the ultraviolet irradiation, a hard coat layer 1B was further provided thereon so as to have a predetermined dry film thickness.
(Hard coat layer 1A coating composition)
Dipentaerythritol hexaacrylate monomer 60 parts by mass
Dipentaerythritol hexaacrylate dimer 20 parts by mass
Dipentaerythritol hexaacrylate trimer or higher component 20 parts by mass
Dimethoxybenzophenone photoreaction initiator 4 parts by mass
1 part by mass of triphenyl phosphate
Ethyl acetate 50 parts by mass
Methyl ethyl ketone 50 parts by mass
50 parts by mass of isopropyl alcohol
The above coating composition was appropriately diluted with the above solvent to form a clear hard coat layer 1A having a different dry film thickness.
(Hard coat layer 1B coating composition)
Dipentaerythritol hexaacrylate monomer 60 parts by mass
Dipentaerythritol hexaacrylate dimer 20 parts by mass
Dipentaerythritol hexaacrylate trimer or higher component 20 parts by mass
Dimethoxybenzophenone photoreaction initiator 4 parts by mass
Ethyl acetate 50 parts by mass
Methyl ethyl ketone 50 parts by mass
50 parts by mass of isopropyl alcohol
The coating composition was diluted with the solvent to form a clear hard coat layer 1B having a different dry thickness.
[0327]
<Coating of hard coat layer 3>
The following coating composition of the hard coat layer 3 was extrusion-coated with a die on the side of the cellulose ester film B prepared above, and then dried in a drying unit set at 80 ° C., and then 120 mJ / cm.2And a hard coat layer 3 containing a plasticizer having a predetermined thickness was provided.
[0328]
<< Hard coat layer 3 coating composition >>
Ethyl acetate 50 parts by mass
Methyl ethyl ketone 50 parts by mass
50 parts by mass of isopropyl alcohol
Aerosil R972V (average particle size 16 nm) 2 parts by mass
The above was stirred with a high-speed stirrer (TK homomixer, manufactured by Tokushu Kika Kogyo Co., Ltd.) and then dispersed by a collision type disperser (Manton Gorin, manufactured by Gorin Co., Ltd.), and then the following components were added.
[0329]
Dipentaerythritol hexaacrylate monomer 30 parts by mass
Dipentaerythritol hexaacrylate dimer 10 parts by mass
Dipentaerythritol hexaacrylate trimer or higher component 10 parts by mass
2 parts by weight of dimethoxybenzophenone photoinitiator
3 parts by mass of triphenyl phosphate
<Coating of hard coat layer 2>
The following coating composition of the hard coat layer 2 was extrusion-coated on the hard coat layer 1A or the hard coat layer 3 on the side of the cellulose ester film B prepared above, and then dried in a drying section set at 80 ° C. , 120mJ / cm2To provide a hard coat layer 2 (center line average roughness (Ra) 0.2 μm) of a predetermined thickness.
[0330]
<< Hard coat layer 2 coating composition >>
Ethyl acetate 50 parts by mass
Methyl ethyl ketone 50 parts by mass
50 parts by mass of isopropyl alcohol
Sylysia 431 (average particle size 2.5 μm, manufactured by Fuji Silysia Chemical Ltd.)
2.5 parts by mass
Aerosil R972V (average particle size 16 nm) 3 parts by mass
The above was stirred with a high-speed stirrer (TK homomixer, manufactured by Tokushu Kika Kogyo Co., Ltd.) and then dispersed by a collision type disperser (Manton Gorin, manufactured by Gorin Co., Ltd.), and then the following components were added.
[0331]
Dipentaerythritol hexaacrylate monomer 60 parts by mass
Dipentaerythritol hexaacrylate dimer 20 parts by mass
Dipentaerythritol hexaacrylate trimer or higher component 20 parts by mass
Dimethoxybenzophenone photoreaction initiator 4 parts by mass
Then, a metal compound layer (anti-reflection layer) was formed by plasma discharge treatment using a reaction gas at or near atmospheric pressure.
