JP2003154605A - Laminated sheet, laminate and laminate manufacturing method - Google Patents
Laminated sheet, laminate and laminate manufacturing methodInfo
- Publication number
- JP2003154605A JP2003154605A JP2002256825A JP2002256825A JP2003154605A JP 2003154605 A JP2003154605 A JP 2003154605A JP 2002256825 A JP2002256825 A JP 2002256825A JP 2002256825 A JP2002256825 A JP 2002256825A JP 2003154605 A JP2003154605 A JP 2003154605A
- Authority
- JP
- Japan
- Prior art keywords
- laminated sheet
- layer
- laminated
- adhesive
- adhesive layer
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【0001】[0001]
【発明の属する技術分野】この発明は、表面に天然木を
主体とする木質層を備えた積層シート、この積層シート
の裏面側に熱可塑性樹脂組成物製成形体を積層一体化し
た積層体、この積層体の製造方法に関するものである。BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a laminated sheet having on its surface a wood layer mainly composed of natural wood, and a laminated body in which a molded product made of a thermoplastic resin composition is laminated and integrated on the back side of the laminated sheet, The present invention relates to a method for manufacturing the laminated body.
【0002】[0002]
【従来の技術】近年、特に自動車分野において自動車内
装部品であるセンタークラスターやコンソールアッパー
やオーナメントドアトリム等では、優れた意匠性を有す
る天然木からなる積層シートを意匠面に施した部品(積
層体)が多くなっている。2. Description of the Related Art In recent years, particularly in the automobile field, center clusters, console uppers, ornament door trims, etc., which are interior parts of automobiles, have a design surface provided with a laminated sheet made of natural wood having excellent design properties (laminate). Is increasing.
【0003】例えば、下記のようにして積層体を製造し
ている(例えば特許文献1や特許文献2などを参照)。
ウォールナットやメープル等の意匠性に優れた天然木を
0.1〜0.2mmにスライスしたものに対し、補強を
目的とした不織布シートやアルミ薄板等を貼り合わせ
て、単板とする。さらに、熱可塑性樹脂組成物との積層
一体化工程における密着力確保を目的として、この単板
に対し天然木のマンガシロノ材等を裏打ちして積層シー
トを準備する。この積層シートを所望の形状にカット
し、金型キャビティ内面にこの積層シートを沿わせてセ
ットする。そして、金型キャビティ内に溶融状態の熱可
塑性樹脂組成物を射出注入し、この積層シートを有する
積層体を得る。For example, a laminated body is manufactured as follows (see, for example, Patent Document 1 and Patent Document 2).
A natural wood such as walnut or maple, which is excellent in design, is sliced into 0.1 to 0.2 mm, and a non-woven sheet or aluminum thin plate for reinforcement is attached to the sliced veneer. Further, a laminated sheet is prepared by lining this veneer with a mangashirono material of natural wood and the like for the purpose of ensuring adhesion in the step of laminating and integrating with the thermoplastic resin composition. This laminated sheet is cut into a desired shape, and the laminated sheet is set along the inner surface of the mold cavity. Then, the molten thermoplastic resin composition is injected and injected into the mold cavity to obtain a laminate having this laminated sheet.
【0004】上記積層体のままでも意匠性に優れている
が、自動車内装部品の場合には、さらなる意匠性の向上
と、耐候性や耐湿性や耐傷付き性の向上のために、着色
塗装やポリエステル樹脂等のクリア塗装を行っている。The above laminated body is excellent in designability as it is, but in the case of automobile interior parts, in order to further improve the designability and weather resistance, moisture resistance and scratch resistance, a colored coating or Clear coating such as polyester resin is applied.
【0005】そのほか、特許文献3では、下記のように
して積層体を製造している。ウォールナットやメープル
等の意匠性に優れた天然木を0.1〜0.2mmにスラ
イスしたものに対し、熱可塑性樹脂組成物を含浸する
か、アルカリ処理を施し、これに裏打ち材を補強目的で
貼り合わせて、積層シートを準備する。さらに、この積
層シートを金型キャビティ内面に沿わせてセットし、こ
の金型キャビティ内に溶融状態の熱可塑性樹脂組成物を
射出注入して、この積層シートを有する積層体を得る。In addition, in Patent Document 3, a laminated body is manufactured as follows. For natural wood such as walnut or maple, sliced into 0.1 to 0.2 mm slices of natural wood, either impregnated with a thermoplastic resin composition or treated with an alkali, and reinforced with a lining material A laminated sheet is prepared by laminating them. Further, the laminated sheet is set along the inner surface of the mold cavity, and the molten thermoplastic resin composition is injected and injected into the mold cavity to obtain a laminated body having the laminated sheet.
【0006】[0006]
【特許文献1】特公平5ー58890号公報[Patent Document 1] Japanese Patent Publication No. 5-58890
【特許文献2】特開平1ー64817号公報[Patent Document 2] Japanese Patent Laid-Open No. 1-64817
【特許文献3】特公平7ー55515号公報[Patent Document 3] Japanese Patent Publication No. 7-55515
【0007】[0007]
【発明が解決しようとする課題】しかし、センタークラ
スターやコンソールアッパーやオーナメントドアトリム
等の自動車内装部品の意匠面形状はますます三次元化し
てきているので、マンガシロノ材等の天然木を裏打ちし
たために剛性のある積層シートを金型キャビティ内面に
沿わせてセットすることが困難になる場合がある。ま
た、積層体の製造工程において積層シートに対し熱可塑
性樹脂組成物を積層して一体化する場合に木質層に割れ
が発生することもある。[Problems to be Solved by the Invention] However, the design surface shapes of automobile interior parts such as center clusters, console uppers, and ornament door trims are becoming three-dimensional more and more. In some cases, it may be difficult to set a laminated sheet having the above-mentioned shape along the inner surface of the mold cavity. In addition, when the thermoplastic resin composition is laminated and integrated on the laminated sheet in the manufacturing process of the laminated body, cracks may occur in the wood layer.
【0008】その割れを防止する方法として、積層シー
トを予め熱プレス等により予備賦形する方法が知られて
いる。しかし、この方法では予備賦形段階で割れが発生
するために効果のある対策ではない。あるいは、特許文
献3のように木質シートに熱可塑性樹脂組成物を含浸さ
せたりアルカリ処理を施す方法が知られている。しか
し、この方法では熱可塑性樹脂組成物の含浸やアルカリ
処理に時間を要するとともに、それらが煩雑な工程であ
るにもかかわらず得られる効果は少ない。As a method of preventing the cracks, a method of preliminarily shaping the laminated sheet by hot pressing or the like is known. However, this method is not an effective measure because it causes cracks in the pre-forming step. Alternatively, as in Patent Document 3, a method of impregnating a wood sheet with a thermoplastic resin composition or performing an alkali treatment is known. However, this method requires a long time for impregnation of the thermoplastic resin composition and alkali treatment, and there is little effect obtained even though they are complicated steps.
【0009】ところで、積層体を得るための積層一体化
工程においては、マンガシロノ材等の天然木からなる裏
打ち材を有する積層シートと、熱可塑性樹脂組成物との
接着は、アンカー効果(凹凸による密着効果)によるも
のである。この場合、裏打ち材と熱可塑性樹脂組成物と
の間で一定の密着強度を得るためには、溶融させた熱可
塑性樹脂組成物を高圧で裏打ち材に押し付けなければな
らない。そのため、必然的に積層一体化時の成形条件幅
が狭くなる問題があった。By the way, in the step of laminating and integrating to obtain a laminated body, the adhesion between the laminated sheet having a backing material made of natural wood such as mangashirono wood and the thermoplastic resin composition is anchor effect (adhesion due to unevenness). Effect). In this case, in order to obtain a constant adhesion strength between the backing material and the thermoplastic resin composition, the molten thermoplastic resin composition must be pressed against the backing material at high pressure. Therefore, there is a problem inevitably that the range of molding conditions at the time of stacking and integration becomes narrow.
【0010】一方、特許文献3に示すプライマー処理を
施して密着性を向上させる方法の場合、このプライマー
処理工程が付加されて工程が増えるにもかかわらず、劇
的な効果は得られなかった。On the other hand, in the case of the method of applying the primer treatment shown in Patent Document 3 to improve the adhesion, the dramatic effect was not obtained although the primer treatment step was added and the number of steps was increased.
【0011】さらに、天然木からなる裏打ち材を有する
積層シートの場合、熱可塑性樹脂組成物と積層一体化し
て得られた積層体において積層シートの木口近傍で熱可
塑性樹脂組成物表面に裏打ち材の小片が散在する場合が
あった。この現象は、積層一体化時に熱可塑性樹脂組成
物の圧力に負けて剥離した裏打ち材の小片が熱可塑性樹
脂組成物の表面に現れたものである。この散在小片は、
外観上の不具合となるために除去しなければならず、そ
の除去工程が増えて製造コストが高くなる問題があっ
た。Further, in the case of a laminated sheet having a backing material made of natural wood, in a laminate obtained by laminating and integrating with a thermoplastic resin composition, the backing material is provided on the surface of the thermoplastic resin composition near the mouth of the laminated sheet. Sometimes small pieces were scattered. This phenomenon is due to the fact that a small piece of the backing material, which was peeled off due to the pressure of the thermoplastic resin composition during the integration of the layers, appeared on the surface of the thermoplastic resin composition. These scattered pieces are
Since it becomes a defect in appearance, it has to be removed, and there is a problem that the number of removing steps increases and the manufacturing cost increases.
【0012】本発明は、天然木積層シートの裏打ち材で
あるマンガシロノ材等の木質シートを利用しない積層構
造を採用して、前述した問題点を解消し、広い成形条件
幅と良好な製品外観と良好な予備賦形性とを持たせるこ
とを目的にしている。The present invention adopts a laminated structure which does not use a wood sheet such as mangashirono material which is a lining material of a natural wood laminated sheet, solves the above-mentioned problems, has a wide molding condition width and a good product appearance. The purpose is to have good preformability.
【0013】[0013]
【課題を解決するための手段】後記実施形態の図面(図
1〜6)の符号を援用して本発明を説明する。
* 請求項1〜10の発明は、積層シート(1)に関す
るものである。The present invention will be described with reference to the reference numerals in the drawings (FIGS. 1 to 6) of the embodiment described later. * The inventions of claims 1 to 10 relate to the laminated sheet (1).
【0014】請求項1の発明にかかる積層シート(1)
においては、天然木を主体として所定の厚みにスライス
した木質層(2)と、熱可塑性樹脂組成物に対し接着性
を持つ接着剤を有する接着層(3)とを備え、この木質
層(2)とこの接着層(3)とを互いに積層して一体化
し、この木質層(2)を表面側に露出させるとともに、
この接着層(3)を裏面側に露出させている。Laminated sheet (1) according to the invention of claim 1
In the above, a wood layer (2) mainly composed of natural wood and sliced to a predetermined thickness and an adhesive layer (3) having an adhesive having adhesiveness to a thermoplastic resin composition are provided, and the wood layer (2 ) And this adhesive layer (3) are laminated and integrated with each other to expose the wood layer (2) to the surface side,
The adhesive layer (3) is exposed on the back surface side.
【0015】請求項2の発明においては、請求項1の発
明にかかる木質層(2)と接着層(3)とを互いに直接
的に接触させて二層構造とした。請求項3の発明におい
ては、請求項1の発明にかかる木質層(2)と接着層
(3)との間に、柔軟性を有する補強層(4)を介在さ
せてこの木質層(2)とこの補強層(4)とを互いに直
接的に接触させるとともにこの補強層(4)とこの接着
層(3)とを互いに直接的に接触させ、この木質層
(2)とこの補強層(4)とこの接着層(3)とを互い
に積層して一体化した三層構造とした。In the second aspect of the invention, the wood layer (2) and the adhesive layer (3) according to the first aspect of the invention are in direct contact with each other to form a two-layer structure. In the invention of claim 3, the reinforcing layer (4) having flexibility is interposed between the wood layer (2) and the adhesive layer (3) according to the invention of claim 1, and the wood layer (2) is provided. And the reinforcing layer (4) are in direct contact with each other, and the reinforcing layer (4) and the adhesive layer (3) are in direct contact with each other, and the wood layer (2) and the reinforcing layer (4) are in contact with each other. ) And this adhesive layer (3) are laminated together to form a three-layer structure.
【0016】請求項4の発明においては、請求項3の発
明にかかる補強層(4)の厚みを0.1〜0.4mmに
した。請求項5の発明においては、請求項3または請求
項4の発明にかかる補強層(4)を不織布により構成し
た。In the invention of claim 4, the reinforcing layer (4) according to the invention of claim 3 has a thickness of 0.1 to 0.4 mm. In the invention of claim 5, the reinforcing layer (4) according to the invention of claim 3 or 4 is made of a nonwoven fabric.
【0017】請求項6の発明においては、請求項1から
請求項5のうちいずれかの請求項の発明にかかる木質層
(2)の厚みを0.1〜0.4mmとし、同じく接着層
(3)の厚みを0.05〜0.2mmとした。In the invention of claim 6, the wood layer (2) according to the invention of any one of claims 1 to 5 has a thickness of 0.1 to 0.4 mm, and the same adhesive layer ( The thickness of 3) was 0.05 to 0.2 mm.
【0018】請求項7の発明においては、請求項1から
請求項6のうちいずれかの請求項の発明にかかる接着層
(3)を、不織布と、この不織布内に含浸させた接着剤
とから構成した。In the invention of claim 7, the adhesive layer (3) according to any one of claims 1 to 6 is formed from a nonwoven fabric and an adhesive impregnated in the nonwoven fabric. Configured.
【0019】請求項8の発明においては、請求項1から
請求項7のうちいずれかの請求項の発明にかかる接着層
(3)の接着剤を、熱可塑性樹脂組成物であるABS樹
脂(アクリルニトリルブタジエンスチレン樹脂)に対し
接着性を持つものとした。In the invention of claim 8, the adhesive of the adhesive layer (3) according to the invention of any one of claims 1 to 7 is made of an ABS resin (acrylic) which is a thermoplastic resin composition. Nitrile butadiene styrene resin).
【0020】請求項9の発明においては、請求項1から
請求項8のうちいずれかの請求項の発明にかかる接着層
(3)の接着剤を、ホットメルト接着剤とした。請求項
10の発明においては、請求項9の発明にかかる接着剤
(3)であるホットメルト接着剤を、ポリエステル系の
ものとした。In the invention of claim 9, the adhesive of the adhesive layer (3) according to the invention of any one of claims 1 to 8 is a hot melt adhesive. In the invention of claim 10, the hot melt adhesive which is the adhesive (3) according to the invention of claim 9 is made of polyester.
【0021】* 請求項11〜12の発明は、積層体
(5)に関するものである。請求項11の発明にかかる
積層体(5)は、請求項1から請求項10のうちいずれ
かの請求項の発明に記載の積層シート(1)と、この積
層シート(1)の裏面側にある接着層(3)に対し直接
的に接触させて一体化した熱可塑性樹脂組成物製成形体
(6)とからなる。* The inventions of claims 11 to 12 relate to a laminate (5). The laminated body (5) according to the invention of claim 11 comprises a laminated sheet (1) according to the invention of any one of claims 1 to 10 and a back surface side of the laminated sheet (1). It comprises a molded body (6) made of a thermoplastic resin composition, which is brought into direct contact with and integrated with a certain adhesive layer (3).
【0022】請求項12の発明において、請求項11の
発明にかかる成形体(6)を構成する熱可塑性樹脂組成
物はABS樹脂(アクリルニトリルブタジエンスチレン
樹脂)を含む。In the twelfth aspect of the invention, the thermoplastic resin composition constituting the molded body (6) according to the eleventh aspect of the invention contains an ABS resin (acrylonitrile butadiene styrene resin).
【0023】* 請求項13〜16の発明は積層体
(5)の製造方法に関するものである。請求項13の発
明において積層体(5)は、下記・の工程を経て製造さ
れる。
・ 請求項1から請求項10のうちいずれかの請求項の
発明に記載の積層シート(1)からその一部を切り抜い
て成形用積層シート(1a)とする。* The invention of claims 13 to 16 relates to a method for producing a laminate (5). In the invention of claim 13, the laminate (5) is manufactured through the following steps. -A part of the laminated sheet (1) according to the invention of any one of claims 1 to 10 is cut out to obtain a laminated sheet (1a) for molding.
【0024】・ 図5(a)に示すように、前記成形用
積層シート(1a)の表面側にある木質層(2)を成形
型(8)のキャビティ(8a)の内面に沿うように当て
がってこの成形用積層シート(1a)をこの成形型
(8)に位置決めする。As shown in FIG. 5 (a), the wood layer (2) on the surface side of the forming laminated sheet (1a) is applied along the inner surface of the cavity (8a) of the forming die (8). Then, the molding laminated sheet (1a) is positioned on the molding die (8).
【0025】・ 図5(b)(c)に示すように、前記
キャビティ(8a)で前記成形用積層シート(1a)の
裏面側にある接着層(3)に面する成形空間に対し溶融
状態の熱可塑性樹脂組成物を供給してこの接着層(3)
に対し直接的に接触させ、この熱可塑性樹脂組成物から
なる成形体(6)とこの成形用積層シート(1a)とを
一体化した積層体(5)を製造する。As shown in FIGS. 5 (b) and 5 (c), a molten state is present in the cavity (8a) in the molding space facing the adhesive layer (3) on the back surface side of the molding laminated sheet (1a). This adhesive layer (3) by supplying the thermoplastic resin composition of
Is directly contacted with the above to produce a laminated body (5) in which the molded body (6) made of the thermoplastic resin composition and the molding laminated sheet (1a) are integrated.
【0026】請求項14の発明において積層体(5)
は、下記・の工程を経て製造される。
・ 図3(a)(b)(c)に示すように、請求項1か
ら請求項10のうちいずれかの請求項の発明に記載の積
層シート(1)に対し予備賦形を施した後にこの積層シ
ート(1)からその一部を切り抜いて成形用積層シート
(1a)とするか、または、図4(a)(b)に示すよ
うに、請求項1から請求項10のうちいずれかの請求項
の発明に記載の積層シート(1)からその一部を切り抜
いて成形用積層シート(1a)とした後にこの成形用積
層シート(1a)に対し予備賦形を施す。In the fourteenth aspect of the invention, the laminate (5)
Is manufactured through the following steps. As shown in FIGS. 3 (a), (b) and (c), after preliminarily shaping the laminated sheet (1) according to the invention of any one of claims 1 to 10. A part of this laminated sheet (1) is cut out to form a laminated sheet (1a) for molding, or as shown in FIGS. 4 (a) and 4 (b), one of claims 1 to 10. Part of the laminated sheet (1) according to the invention of claim 1 is cut out to obtain a forming laminated sheet (1a), and then the forming laminated sheet (1a) is preshaped.
【0027】・ 図5(a)に示すように、前記成形用
積層シート(1a)の表面側にある木質層(2)を成形
型(8)のキャビティ(8a)の内面に沿うように当て
がってこの成形用積層シート(1a)をこの成形型
(8)に位置決めする。As shown in FIG. 5 (a), the wood layer (2) on the surface side of the molding laminated sheet (1a) is applied along the inner surface of the cavity (8a) of the molding die (8). Then, the molding laminated sheet (1a) is positioned on the molding die (8).
【0028】・ 図5(b)(c)に示すように、前記
キャビティ(8a)で前記成形用積層シート(1a)の
裏面側にある接着層(3)に面する成形空間に対し溶融
状態の熱可塑性樹脂組成物を供給してこの接着層(3)
に対し直接的に接触させ、この熱可塑性樹脂組成物から
なる成形体(6)とこの成形用積層シート(1a)とを
一体化した積層体(5)を製造する。As shown in FIGS. 5 (b) and 5 (c), a molten state is present in the cavity (8a) in the molding space facing the adhesive layer (3) on the back surface side of the molding laminated sheet (1a). This adhesive layer (3) by supplying the thermoplastic resin composition of
Is directly contacted with the above to produce a laminated body (5) in which the molded body (6) made of the thermoplastic resin composition and the molding laminated sheet (1a) are integrated.