[0332]
《Formation of anti-reflection layer》
Antireflection layers were formed on the hard coat layers (ultraviolet curable resin layers) provided on the cellulose ester films 1 to 12, respectively, by atmospheric pressure plasma discharge treatment using the following plasma discharge treatment apparatus.
[0333]
《Plasma discharge treatment device》
(Preparation of electrode)
In the plasma discharge processing apparatus shown in FIG. 10, a roll electrode covered with a dielectric and a set of a plurality of rectangular cylindrical electrodes similarly covered with a dielectric were produced as follows.
[0334]
The roll electrode serving as the first electrode was coated with a sprayed alumina film on a titanium alloy T64 jacket roll metal base material having cooling means with cooling water, and a solution obtained by diluting tetramethoxysilane with ethyl acetate was applied and dried. Thereafter, the film was cured by irradiation with ultraviolet rays to perform a sealing treatment. The dielectric surface coated in this manner was polished, smoothed, and processed to have an Rmax of 5 μm. The final film thickness of the dielectric was 1 mm, and the dielectric constant of the dielectric was 10. Further, the difference between the linear thermal expansion coefficient of the conductive metal base material and that of the dielectric material is 1.7 × 10-4The heat resistant temperature was 260 ° C.
[0335]
On the other hand, the rectangular cylindrical electrode of the second electrode was formed by coating a hollow rectangular cylindrical titanium alloy T64 with the same dielectric material as described above under the same conditions, thereby forming a group of opposed rectangular cylindrical fixed electrodes. The dielectric material of this rectangular cylindrical electrode is the same as that of the above-mentioned roll electrode.
[0336]
Twenty-five such prismatic electrodes were arranged around the roll rotating electrode with a gap of 1 mm between the counter electrodes. The total discharge area of the rectangular cylindrical fixed electrode group is 150 cm (length in the width direction) × 4 cm (length in the transport direction) × 25 (number of electrodes) = 15000 cm2Met.
[0337]
The introduction of the reaction gas and the exhaustion of the used gas were performed alternately between the counter electrodes.
The plasma discharge treatment apparatus is supplied with a continuous frequency of 13.56 MHz and a high frequency voltage of 0.8 kV / mm (high frequency power source manufactured by Pearl Industries) on the fixed electrode side, and a continuous frequency of 100 kHz and 8 kV / on the roll electrode side. mm high-frequency voltage (high-frequency power supply manufactured by Heiden Laboratory) was supplied. The roll electrode was rotated using a drive in synchronization with the transport of the cellulose ester film. The plasma discharge treatment apparatus was prepared for each metal oxide layer, and was operated continuously while controlling the thickness of the layer formed for each layer.
[0338]
The gap between the fixed electrode and the roll electrode was set to 1 mm, and the pressure of the reaction gas was set to atmospheric pressure + 1 kPa. The composition of the reaction gas (reaction gas for forming a silicon oxide layer) used in the plasma discharge treatment is described below. The liquid component in the reaction gas was vaporized by a vaporizer and supplied to the discharge section while heating.
[0339]
Plasma treatment was performed on the cellulose ester film having a hard coat layer prepared in Example 1 using the following reaction gas by the plasma discharge treatment apparatus shown in FIG. 10 to form an antireflection layer on the hard coat layer side. Thus, optical films 1 to 12 were produced.
<< Layer configuration of antireflection layer, layer thickness, type of reaction gas >>
Figure 2004203009
On the hard coat layer, an antireflection layer including a first titanium oxide layer, a first silicon oxide layer, a second titanium oxide layer, and a second silicon oxide layer was formed, and further provided in the order of an antifouling layer.
[0340]
《Type of reaction gas》
The reaction gas used for forming the antireflection layer is shown below.
[0341]
(Reactive gas A): For forming a titanium oxide layer (high refractive index layer)
98.7% by volume of nitrogen
Hydrogen 1% by volume
Titanium isopropoxy titanium vapor 0.3% by volume
(Reactive gas B): For forming a silicon oxide layer (low refractive index layer 1)
98.7% by volume of nitrogen
Hydrogen 1% by volume
0.3% by volume of tetraethoxysilane vapor
(Reactive gas C): For forming a silicon oxide layer (low refractive index layer 2)
98.7% by volume of nitrogen
Reaction gas (hydrogen gas) 1% by volume
Reactant gas (methyltriethoxysilane vapor) 0.3% by volume
In addition, when the two hard coat layers were provided, they were coated in the same manner as the optical film 10 of Table 1 except that the lower hard coat layer was applied and then wound once, and then the upper hard coat layer was formed again. Film 13 was produced. An optical film 14 was produced in the same manner as the optical film 11 except that the lower hard coat layer was applied and then wound once, and then the upper hard coat layer was formed again. The optical films 10 and 11 in which the hard coat layer was continuously formed had reduced reflected light unevenness as compared with the optical films 13 and 14. The comparative optical films 1 and 12 were inferior in streak failure, cracks, adhesion, and uneven color (ΔE) of reflected light.
[0342]
As described above, the results of Example 1 are shown in Tables 1, 2, 3, and 4.
[0343]
[Table 1]
Figure 2004203009
[0344]
[Table 2]
Figure 2004203009
[0345]
[Table 3]
Figure 2004203009
[0346]
[Table 4]
Figure 2004203009
[0347]
Example 2
(Preparation of polarizing plate)
The optical films 10, 11, 13 and 14 were immersed in the A side for 90 seconds in a 2 mol / L NaOH aqueous solution at 60 ° C., then washed with normal temperature water, dried at 80 ° C., and saponified on one side. A film was obtained.
[0348]
The cellulose ester film used as the base film of the optical film was similarly subjected to a one-sided saponification treatment.
[0349]
Separately, a polyvinyl alcohol having a thickness of 120 μm was immersed in 100 parts by mass of an aqueous solution containing 1 part by mass of iodine and 4 parts by mass of boric acid, and a polarizing film stretched four times in the longitudinal direction at 50 ° C. was prepared. One side of the polarizing film is bonded to the saponified surface of the saponified optical film with a 5% by mass aqueous solution of completely saponified polyvinyl alcohol, and the other side is bonded to a saponified cellulose ester film. And a polarizing plate. The storage stability of these polarizing plates was evaluated. The polarizing plates using the optical films 10 and 11 showed better results than the polarizing plates using the optical films 13 and 14.
[0350]
Example 3
(Liquid crystal image display device)
The polarizing plate on the outermost surface of a commercially available liquid crystal display panel (NEC color liquid crystal display MultiSync LCD1525J, model name LA-1529HM) was carefully peeled off. Here, the polarizing plate sample prepared in Example 2 was attached to a liquid crystal display panel with the polarization direction adjusted. The visibility of each liquid crystal display panel was evaluated visually using the polarizing plate sample that had been forcibly deteriorated, and those using the optical films 10 and 11 were better than those using the optical films 13 and 14. Results were shown.
[0351]
In addition, the said evaluation was performed as follows.
《Evaluation》
L of the manufactured low reflection laminate*a*b*The values, ΔE (color difference, uneven reflected light), and reflectivity were measured by the following methods.
[0352]
(L*a*b*Value measurement)
L of low reflection laminate*a*b*The value was obtained from the spectral reflectance measured by SCI (including regular reflection light) using a color chromaticity meter CM-2022 (manufactured by Minolta Co., Ltd.). The sample was subjected to light absorption treatment (transmittance from 370 nm to 730 nm is less than 10%) with a black spray after roughening the back surface on the measurement side, and measurement was performed on a black table.
[0353]
(ΔE1 and average L*a*b*Value measurement)
From the prepared sample, 100 points of L in a range of 10 cm × 10 cm at 1 cm intervals*a*b*The value was measured, and the maximum value ΔE1 of ΔE between two points adjacent at an interval of 1 cm was obtained. In addition, the measured L*a*b*From each 100 point average, average L*a*b*The value was determined.
[0354]
(Reflectance)
L*a*b*The average value was determined from the spectral reflectance in the range of 450 nm to 650 nm measured by the SCI (including regular reflection light) method using a color chromaticity meter CM-2022 (manufactured by Minolta) for the measurement of the value. .