【0029】請求項15の発明において積層体(5)
は、下記・の工程を経て製造される。
・ 図6(a)に示すように、熱可塑性樹脂組成物によ
り成形体(6)を予め成形する。In the invention of claim 15, the laminate (5)
Is manufactured through the following steps. -As shown in Fig. 6 (a), a molded body (6) is molded in advance with a thermoplastic resin composition.
【0030】・ 図6(b)(c)に示すように、請求
項1から請求項10のうちいずれかの請求項の発明に記
載の積層シート(1)の裏面側にある接着層(3)をこ
の成形体(6)に対し直接的に接触させてこの積層シー
ト(1)を熱成形し、この成形体(6)とこの積層シー
ト(1)とを一体化した積層体(5)を製造する。As shown in FIGS. 6B and 6C, the adhesive layer (3) on the back surface side of the laminated sheet (1) according to the invention of any one of claims 1 to 10. ) Is directly contacted with the molded body (6) to thermoform the laminated sheet (1), and the molded body (6) and the laminated sheet (1) are integrated into a laminated body (5). To manufacture.
【0031】請求項16の発明において、請求項13ま
たは請求項14または請求項15の発明にかかる熱可塑
性樹脂組成物はABS樹脂(アクリルニトリルブタジエ
ンスチレン樹脂)を含む。In the sixteenth aspect of the invention, the thermoplastic resin composition according to the thirteenth, fourteenth or fifteenth aspect of the invention contains an ABS resin (acrylonitrile butadiene styrene resin).
【0032】[0032]
【発明の実施の形態】以下、本発明の一実施形態を図面
を参照して説明する。
<図1(a)に示す積層シート1>この積層シート1の
断面構造としては、図2(a)(b)(c)(d)にそ
れぞれ示す4種類のものがある。図2(a)に示す積層
シート1と、図2(b)に示す積層シート1において
は、いずれも、木質層2と接着層3とが互いに直接的に
接触した二層構造で積層されて一体化され、この木質層
2が表面側に露出しているとともに、この接着層3が裏
面側に露出している。また、図2(c)に示す積層シー
ト1と、図2(d)に示す積層シート1においては、い
ずれも、補強層4が前記木質層2と前記接着層3との間
に介在され、この木質層2とこの補強層4とが互いに直
接的に接触しているとともに、この補強層4とこの接着
層3とが互いに直接的に接触し、この木質層2とこの補
強層4とこの接着層3とが互いに積層されて一体化され
た三層構造になっている。BEST MODE FOR CARRYING OUT THE INVENTION An embodiment of the present invention will be described below with reference to the drawings. <Laminated Sheet 1 Shown in FIG. 1 (a)> The sectional structure of the laminated sheet 1 includes four types shown in FIGS. 2 (a) (b) (c) (d). The laminated sheet 1 shown in FIG. 2A and the laminated sheet 1 shown in FIG. 2B are both laminated in a two-layer structure in which the wood layer 2 and the adhesive layer 3 are in direct contact with each other. The wood layer 2 is integrated and exposed on the front surface side, and the adhesive layer 3 is exposed on the back surface side. In both the laminated sheet 1 shown in FIG. 2C and the laminated sheet 1 shown in FIG. 2D, the reinforcing layer 4 is interposed between the wood layer 2 and the adhesive layer 3, The wooden layer 2 and the reinforcing layer 4 are in direct contact with each other, and the reinforcing layer 4 and the adhesive layer 3 are in direct contact with each other, and the wooden layer 2 and the reinforcing layer 4 are in contact with each other. It has a three-layer structure in which the adhesive layer 3 and the adhesive layer 3 are laminated and integrated.
【0033】* 前記各木質層2について
この各木質層2は天然木を主体とする。この天然木と
は、原生林あるいは植林から伐採した原木である。この
原木の種類としては如何なるものでも良いが、意匠性の
面から好ましくは銘木と呼ばれる種類の樹木が良い。例
えば、唐松、屋久杉、楢、楡、欅、桜、栃、楠、桂、黄
蘖、楓、槐、シカモア、ローズウッド、チーク、マホガ
ニー、アフリカンマホガニー、メランチ、コクタン、シ
タン、アメリカンブラックウォールナット、カリン、ゼ
ブラウッド、ブラジリアンローズ、バーシモン、シルバ
ーローズ、パルマ、シルキーオーク、シルバーハート、
タイワンクス、チェリー、ミルトル、黒レオ、白レオ、
サペリ、ブビンガ、マコレ、マドローナ、メープル、ク
ラロウォールナット、アッシュなどが好ましい。* Regarding each wood layer 2, each wood layer 2 is mainly made of natural wood. The natural tree is a raw tree cut from a primary forest or afforestation. Any kind of raw wood may be used, but from the viewpoint of designability, a kind of tree called a name tree is preferable. For example, Karamatsu, Yakusugi, Nara, 楡, Keyaki, Sakura, Tochi, Kusunoki, Katsura, Yellow 蘖, Kaede, Sophora, Sycamore, Rosewood, Teak, Mahogany, African Mahogany, Merranch, Kotan, Rosewood, American Black Walnut, Karin, Zebrawood, Brazilian Rose, Versimon, Silver Rose, Palma, Silky Oak, Silver Heart,
Thai Wanks, Cherry, Myrtle, Black Leo, White Leo,
Sapele, Bubinga, Macole, Madrona, maple, claro walnut, ash and the like are preferable.
【0034】このような天然木を主体とする木質層2と
は、天然木を所定の厚みにスライスしたもの、あるい
は、そのスライス天然木に熱可塑性樹脂組成物を含浸さ
せたものなどをいう。含浸させる熱可塑性樹脂組成物と
しては如何なるものでも良いが、好ましくは、アクリル
樹脂、ポリ塩化ビニル、酢酸ビニル、エチレンー酢ビ共
重合体及びポリウレタンなどが良い。The wood layer 2 mainly composed of natural wood is a natural wood sliced into a predetermined thickness, or a sliced natural wood impregnated with a thermoplastic resin composition. Any thermoplastic resin composition may be impregnated, but acrylic resin, polyvinyl chloride, vinyl acetate, ethylene-vinyl acetate copolymer, polyurethane and the like are preferable.
【0035】前記木質層2の厚みとしては、0.1〜
0.4mmが良く、好ましくは0.1〜0.3mm、さ
らに好ましくは0.1〜0.2mmが良い。0.1mm
未満では、木質層2が脆くなって積層シート1の取扱性
が悪くなり、また、天然木に対するスライス加工の難易
度が高くなる。一方、0.4mmを越える場合には、積
層シート1の剛性が高くなり過ぎてその柔軟性に欠ける
ため、後述する積層体5の製造工程において積層シート
1に対し熱可塑性樹脂組成物を積層して一体化する場合
に木質層2に割れが発生する。The wood layer 2 has a thickness of 0.1 to
0.4 mm is preferable, 0.1-0.3 mm is preferable, 0.1-0.2 mm is more preferable. 0.1 mm
When it is less than 1, the wood layer 2 becomes brittle, the handleability of the laminated sheet 1 is deteriorated, and the difficulty of slicing the natural wood becomes high. On the other hand, if the thickness exceeds 0.4 mm, the laminated sheet 1 becomes too rigid and lacks in flexibility. Therefore, the thermoplastic resin composition is laminated on the laminated sheet 1 in the manufacturing process of the laminated body 5 described later. When they are integrated with each other, cracks occur in the wood layer 2.
【0036】* 前記接着層3について
図2(a)(c)に示す積層シート1の接着層3は、後
記接着剤のみからなる層3aである。また、図2(b)
(d)に示す積層シート1の接着層3は、この接着剤を
不織布内に含浸させた層3bである。* Regarding the Adhesive Layer 3 The adhesive layer 3 of the laminated sheet 1 shown in FIGS. 2 (a) and 2 (c) is a layer 3a composed only of the adhesive described later. In addition, FIG.
The adhesive layer 3 of the laminated sheet 1 shown in (d) is a layer 3b in which a nonwoven fabric is impregnated with this adhesive.
【0037】前記接着剤としては、後述する積層体5の
製造工程において積層シート1に対し熱可塑性樹脂組成
物を積層して一体化する場合に、その熱可塑性樹脂組成
物に対し接着性を持つものであれば如何なるものでも良
く、適宜選択して使用する。好ましくは、ホットメルト
接着剤、特にABS樹脂(アクリルニトリルブタジエン
スチレン樹脂)に対し接着性を持つホットメルト接着
剤、例えばポリエステル系のホットメルト接着剤が好ま
しい。また、感圧型接着剤でも良い。The above-mentioned adhesive has adhesiveness to the thermoplastic resin composition when the thermoplastic resin composition is laminated on and integrated with the laminated sheet 1 in the manufacturing process of the laminate 5 described later. Any material may be used as long as it is selected appropriately. A hot melt adhesive, particularly a hot melt adhesive having adhesiveness to an ABS resin (acrylonitrile butadiene styrene resin), for example, a polyester-based hot melt adhesive is preferable. Alternatively, a pressure sensitive adhesive may be used.
【0038】前記ホットメルト接着剤としては、エチレ
ン酢酸ビニル共重合体、エチレンエチルアクリレート共
重合体、エチレンアクリル酸、ポリエステル、アタクチ
ックポリプロピレン、プロピレンエチレン共重合体、プ
ロピレンエチレンブテンー1共重合体、ポリカーボネー
ト、ポリビニルエーテル、ポリウレタン、スチレンイソ
プレンスチレン共重合体、スチレンブタジエンスチレン
共重合体、スチレンエチレンブチレンスチレン共重合
体、スチレンエチレンプロピレンスチレン共重合体、ブ
チルゴム、エチレンプロピレンゴム、ポリアミドのう
ち、少なくともいずれか一つのものが含まれているもの
が良い。Examples of the hot melt adhesive include ethylene vinyl acetate copolymer, ethylene ethyl acrylate copolymer, ethylene acrylic acid, polyester, atactic polypropylene, propylene ethylene copolymer, propylene ethylene butene-1 copolymer, At least one of polycarbonate, polyvinyl ether, polyurethane, styrene isoprene styrene copolymer, styrene butadiene styrene copolymer, styrene ethylene butylene styrene copolymer, styrene ethylene propylene styrene copolymer, butyl rubber, ethylene propylene rubber, and polyamide. The one that contains one is good.
【0039】前記感圧型接着剤としては、天然ゴム、ス
チレンブタジエンゴム、シリコーンゴム、ポリイソブチ
レン、ポリビニルエーテル、アクリル酸エステル共重合
体のうち、少なくともいずれか一つのものが含まれてい
るものが良い。As the pressure-sensitive adhesive, one containing at least one of natural rubber, styrene-butadiene rubber, silicone rubber, polyisobutylene, polyvinyl ether, and acrylic acid ester copolymer is preferable. .
【0040】前記不織布としては、レーヨン、ナイロ
ン、ポリエステル、アクリル、ポリエチレン、ビニロ
ン、ポリプロピレン、キュプラなどの各種繊維を原料と
するものが良い。この不織布により、積層シート1とし
ての強度と柔軟性とを向上させることができる。The non-woven fabric is preferably made of various fibers such as rayon, nylon, polyester, acrylic, polyethylene, vinylon, polypropylene and cupra. The nonwoven fabric can improve the strength and flexibility of the laminated sheet 1.
【0041】前記接着層3の厚みとしては、0.05〜
0.2mmが良く、好ましくは0.05〜0.1mmが
良い。0.05mm未満では、所望の密着強度が得られ
ない場合がある。一方、0.2mmを越える場合には、
接着層3での凝集破壊が発生して所望の密着強度が得ら
れない場合がある。The adhesive layer 3 has a thickness of 0.05 to
0.2 mm is preferable, and 0.05 to 0.1 mm is preferable. If it is less than 0.05 mm, the desired adhesion strength may not be obtained. On the other hand, if it exceeds 0.2 mm,
In some cases, cohesive failure occurs in the adhesive layer 3 and desired adhesion strength cannot be obtained.
【0042】* 前記補強層4について
この補強層4としては柔軟性を有する不織布または紙が
良い。不織布としては、レーヨン、ナイロン、ポリエス
テル、アクリル、ポリエチレン、ビニロン、ポリプロピ
レン、キュプラなどの各種繊維を原料とするものが良
い。紙としては、和紙、洋紙クラフト紙、樹脂含浸紙な
どが良い。* Regarding the Reinforcement Layer 4, the reinforcement layer 4 is preferably a non-woven fabric or paper having flexibility. As the non-woven fabric, those made of various fibers such as rayon, nylon, polyester, acrylic, polyethylene, vinylon, polypropylene and cupra are preferable. As the paper, Japanese paper, paper kraft paper, resin-impregnated paper and the like are preferable.
【0043】前記補強層4の厚みとしては、0.1〜
0.4mmが良く、好ましくは0.1〜0.2mmが良
い。0.1mm未満では、所望の強度が得られない。一
方、0.4mmを越える場合には、積層シート1の剛性
が高くなり過ぎてその柔軟性に欠けるため、後述する積
層体5の製造工程において積層シート1に対し熱可塑性
樹脂組成物を積層して一体化する場合に木質層2に割れ
が発生する。The reinforcing layer 4 has a thickness of 0.1 to
0.4 mm is preferable, and 0.1 to 0.2 mm is preferable. If it is less than 0.1 mm, the desired strength cannot be obtained. On the other hand, if the thickness exceeds 0.4 mm, the laminated sheet 1 becomes too rigid and lacks in flexibility. Therefore, the thermoplastic resin composition is laminated on the laminated sheet 1 in the manufacturing process of the laminated body 5 described later. When they are integrated with each other, cracks occur in the wood layer 2.
【0044】<前記積層シート1の積層方法>
* 図2(a)(c)に示す積層シート1においてその
接着層3の積層方法
木質層2または補強層4に対し液状の接着剤を霧状に塗
布してその接着剤を接着層3にするか、木質層2または
補強層4に対し接着剤をローラにより塗布してその接着
剤を接着層3にする。また、ポリエステル系ホットメル
ト接着剤の場合には、木質層2または補強層4に対しこ
のポリエステル系ホットメルト接着剤を押出ラミネーシ
ョンして接着層3にするか、このポリエステル系ホット
メルト接着剤を予めフィルム状に加工した後にこのフィ
ルム状ポリエステル系ホットメルト接着剤を木質層2ま
たは補強層4に対し熱ラミネーションして接着層3にす
る。<Laminating Method of Laminating Sheet 1> * Laminating Method of Adhesive Layer 3 in Laminating Sheet 1 shown in FIGS. 2 (a) and 2 (c) Or the adhesive is applied to the wood layer 2 or the reinforcing layer 4 with a roller to form the adhesive layer 3. In the case of a polyester hot melt adhesive, the polyester hot melt adhesive is extrusion-laminated to the wood layer 2 or the reinforcing layer 4 to form the adhesive layer 3, or the polyester hot melt adhesive is previously prepared. After being processed into a film, the film polyester hot melt adhesive is heat laminated to the wood layer 2 or the reinforcing layer 4 to form the adhesive layer 3.
【0045】* 図2(b)(d)に示す積層シート1
においてその接着層3の積層方法
不織布に対し液状の接着剤を霧状に塗布するか又は接着
剤をローラにより塗布し、この不織布を木質層2または
補強層4に対し熱プレス等により貼着して接着層3にす
る。また、ポリエステル系ホットメルト接着剤の場合に
は、不織布に対しこのポリエステル系ホットメルト接着
剤を押出ラミネーションした後、この不織布を木質層2
または補強層4に対し熱プレス等により貼着して接着層
3にする。あるいは、このポリエステル系ホットメルト
接着剤を予めフィルム状に加工した後、木質層2または
補強層4に対しフィルム状ポリエステル系ホットメルト
接着剤と不織布とを順次重ねてそれらを熱ラミネーショ
ンし、このフィルム状ポリエステル系ホットメルト接着
剤と不織布とで接着層3にする。* Laminated sheet 1 shown in FIGS. 2 (b) and 2 (d)
In the laminating method of the adhesive layer 3, a liquid adhesive is applied to the nonwoven fabric in a mist state or an adhesive is applied by a roller, and the nonwoven fabric is attached to the wood layer 2 or the reinforcing layer 4 by hot pressing or the like. To form the adhesive layer 3. In the case of a polyester-based hot melt adhesive, the polyester-based hot melt adhesive is extrusion-laminated onto a non-woven fabric, and then the non-woven fabric is applied to the wood layer 2
Alternatively, it is attached to the reinforcing layer 4 by heat pressing or the like to form the adhesive layer 3. Alternatively, after the polyester hot melt adhesive is preliminarily processed into a film, the film polyester hot melt adhesive and the non-woven fabric are sequentially laminated on the wood layer 2 or the reinforcing layer 4 to heat-laminate the film. The adhesive layer 3 is made of a polyester hot melt adhesive and a non-woven fabric.
【0046】* 図2(c)(d)に示す積層シート1
においてその補強層4の積層方法
離型紙やポリエチレンフィルム等の離型基材上に水溶性
接着剤を塗布して補強層4を貼着し、この補強層4上に
水溶性接着剤を介して木質層2を重ね、それらを熱プレ
ス等により貼着する。その後、前記離型基材を剥がす。* The laminated sheet 1 shown in FIGS. 2 (c) and 2 (d)
In the method of laminating the reinforcing layer 4, a water-soluble adhesive is applied to a release substrate such as release paper or polyethylene film to adhere the reinforcing layer 4, and the water-soluble adhesive is applied on the reinforcing layer 4. The wood layers 2 are overlaid and they are attached by a heat press or the like. Then, the release substrate is peeled off.
【0047】<図1(b)に示す積層体5>この積層体
5は、後記各種方法により製造され、前述した各種積層
シート1と、その裏面側にある接着層3に対し直接的に
接触して一体化された熱可塑性樹脂組成物製の成形体6
とからなる。<Laminate 5 shown in FIG. 1 (b)> This laminate 5 is manufactured by various methods described below, and directly contacts the above-mentioned various laminated sheets 1 and the adhesive layer 3 on the back side thereof. Molded body 6 made of a thermoplastic resin composition
Consists of.
【0048】この成形体6を構成する熱可塑性樹脂組成
物としては、前述した各種積層シート1の接着層3に対
し接着可能なものであれば如何なるものでも良く、適宜
選択して使用する。As the thermoplastic resin composition constituting this molded body 6, any thermoplastic resin composition may be used so long as it can be bonded to the adhesive layer 3 of the various laminated sheets 1 described above, and it is appropriately selected and used.
【0049】この熱可塑性樹脂組成物としては、アクリ
ルニトリルブタジエンスチレン樹脂、アクリルニトリル
スチレンアクリル酸エステル、ポリアミド、ポリカーボ
ネート、ポリエチレン、ポリエチレンテレフタレート、
ポリブチルテレフタレート、ポリメタクリル酸メチル、
ポリアセタール、ポリプロピレン、ポリスチレン、ポリ
酢酸ビニル、ポリビニルアルコール、ポリ塩化ビニル、
ポリ塩化ビニリデンのうち、少なくともいずれか一つの
ものが含まれているものが良い。好ましくは、アクリル
ニトリルブタジエンスチレン樹脂、アクリルニトリルス
チレンアクリル酸エステル、ポリアミド、ポリカーボネ
ート、ポリエチレン、ポリエチレンテレフタレート、ポ
リブチルテレフタレート、ポリメタクリル酸メチル、ポ
リアセタール、ポリプロピレン、ポリスチレンのうち、
少なくともいずれか一つのものが含まれているものが良
い。Examples of the thermoplastic resin composition include acrylonitrile butadiene styrene resin, acrylonitrile styrene acrylate, polyamide, polycarbonate, polyethylene, polyethylene terephthalate,
Polybutyl terephthalate, polymethyl methacrylate,
Polyacetal, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl chloride,
It is preferable that at least one of polyvinylidene chloride is contained. Preferably, among acrylonitrile butadiene styrene resin, acrylonitrile styrene acrylate, polyamide, polycarbonate, polyethylene, polyethylene terephthalate, polybutyl terephthalate, polymethyl methacrylate, polyacetal, polypropylene, polystyrene,
It is good that at least one of them is included.