[0355]
(A*Value and b*Value relationship)
To obtain ΔE1, the measured L of 100 points*a*b*The value a*And b*Was in the range of the following (Equation 1).
[0356]
Equation 1b*= −1.5 × a*± 5
(Evaluation of color unevenness)
L*a*b*The sample prepared for measuring the value was visually evaluated. The evaluation criteria are as follows and are evaluated in five stages, with A being the best.
[0357]
A: almost no change in color tone of reflected light
B: slight change in color tone of reflected light
C: Color tone change of reflected light is partially observed
D: Color tone change of reflected light is recognized as a whole
E A large change in the color tone of the reflected light is observed overall
Streak failure
The samples formed continuously for a long time were visually evaluated for the presence or absence of streak-like unevenness.
◎ No streak-like unevenness can be confirmed.
○ Slightly streak-like failure is observed.
△ Weak streak-like failure is observed.
X: A streak failure is clearly observed.
[0358]
For cracks, steel wool and overall evaluation,
◎ Sufficiently stable
○ Practically stable
△ Somewhat unstable
× Not practical
And
[0359]
【The invention's effect】
On one side of the substrate sheet, each film has at least two active ray-curable resin layers having a thickness of 0.5 μm or more, at least the lower active ray-curable resin layer contains a plasticizer, and the upper layer The optical film of the present invention having a metal compound layer formed by a plasma treatment under a gas atmosphere near the atmospheric pressure mainly containing nitrogen directly or through another layer on the actinic radiation curable resin layer, It exhibited stable and excellent durability even when subjected to cycle treatment or long-term treatment under wet conditions, and exhibited low reflectance and reduced color unevenness. In addition, it has become possible to provide a polarizing plate and an image display device that are stable even under high temperature and high humidity conditions using the optical film.
[Brief description of the drawings]
FIG. 1 schematically shows a cross section of a substrate sheet having a three-layer structure.
FIG. 2 is a view showing a co-casting die and a state where a multilayer structure web is formed by casting (the web is also called a doped film immediately after casting).
FIG. 3 is a diagram illustrating a sequential casting die and a web having a multilayer structure that is cast.
FIG. 4 is a diagram showing a cross section of another type of co-casting die.
FIG. 5 is a view showing a dope preparation step of the solution casting film forming apparatus.
FIG. 6 is a view schematically showing a process from a casting step to a drying step of the solution casting film forming apparatus.
FIG. 7 schematically illustrates a cross section of an optical film in which two hard coat layers are arranged on a base sheet having a two-layer structure and a single-layer structure.
FIG. 8 is a schematic diagram of a coating apparatus for coating two hard coat layers on a base sheet.
FIG. 9 is a schematic view showing an example of a jet type atmospheric pressure plasma discharge processing apparatus useful for the present invention.
FIG. 10 is a schematic view showing an example of an atmospheric pressure plasma discharge treatment apparatus of a type for treating a substrate between opposed electrodes useful in the present invention.
FIG. 11 is a perspective view showing an example of the structure of a conductive metal base material of the roll rotating electrode shown in FIG. 10 and a dielectric material coated thereon.
FIG. 12 is a perspective view showing an example of the structure of a conductive metal base material of a rectangular cylindrical electrode and a dielectric material coated thereon.