【0050】<前記積層体5の製造方法>
* 図3及び図5に示す積層体5の製造方法
まず、図3(a)(b)に示すように前記各種積層シー
ト1に対し熱成形型7により予備賦形を施した後に、図
3(c)に示すようにこの積層シート1からその一部を
切り抜いて成形用積層シート1aとする。次に、図5
(a)(b)に示すようにこの成形用積層シート1aの
表面側にある木質層2を成形型8のキャビティ8aの内
面に沿うように当てがってこの成形用積層シート1aを
この成形型8に位置決めする。その後、図5(c)に示
すように前記キャビティ8aで前記成形用積層シート1
aの裏面側にある接着層3に面する成形空間に対し溶融
状態の熱可塑性樹脂組成物を供給してこの接着層3に対
し直接的に接触させる。なお、成形手段としては射出成
形等の従来周知のものを採用する。そして、図5(d)
に示すように成形型8から取り出した成形物の一部を切
断して積層体5とする。<Manufacturing Method of Laminate 5> * Manufacturing Method of Laminate 5 shown in FIGS. 3 and 5 First, as shown in FIGS. 3 (a) and 3 (b), a thermoforming mold is applied to each of the laminated sheets 1. After preliminarily shaping according to 7, a part of the laminated sheet 1 is cut out as shown in FIG. Next, FIG.
As shown in (a) and (b), the wood layer 2 on the surface side of the forming laminated sheet 1a is applied along the inner surface of the cavity 8a of the forming die 8 to form the forming laminated sheet 1a. Position in mold 8. After that, as shown in FIG. 5C, the molding laminated sheet 1 is formed in the cavity 8a.
The thermoplastic resin composition in a molten state is supplied to the molding space facing the adhesive layer 3 on the back surface side of a and is brought into direct contact with the adhesive layer 3. As the molding means, a conventionally known one such as injection molding is adopted. And FIG. 5 (d)
As shown in, a part of the molded product taken out from the molding die 8 is cut to obtain the laminated body 5.
【0051】* 図4及び図5に示す積層体5の製造方
法
まず、図4(a)に示すように前記各種積層シート1か
らその一部を切り抜いて成形用積層シート1aの素材と
する。次に、図4(b)に示すようにこの素材に対し熱
成形型7により予備賦形を施して成形用積層シート1a
とする。その後は、図5(a)(b)(c)(d)に示
すように同様に型成形する。* Manufacturing Method of Laminated Body 5 Shown in FIGS. 4 and 5 First, as shown in FIG. 4 (a), a part of each of the various laminated sheets 1 is cut out and used as a material for the laminated sheet for molding 1 a. Next, as shown in FIG. 4 (b), this material is preshaped by a thermoforming die 7 to form a laminated sheet 1a for molding.
And After that, as shown in FIGS. 5A, 5B, 5C, and 5D, mold molding is performed in the same manner.
【0052】* 図6に示す積層体5の製造方法
まず、射出成形等の成形手段により、積層体5の一部で
ある成形体6を予め成形する。そして、図6(a)に示
すようにこの成形体6を熱成形型7にセットする。次
に、図6(b)に示すように、加熱軟化させた各種積層
シート1を熱成形してその裏面側にある接着層3をこの
成形体6に対し直接的に接触させて貼着する。その後、
図6(c)に示すように、積層シート1からその一部を
切り抜いて積層体5とする。* Manufacturing Method of Laminated Body 5 Shown in FIG. 6 First, the molded body 6 which is a part of the laminated body 5 is molded in advance by molding means such as injection molding. Then, as shown in FIG. 6A, the molded body 6 is set in the thermoforming die 7. Next, as shown in FIG. 6B, various laminated sheets 1 that have been softened by heating are thermoformed, and the adhesive layer 3 on the back surface side is directly brought into contact with the molded body 6 to be attached. . afterwards,
As shown in FIG. 6C, a part of the laminated sheet 1 is cut out to form a laminated body 5.
【0053】〔実施例及び比較例〕次に、本発明の効果
を評価するため、後記実施例1〜4と後記比較例1とを
比較した結果を下記の表1で、後記実施例5と後記比較
例2とを比較した結果を下記の表2でそれぞれ示す。[Examples and Comparative Examples] Next, in order to evaluate the effects of the present invention, the results of comparing Examples 1 to 4 below and Comparative Example 1 below are shown in Table 1 below, and in Example 5 below. The results of comparison with Comparative Example 2 described below are shown in Table 2 below.
【0054】[0054]
【表1】 [Table 1]
【0055】[0055]
【表2】
ちなみに、上記表1及び表2において、2は木質層、3
aは接着剤のみからなる接着層、3bは接着剤を不織布
内に含浸させた接着層、4は補強層、Mはマンガシロノ
材からなる裏打ち層をそれぞれ指す。[Table 2] By the way, in Tables 1 and 2 above, 2 is a wood layer, 3
a is an adhesive layer made of only an adhesive, 3b is an adhesive layer in which a nonwoven fabric is impregnated with an adhesive, 4 is a reinforcing layer, and M is a backing layer made of mangashirono material.
【0056】* 実施例1
原木からスライスして得たクラロウォールナットの木質
シート(北三株式会社製、厚み0.1mm)と、ポリエ
ステル系ホットメルト接着剤フィルム(クランベターG
ー5PPセパレータ付き、倉敷紡績株式会社製、厚み
0.05mm、融点107℃、MFR40g/min)
とを準備する。この接着剤フィルムでPPセパレータの
ない側とこの木質シートとを互いに対向するように重ね
合わせ、さらにこの木質シートとこの接着剤フィルムと
を厚み0.5mmのステンレス平板二枚で挟む。その
後、140℃に加熱した平状熱板間にこの挟持物を挿入
して1x9.8/104 Pa(1Kgf/cm2 )の圧
力で90秒間加圧する。次いで、この挟持物を熱板から
取り出して常温中で冷却後PPセパレータを剥がし、積
層シート1を得た。* Example 1 A wood sheet of Claro walnut (manufactured by Kitasan Co., Ltd., thickness: 0.1 mm) obtained by slicing raw wood, and a polyester hot melt adhesive film (Cranbetter G
With 5PP separator, Kurashiki Spinning Co., Ltd., thickness 0.05mm, melting point 107 ° C, MFR 40g / min)
And prepare. With this adhesive film, the side without the PP separator and this wood sheet are laminated so as to face each other, and this wood sheet and this adhesive film are sandwiched between two stainless steel flat plates having a thickness of 0.5 mm. Then, this sandwich is inserted between the flat hot plates heated to 140 ° C., and pressed at a pressure of 1 × 9.8 / 10 4 Pa (1 Kgf / cm 2 ) for 90 seconds. Next, the sandwiched product was taken out from the hot plate, cooled at room temperature, and then the PP separator was peeled off to obtain a laminated sheet 1.
【0057】この積層シート1を70x100mmのサ
イズにカットし、フランジ付き70x100x3.2m
m平板金型のキャビティ内面にクラロウォールナットの
木質層2が沿うように、この積層シート1をセットす
る。この金型を閉じた後、260℃に加熱溶融したポリ
カーボネートABSアロイ樹脂(日本エイアンドエル株
式会社製、テクニエースPAXー1420)を金型キャ
ビティ内に射出注入し、この積層シート1とポリカーボ
ネートABSアロイ樹脂とを積層一体化して積層体5を
得た。This laminated sheet 1 was cut into a size of 70 × 100 mm, and a flanged 70 × 100 × 3.2 m was prepared.
The laminated sheet 1 is set so that the wood layer 2 of Claro walnut is along the inner surface of the cavity of the m flat plate mold. After closing the mold, a polycarbonate ABS alloy resin (Techniace PAX-1420 manufactured by Nippon A & L Co., Ltd.) heated and melted at 260 ° C. was injected and injected into the mold cavity, and this laminated sheet 1 and the polycarbonate ABS alloy resin were injected. And were laminated and integrated to obtain a laminated body 5.
【0058】* 実施例2
原木からスライスして得たクラロウォールナットの木質
シート(北三株式会社製、厚み0.1mm)と、ナイロ
ン不織布(厚み0.1mm)と、ポリエステル系ホット
メルト接着剤フィルム(クランベターGー5PPセパレ
ータ付き、倉敷紡績株式会社製、厚み0.05mm、融
点107℃、MFR40g/min)とを準備する。ま
ず、この木質シートとこのナイロン不織布とを重ね合わ
せ、さらにこの接着剤フィルムでPPセパレータのない
側とこのナイロン不織布とを互いに対向するように重ね
合わせ、この木質シートとこのナイロン不織布とこの接
着剤フィルムとを厚み0.5mmのステンレス平板二枚
で挟む。その後、140℃に加熱した平状熱板間にこの
挟持物を挿入して1x9.8/104 Pa(1Kgf/
cm2 )の圧力で90秒間加圧する。次いで、この挟持
物を熱板から取り出して常温中で冷却後PPセパレータ
を剥がし、積層シート1を得た。* Example 2 A wood sheet of Claro walnut (manufactured by Kitasan Co., Ltd., thickness 0.1 mm) obtained by slicing raw wood, a nylon nonwoven fabric (thickness 0.1 mm), and a polyester hot melt adhesive film ( Cranbetter G-5PP with separator, Kurashiki Spinning Co., Ltd., thickness 0.05 mm, melting point 107 ° C., MFR 40 g / min) are prepared. First, the wood sheet and the nylon non-woven fabric are laminated, and the adhesive film is laminated so that the side not having the PP separator and the nylon non-woven fabric face each other. The film and the film are sandwiched by two stainless steel plates having a thickness of 0.5 mm. After that, this sandwich was inserted between flat heating plates heated to 140 ° C. and 1 × 9.8 / 10 4 Pa (1 Kgf /
Press for 90 seconds with a pressure of cm 2 ). Next, the sandwiched product was taken out from the hot plate, cooled at room temperature, and then the PP separator was peeled off to obtain a laminated sheet 1.
【0059】この積層シート1を70x100mmのサ
イズにカットし、フランジ付き70x100x3.2m
m平板金型のキャビティ内面にクラロウォールナットの
木質層2が沿うように、この積層シート1をセットす
る。この金型を閉じた後、260℃に加熱溶融したポリ
カーボネートABSアロイ樹脂(日本エイアンドエル株
式会社製、テクニエースPAXー1420)を金型キャ
ビティ内に射出注入し、この積層シート1とポリカーボ
ネートABSアロイ樹脂とを積層一体化して積層体5を
得た。This laminated sheet 1 was cut into a size of 70 × 100 mm, and a flanged 70 × 100 × 3.2 m was prepared.
The laminated sheet 1 is set so that the wood layer 2 of Claro walnut is along the inner surface of the cavity of the m flat plate mold. After closing the mold, a polycarbonate ABS alloy resin (Techniace PAX-1420 manufactured by Nippon A & L Co., Ltd.) heated and melted at 260 ° C. was injected and injected into the mold cavity, and this laminated sheet 1 and the polycarbonate ABS alloy resin were injected. And were laminated and integrated to obtain a laminated body 5.
【0060】* 実施例3
原木からスライスして得たクラロウォールナットの木質
シート(厚み0.1mm)と、水溶性接着剤を塗布した
ナイロン不織布(補強層4に該当する部分)とを熱プレ
スにより互いに貼リ合わせて、単板(特公昭61ー53
204号公報記載の北三株式会社製化粧単板シート、厚
み0.25mm)を準備するとともに、ポリエステル系
ホットメルト接着剤フィルム(クランベターGー5PP
セパレータ付き、倉敷紡績株式会社製、厚み0.05m
m、融点107℃、MFR40g/min)を準備す
る。この接着剤フィルムでPPセパレータのない側とこ
の単板のナイロン不織布(補強層4に該当する部分)と
を互いに対向するように重ね合わせ、さらにこの単板と
この接着剤フィルムとを厚み0.5mmのステンレス平
板二枚で挟んで重ね合わせる。その後、140℃に加熱
した平状熱板間にこの挟持物を挿入して1x9.8/1
04 Pa(1Kgf/cm2 )の圧力で90秒間加圧す
る。次いで、この挟持物を熱板から取り出して常温中で
冷却後PPセパレータを剥がし、積層シート1を得た。* Example 3 A wood sheet of claro walnut (thickness 0.1 mm) obtained by slicing raw wood and a nylon non-woven fabric coated with a water-soluble adhesive (corresponding to the reinforcing layer 4) were hot-pressed. Attached to each other, veneer (Japanese Patent Publication Sho 61-53)
The Kitasan Co., Ltd. decorative veneer sheet described in No. 204, thickness 0.25 mm) is prepared, and a polyester hot melt adhesive film (Cranbetter G-5PP) is prepared.
With separator, Kurashiki Spinning Co., Ltd., thickness 0.05m
m, melting point 107 ° C., MFR 40 g / min). With this adhesive film, the side without the PP separator and the nylon nonwoven fabric (the portion corresponding to the reinforcing layer 4) of this veneer are laminated so as to face each other, and the veneer and this adhesive film are made to have a thickness of 0. It is sandwiched between two 5 mm stainless steel flat plates and stacked. Then, insert this sandwich between flat heating plates heated to 140 ° C. and 1 × 9.8 / 1.
Pressurize at a pressure of 0 4 Pa (1 Kgf / cm 2 ) for 90 seconds. Next, the sandwiched product was taken out from the hot plate, cooled at room temperature, and then the PP separator was peeled off to obtain a laminated sheet 1.
【0061】この積層シート1を70x100mmのサ
イズにカットし、フランジ付き70x100x3.2m
m平板金型のキャビティ内面にクラロウォールナットの
木質層2が沿うように、この積層シート1をセットす
る。この金型を閉じた後、260℃に加熱溶融したポリ
カーボネートABSアロイ樹脂(日本エイアンドエル株
式会社製、テクニエースPAXー1420)を金型キャ
ビティ内に射出注入し、この積層シート1とポリカーボ
ネートABSアロイ樹脂とを積層一体化して積層体5を
得た。This laminated sheet 1 is cut into a size of 70 × 100 mm, and is provided with a flange 70 × 100 × 3.2 m
The laminated sheet 1 is set so that the wood layer 2 of Claro walnut is along the inner surface of the cavity of the m flat plate mold. After closing the mold, a polycarbonate ABS alloy resin (Techniace PAX-1420 manufactured by Nippon A & L Co., Ltd.) heated and melted at 260 ° C. was injected and injected into the mold cavity, and this laminated sheet 1 and the polycarbonate ABS alloy resin were injected. And were laminated and integrated to obtain a laminated body 5.
【0062】* 実施例4
原木からスライスして得たクラロウォールナットの木質
シート(厚み0.1mm)と、水溶性接着剤を塗布した
ナイロン不織布(補強層4に該当する部分)とを熱プレ
スにより互いに貼リ合わせて、単板(特公昭61ー53
204号公報記載の北三株式会社製化粧単板シート、厚
み0.25mm)を準備するとともに、接着層3に該当
する部分であるナイロン不織布(厚み0.1mm)及び
ポリエステル系ホットメルト接着剤フィルム(クランベ
ターG−5PPセパレータ付き、倉敷紡績株式会社製、
厚み0.05mm、融点107℃、MFR40g/mi
n)を準備する。まず、この単板のナイロン不織布(補
強層4に該当する部分)とこのナイロン不織布(接着層
3に該当する部分)とを重ね合わせ、さらにこの接着剤
フィルムでPPセパレータのない側とこのナイロン不織
布(接着層3に該当する部分)とを互いに対向するよう
に重ね合わせ、これらを厚み0.5mmのステンレス平
板二枚で挟む。その後、140℃に加熱した平状熱板間
にこの挟持物を挿入して1x9.8/104 Pa(1K
gf/cm2 )の圧力で90秒間加圧する。次いで、こ
の挟持物を熱板から取り出して常温中で冷却後PPセパ
レータを剥がし、積層シート1を得た。* Example 4 A wood sheet of claro walnut (thickness 0.1 mm) obtained by slicing raw wood and a nylon nonwoven fabric coated with a water-soluble adhesive (corresponding to the reinforcing layer 4) were subjected to hot pressing. Attached to each other, veneer (Japanese Patent Publication Sho 61-53)
The Kitasan Co., Ltd. decorative veneer sheet described in No. 204, thickness 0.25 mm) is prepared, and the nylon nonwoven fabric (thickness 0.1 mm) and the polyester hot melt adhesive film (corresponding to the adhesive layer 3) are prepared. Cranbetter G-5PP with separator, Kurashiki Spinning Co., Ltd.,
Thickness 0.05mm, melting point 107 ° C, MFR 40g / mi
n) is prepared. First, the single-ply nylon nonwoven fabric (the portion corresponding to the reinforcing layer 4) and the nylon nonwoven fabric (the portion corresponding to the adhesive layer 3) are superposed, and the adhesive film does not have the PP separator side and the nylon nonwoven fabric. (A portion corresponding to the adhesive layer 3) is laminated so as to face each other, and these are sandwiched by two stainless steel flat plates having a thickness of 0.5 mm. After that, this sandwich is inserted between flat heating plates heated to 140 ° C. and 1 × 9.8 / 10 4 Pa (1K
Pressurize at a pressure of gf / cm 2 ) for 90 seconds. Next, the sandwiched product was taken out from the hot plate, cooled at room temperature, and then the PP separator was peeled off to obtain a laminated sheet 1.
【0063】この積層シート1を70x100mmのサ
イズにカットし、フランジ付き70x100x3.2m
m平板金型のキャビティ内面にクラロウォールナットの
木質層2が沿うように、この積層シート1をセットす
る。この金型を閉じた後、260℃に加熱溶融したポリ
カーボネートABSアロイ樹脂(日本エイアンドエル株
式会社製、テクニエースPAXー1420)を金型キャ
ビティ内に射出注入し、この積層シート1とポリカーボ
ネートABSアロイ樹脂とを積層一体化して積層体5を
得た。This laminated sheet 1 was cut into a size of 70 × 100 mm, and a flanged 70 × 100 × 3.2 m was used.
The laminated sheet 1 is set so that the wood layer 2 of Claro walnut is along the inner surface of the cavity of the m flat plate mold. After closing the mold, a polycarbonate ABS alloy resin (Techniace PAX-1420 manufactured by Nippon A & L Co., Ltd.) heated and melted at 260 ° C. was injected and injected into the mold cavity, and this laminated sheet 1 and the polycarbonate ABS alloy resin were injected. And were laminated and integrated to obtain a laminated body 5.