[Explanation of symbols]
10 Co-casting die
11 base part
13, 15 Slit for surface layer
14 Slit for base layer
16 Metal support
17, 19 Dope for surface layer
18 Dope for base layer
20 Multi-layered web
21,23 surface layer
22 Base layer
100 Cellulose ester solution
101 melting pot
102, 105, 112, 115 Liquid sending pump
103 Filter
104, 114 Stock tank
106, 113, 116 Filter
108, 117 conduit
110 In-line additive liquid
120 Confluence pipe
121 mixing machine
200 Co-casting die
201, 202, 203 inlet
204 metal support
205 Peeling position
206 Web
207 tenter device
208 Roll dryer
210 Cellulose ester film
311 First electrode
312 2nd electrode
325,326 High frequency probe
330 Plasma Discharge Treatment System
401,402 Extrusion type coating device
403,404 UV irradiation device
F Base sheet

Claims (7)

プラスチックの基材シートの少なくとも片方の面に、各々の膜厚が0.5μm以上の少なくとも2層の活性線硬化樹脂層を有し、少なくとも下層の活性線硬化樹脂層は可塑剤を含有し、上層の活性線硬化樹脂層の上に直接又は他の層を介して主に窒素を含有する大気圧近傍のガス雰囲気下でプラズマ処理によって形成された金属化合物層を有することを特徴とする光学フィルム。At least one surface of the plastic substrate sheet has at least two active ray-curable resin layers each having a thickness of 0.5 μm or more, and at least the lower active ray-curable resin layer contains a plasticizer, An optical film having a metal compound layer formed by a plasma treatment under a gas atmosphere near the atmospheric pressure containing nitrogen mainly directly or via another layer on the upper active ray curable resin layer. . 前記光学フィルムが分子内に3個以上の芳香族環を有する化合物を含有することを特徴とする請求項1に記載の光学フィルム。The optical film according to claim 1, wherein the optical film contains a compound having three or more aromatic rings in a molecule. プラスチックの基材シートの少なくとも片方の面に、各々の膜厚が0.5μm以上の少なくとも2層のハードコート層の性能を有する活性線硬化樹脂層を形成させ、更にその上に直接又は他の層を介して主に窒素を含有する大気圧近傍のガス雰囲気下でプラズマ処理によって金属化合物層を形成させることを特徴とする光学フィルムの製造方法。On at least one surface of the plastic substrate sheet, an active ray-curable resin layer having the performance of at least two hard coat layers each having a thickness of 0.5 μm or more is formed, and further directly or other A method for producing an optical film, wherein a metal compound layer is formed by plasma treatment in a gas atmosphere near the atmospheric pressure containing mainly nitrogen through a layer. 前記プラズマ処理が対向する少なくとも2つの電極との間に窒素を主成分とするガスを供給し、該第1電極と該第2電極との間に高周波電圧を印加することにより前記ガスを励起し、活性線硬化樹脂層が施された前記基材シートを励起された該ガスに晒すことにより該基材シートに施した活性線硬化樹脂層上に金属化合物層を形成させるものであり、該高周波電圧が、第1の周波数ωの電圧成分と、該第1の周波数ωより高い第2の周波数ωの電圧成分とを有することを特徴とする請求項3に記載の光学フィルムの製造方法。The plasma treatment supplies a gas containing nitrogen as a main component between at least two electrodes facing each other, and excites the gas by applying a high-frequency voltage between the first electrode and the second electrode. Exposing the base sheet provided with the actinic ray-curable resin layer to the excited gas to form a metal compound layer on the actinic ray-curable resin layer applied to the base sheet; voltage, the manufacture of the optical film according to claim 3, characterized in that it comprises a first frequency omega 1 of the voltage component, and higher than the frequency omega 1 of the first second frequency omega 2 of the voltage component Method. 前記ハードコート層として可塑剤を含有する活性線硬化樹脂層を形成した後、巻き取ることなく2層目の活性線硬化樹脂層を設け、更にその上に直接又は他の層を介して主に窒素を含有する大気圧近傍のガス雰囲気下でプラズマ処理によって2層以上の金属化合物層を連続的に形成させることを特徴とする請求項3又は4に記載の光学フィルムの製造方法。After forming an actinic ray-curable resin layer containing a plasticizer as the hard coat layer, a second actinic ray-curable resin layer is provided without winding, and further mainly directly or via another layer thereover. The method for producing an optical film according to claim 3, wherein two or more metal compound layers are continuously formed by a plasma treatment in a gas atmosphere near the atmospheric pressure containing nitrogen. 請求項1又は2に記載の光学フィルムを有することを特徴とする偏光板。A polarizing plate comprising the optical film according to claim 1. 請求項1又は2に記載の光学フィルムを有することを特徴とする表示装置。A display device comprising the optical film according to claim 1.
JP2003010483A 2002-10-31 2003-01-20 Manufacturing method of optical film Expired - Fee Related JP4196686B2 (en)