【0064】* 比較例1
原木からスライスして得たクラロウォールナットの木質
シート(厚み0.1mm)と、水溶性接着剤を塗布した
ナイロン不織布(補強層4に該当する部分)とを熱プレ
スにより互いに貼リ合わせて、単板(特公昭61ー53
204号公報記載の北三株式会社製化粧単板シート、厚
み0.25mm)を準備する。熱可塑性樹脂組成物との
積層一体化時のアンカー効果(凹凸による密着効果)を
得るためにマンガシロノ材からなる裏打ち層Mをこの単
板のナイロン不織布(補強層4に該当する部分)に積層
して積層シート1(北三株式会社製、厚み0.35m
m)とする。この積層シート1を70x100mmのサ
イズにカットし、フランジ付き70x100x3.2m
m平板金型のキャビティ内面にクラロウォールナットの
木質層2が沿うように、この積層シート1をセットす
る。この金型を閉じた後、260℃に加熱溶融したポリ
カーボネートABSアロイ樹脂(日本エイアンドエル株
式会社製、テクニエースPAXー1420)を金型キャ
ビティ内に射出注入し、この積層シート1とポリカーボ
ネートABSアロイ樹脂とを積層一体化して積層体5を
得た。
* 実施例5
原木からスライスして得たクラロウォールナットの木質
シート(厚み0.1mm)と、水溶性接着剤を塗布した
ナイロン不織布(補強層4に該当する部分)とを熱プレ
スにより互いに貼リ合わせて、単板(特公昭61ー53
204号公報記載の北三株式会社製化粧単板シート、厚
み0.25mm)を準備するとともに、ポリエステル系
ホットメルト接着剤フィルム(クランベターG−5PP
セパレータ付き、倉敷紡績株式会社製、厚み0.05m
m、融点107℃、MFR40g/min)を準備す
る。この接着剤フィルムでPPセパレータのない側とこ
の単板のナイロン不織布(補強層4に該当する部分)と
を互いに対向するように重ね合わせ、さらにこの単板と
この接着剤フィルムとを厚み0.5mmのステンレス平
板二枚で挟む。その後、140℃に加熱した平状熱板間
にこの挟持物を挿入して1x9.8/104 Pa(1K
gf/cm2 )の圧力で90秒間加圧する。次いで、こ
の挟持物を熱板から取り出して常温中で冷却後PPセパ
レータを剥がし、積層シート1を得た。Comparative Example 1 A wood sheet of claro walnut (thickness 0.1 mm) obtained by slicing raw wood and a nylon non-woven fabric coated with a water-soluble adhesive (corresponding to the reinforcing layer 4) were hot-pressed. Attached to each other, veneer (Japanese Patent Publication Sho 61-53)
A decorative veneer sheet manufactured by Kitasan Co., Ltd., having a thickness of 0.25 mm) described in Japanese Patent No. In order to obtain an anchor effect (adhesion effect due to unevenness) at the time of lamination and integration with a thermoplastic resin composition, a backing layer M made of mangashirono material is laminated on this single-sheet nylon nonwoven fabric (corresponding to the reinforcing layer 4). And laminated sheet 1 (made by Kitasan Co., Ltd., thickness 0.35 m
m). This laminated sheet 1 is cut into a size of 70x100 mm and has a flange 70x100x3.2 m
The laminated sheet 1 is set so that the wood layer 2 of Claro walnut is along the inner surface of the cavity of the m flat plate mold. After closing the mold, a polycarbonate ABS alloy resin (Techniace PAX-1420 manufactured by Nippon A & L Co., Ltd.) heated and melted at 260 ° C. was injected and injected into the mold cavity, and this laminated sheet 1 and the polycarbonate ABS alloy resin were injected. And were laminated and integrated to obtain a laminated body 5. * Example 5 A wood sheet (thickness: 0.1 mm) of claro walnut obtained by slicing raw wood and a nylon non-woven fabric coated with a water-soluble adhesive (corresponding to the reinforcing layer 4) are pasted together by heat pressing. In addition, a single plate (Japanese Patent Publication Sho 61-53)
The Kitasan Co., Ltd. decorative veneer sheet described in Japanese Patent No. 204, thickness 0.25 mm) is prepared, and a polyester-based hot melt adhesive film (Cranbetter G-5PP) is prepared.
With separator, Kurashiki Spinning Co., Ltd., thickness 0.05m
m, melting point 107 ° C., MFR 40 g / min). With this adhesive film, the side without the PP separator and the nylon nonwoven fabric (the portion corresponding to the reinforcing layer 4) of this veneer are laminated so as to face each other, and the veneer and this adhesive film are made to have a thickness of 0. It is sandwiched between two 5 mm stainless steel flat plates. After that, this sandwich is inserted between flat heating plates heated to 140 ° C. and 1 × 9.8 / 10 4 Pa (1K
Pressurize at a pressure of gf / cm 2 ) for 90 seconds. Next, the sandwiched product was taken out from the hot plate, cooled at room temperature, and then the PP separator was peeled off to obtain a laminated sheet 1.
【0065】この積層シート1を自動車シフトノブ化粧
部材の意匠展開形状にカットし、この積層シート1の木
質層2に水分を含ませた後、100℃に加熱した熱プレ
ス金型によりこの積層シート1を0.1x9.8/10
4 Pa(0.1Kgf/cm 2 )の圧力で120秒間加
圧して予備賦形を行った。次いで、予備賦形した積層シ
ート1を射出成形金型のキャビティ内面にクラロウォー
ルナットの木質層2が沿うように、この積層シート1を
セットする。この金型を閉じた後、260℃に加熱溶融
したポリカーボネートABSアロイ樹脂(日本エイアン
ドエル株式会社製、テクニエースPAXー1420)を
金型キャビティ内に射出注入し、この積層シート1とポ
リカーボネートABSアロイ樹脂とを積層一体化して積
層体5を得た。This laminated sheet 1 is applied to an automobile shift knob
The wood of this laminated sheet 1 cut into the design development shape of the member
After preliminarily moistening the quality layer 2, heat preheated to 100 ° C
0.1 x 9.8 / 10 of this laminated sheet 1 by a die
FourPa (0.1 Kgf / cm 2) Pressure for 120 seconds
Preliminary shaping was performed by pressing. Then, the pre-shaped laminated sheet
1 on the inner surface of the cavity of the injection mold.
Place this laminated sheet 1 so that the lunate wood layer 2 is along.
set. After closing this mold, heat and melt to 260 ℃
Polycarbonate ABS alloy resin (Japan Aian
Techniace PAX-1420 made by Dwell Co., Ltd.
It is injected and injected into the mold cavity and the laminated sheet 1 and po
Laminated and integrated with polycarbonate ABS alloy resin
A layered body 5 was obtained.
【0066】* 比較例2
原木からスライスして得たクラロウォールナットの木質
シート(厚み0.1mm)と、水溶性接着剤を塗布した
ナイロン不織布(補強層4に該当する部分)とを熱プレ
スにより互いに貼リ合わせて、単板(特公昭61ー53
204号公報記載の北三株式会社製化粧単板シート、厚
み0.25mm)を準備する。熱可塑性樹脂組成物との
積層一体化時のアンカー効果(凹凸による密着効果)を
得るためにマンガシロノ材からなる裏打ち層Mをこの単
板のナイロン不織布(補強層4に該当する部分)に積層
して積層シート1(北三株式会社製、厚み0.35m
m)とする。この積層シート1を自動車シフトノブ化粧
部材の意匠展開形状にカットし、この積層シート1の木
質層2に水分を含ませた後、100℃に加熱した熱プレ
ス金型によりこの積層シート1を5x9.8/104 P
a(5Kgf/cm2)の圧力で10分間加圧して予備
賦形を行った。次いで、予備賦形した積層シート1を射
出成形金型のキャビティ内面にクラロウォールナットの
木質層2が沿うように、この積層シート1をセットす
る。この金型を閉じた後、260℃に加熱溶融したポリ
カーボネートABSアロイ樹脂(日本エイアンドエル株
式会社製、テクニエースPAXー1420)を金型キャ
ビティ内に射出注入し、この積層シート1とポリカーボ
ネートABSアロイ樹脂とを積層一体化して積層体5を
得た。Comparative Example 2 A wood sheet of claro walnut (thickness 0.1 mm) obtained by slicing raw wood and a nylon nonwoven fabric coated with a water-soluble adhesive (corresponding to the reinforcing layer 4) were hot-pressed. Attached to each other, veneer (Japanese Patent Publication Sho 61-53)
A decorative veneer sheet manufactured by Kitasan Co., Ltd., having a thickness of 0.25 mm) described in Japanese Patent No. In order to obtain an anchor effect (adhesion effect due to unevenness) at the time of lamination and integration with a thermoplastic resin composition, a backing layer M made of mangashirono material is laminated on this single-sheet nylon nonwoven fabric (corresponding to the reinforcing layer 4). And laminated sheet 1 (made by Kitasan Co., Ltd., thickness 0.35 m
m). This laminated sheet 1 was cut into a design-developed shape of an automobile shift knob decorative member, the wood layer 2 of this laminated sheet 1 was moistened, and then the laminated sheet 1 was heated to 100 ° C. to obtain 5 × 9. 8/10 4 P
Preliminary shaping was performed by applying a pressure of a (5 Kgf / cm 2 ) for 10 minutes. Next, the preformed laminated sheet 1 is set such that the wood layer 2 of Claro walnut is along the inner surface of the cavity of the injection molding die. After closing the mold, a polycarbonate ABS alloy resin (Techniace PAX-1420 manufactured by Nippon A & L Co., Ltd.) heated and melted at 260 ° C. was injected and injected into the mold cavity, and this laminated sheet 1 and the polycarbonate ABS alloy resin were injected. And were laminated and integrated to obtain a laminated body 5.
【0067】* 本発明の効果の評価
上記表で示した成形条件幅、製品外観及び予備賦形性に
関する評価法は、それぞれ次の通りである。* Evaluation of the Effect of the Present Invention The evaluation methods relating to the molding condition width, product appearance and preliminary shapeability shown in the above table are as follows.
【0068】成形条件幅については、積層シート1を金
型キャビティの内面に沿わせてセットし、この金型を閉
じた後、加熱溶融した熱可塑性樹脂組成物を金型キャビ
ティ内に射出注入する場合に生じる最大射出圧力から判
断し、この最大射出圧力が低いほど成形条件幅が広いこ
とを示す。With respect to the molding condition width, the laminated sheet 1 is set along the inner surface of the mold cavity, the mold is closed, and then the heat-melted thermoplastic resin composition is injected and injected into the mold cavity. Judging from the maximum injection pressure generated in some cases, the lower the maximum injection pressure, the wider the molding condition range.
【0069】製品外観については、積層シート1と熱可
塑性樹脂組成物とを積層一体化して得られた積層体5に
おいて積層シート1の木口近傍の熱可塑性樹脂組成物表
面に現れた裏打ち材の小片の有無で判断する。Regarding the product appearance, in the laminate 5 obtained by laminating and integrating the laminated sheet 1 and the thermoplastic resin composition, a small piece of the backing material appeared on the surface of the thermoplastic resin composition near the mouth of the laminated sheet 1. Judge by the presence or absence of
【0070】予備賦形性については、積層シート1を熱
プレスにより予備賦形する場合に必要な加圧力及び時間
とその場合に生じ得る割れとにより判断し、低圧力及び
短時間で所望の形状に賦形できるとともに割れもない場
合は良好であるとする。Preliminary shapeability is judged by the pressure and time required for preforming the laminated sheet 1 by hot pressing and the cracks that may occur in that case, and the desired shape can be obtained at low pressure and for a short time. It is considered to be good if it can be shaped into and has no cracks.
【0071】上記評価法により判断すると、成形条件
幅、製品外観及び予備賦形性についていずれも前記実施
例1〜5が比較例1〜2よりも改善されていることが分
かる。Judging by the above evaluation method, it can be seen that Examples 1 to 5 are improved over Comparative Examples 1 and 2 in terms of molding condition width, product appearance and preformability.
【0072】[0072]
【発明の効果】請求項1〜10の発明にかかる積層シー
ト(1)によれば、従来から積層シートの裏打ち材とし
て使用されているマンガシロノ材等の木質シートに代え
て、熱可塑性樹脂組成物(成形体6)に対し接着性を持
つ接着剤を有する接着層(3)を採用した。従って、積
層シート(1)に柔軟性を持たせて積層シート(1)を
所望の形状に予備賦形し易くなる。また、積層シート
(1)と熱可塑性樹脂組成物(成形体6)との間で一定
の密着強度を得るために接着層(3)に熱可塑性樹脂組
成物(成形体6)を高圧で押し付ける必要がなくなると
ともに、熱可塑性樹脂組成物(成形体6)に対する接着
層(3)自体の接着性により一定の密着強度を得ること
ができ、請求項11〜12の発明にかかる積層体(5)
を製造する場合、成形条件幅が広くなるとともに、従来
から問題になっていた木質シートからの剥離による散在
小片が積層体(5)の成形体(6)の表面に現れず、優
れた意匠性を持たせることができる。さらに、請求項1
3〜16の発明にかかる積層体(5)の製造方法は、上
記積層体(5)の製造に適している。According to the laminated sheet (1) of the present invention, a thermoplastic resin composition is used in place of a wood sheet such as mangashirono material which has been conventionally used as a backing material for laminated sheets. The adhesive layer (3) having an adhesive having adhesiveness to the (molded body 6) was adopted. Therefore, the laminated sheet (1) can be made flexible and preliminarily shaped into a desired shape. Further, the thermoplastic resin composition (molded body 6) is pressed against the adhesive layer (3) under high pressure in order to obtain a constant adhesion strength between the laminated sheet (1) and the thermoplastic resin composition (molded body 6). A layered product (5) according to the invention of claims 11 to 12, in which a constant adhesion strength can be obtained due to the adhesiveness of the adhesive layer (3) itself to the thermoplastic resin composition (molded product 6) while eliminating the need.
In the case of manufacturing the product, the molding condition range is widened, and scattered small pieces due to peeling from the wood sheet, which has been a problem in the past, do not appear on the surface of the molded product (6) of the laminated body (5), and excellent designability is obtained. Can have Further, claim 1
The method for producing a laminate (5) according to the inventions 3 to 16 is suitable for producing the laminate (5).
【図1】 (a)は本実施形態にかかる積層シートの全
体を示す斜視図であり、(b)は本実施形態にかかる積
層体の全体を示す斜視図である。FIG. 1A is a perspective view showing an entire laminated sheet according to this embodiment, and FIG. 1B is a perspective view showing an entire laminated body according to this embodiment.
【図2】 各種積層シートの積層断面構造を拡大して示
す模式図である。FIG. 2 is an enlarged schematic view showing a laminated sectional structure of various laminated sheets.
【図3】 上記積層シートの予備賦形方法を示す工程図
である。FIG. 3 is a process drawing showing a preliminary shaping method for the laminated sheet.
【図4】 上記積層シートの予備賦形方法を示す工程図
である。FIG. 4 is a process diagram showing a method of preliminarily shaping the laminated sheet.
【図5】 上記積層体の製造方法を示す工程図である。FIG. 5 is a process drawing showing the method for manufacturing the above-mentioned laminated body.
【図6】 上記積層体の製造方法を示す工程図である。FIG. 6 is a process drawing showing the method for manufacturing the above-mentioned laminated body.
1…積層シート、1a…成形用積層シート、2…木質
層、3…接着層、4…補強層、5…積層体、6…熱可塑
性樹脂組成物製成形体、8…成形型、8a…キャビテ
ィ。DESCRIPTION OF SYMBOLS 1 ... Laminated sheet, 1a ... Laminated sheet for molding, 2 ... Wood layer, 3 ... Adhesive layer, 4 ... Reinforcing layer, 5 ... Laminated body, 6 ... Thermoplastic resin composition molded body, 8 ... Mold, 8a ... cavity.
───────────────────────────────────────────────────── フロントページの続き (51)Int.Cl.7 識別記号 FI テーマコート゛(参考) B32B 27/04 B32B 27/04 A C09J 7/02 C09J 7/02 Z 167/00 167/00 Fターム(参考) 4F100 AK41B AK41G AK74D AK74G AP01A BA03 BA04 BA07 BA10A CB03B DG15C EH36 EJ82C GB33 JL11B JL12B 4F206 AA13 AD06 AD08 AD16 AD20 AD27 AG03 AH26 JA07 JB13 JB15 JF05 JQ81 4J004 AA15 AB03 CA02 CA03 CA04 CA06 CB01 CC02 CC03 4J040 CA011 CA081 CA111 DA051 DA061 DA071 DA101 DA111 DA121 DA141 DD051 DF041 DM011 ED001 EF001 EG001 EK031 EL021 JA09 JB01 JB09 LA06 MA08 MA10 MB02 NA11 ─────────────────────────────────────────────────── ─── Continuation of front page (51) Int.Cl. 7 identification code FI theme code (reference) B32B 27/04 B32B 27/04 A C09J 7/02 C09J 7/02 Z 167/00 167/00 F term ( Reference) 4F100 AK41B AK41G AK74D AK74G AP01A BA03 BA04 BA07 BA10A CB03B DG15C EH36 EJ82C GB33 JL11B JL12B 4F206 AA13 AD06 AD08 AD16 AD20 AD27 AG03 CA1 CA01 CA01 CA01 CA01 CA01 CA01 CA01 CA02 CA01 CA02 CA01 CA02 CA01 CA02 CA01 CA02 CA01 CA02 CA01 CA02 CA01 CA01 CA01 CA01 CA01 CA01 DA101 DA111 DA121 DA141 DD051 DF041 DM011 ED001 EF001 EG001 EK031 EL021 JA09 JB01 JB09 LA06 MA08 MA10 MB02 NA11
Claims (16)
スした木質層と、熱可塑性樹脂組成物に対し接着性を持
つ接着剤を有する接着層とを備え、この木質層とこの接
着層とを互いに積層して一体化し、この木質層を表面側
に露出させるとともに、この接着層を裏面側に露出させ
たことを特徴とする積層シート。1. A wood layer, which is mainly composed of natural wood and is sliced to a predetermined thickness, and an adhesive layer having an adhesive having adhesiveness to a thermoplastic resin composition. The wood layer and the adhesive layer are provided. A laminated sheet, which is laminated and integrated with each other to expose the wood layer on the front surface side and the adhesive layer on the back surface side.
的に接触させて二層構造としたことを特徴とする請求項
1に記載の積層シート。2. The laminated sheet according to claim 1, wherein the wood layer and the adhesive layer are in direct contact with each other to form a two-layer structure.
記接着層との間に介在させてこの木質層とこの補強層と
を互いに直接的に接触させるとともにこの補強層とこの
接着層とを互いに直接的に接触させ、この木質層とこの
補強層とこの接着層とを互いに積層して一体化した三層
構造としたことを特徴とする請求項1に記載の積層シー
ト。3. A reinforcing layer having flexibility is interposed between the wood layer and the adhesive layer to bring the wood layer and the reinforcing layer into direct contact with each other, and the reinforcing layer and the adhesive layer. 2. The laminated sheet according to claim 1, wherein the wood layers, the reinforcing layers, and the adhesive layers are laminated on each other so as to be in direct contact with each other to form a three-layer structure.
であることを特徴とする請求項3に記載の積層シート。4. The thickness of the reinforcing layer is 0.1 to 0.4 mm.
The laminated sheet according to claim 3, wherein
とする請求項3または請求項4に記載の積層シート。5. The laminated sheet according to claim 3, wherein the reinforcing layer is made of a non-woven fabric.
であり、前記接着層の厚みは0.05〜0.2mmであ
ることを特徴とする請求項1から請求項5のうちいずれ
かの請求項に記載の積層シート。6. The wood layer has a thickness of 0.1 to 0.4 mm.
The thickness of the adhesive layer is 0.05 to 0.2 mm, and the laminated sheet according to any one of claims 1 to 5.
に含浸させた接着剤とからなることを特徴とする請求項
1から請求項6のうちいずれかの請求項に記載の積層シ
ート。7. The laminated sheet according to claim 1, wherein the adhesive layer comprises a non-woven fabric and an adhesive impregnated in the non-woven fabric.
クリルニトリルブタジエンスチレン樹脂)に対し接着性
を持つことを特徴とする請求項1から請求項7のうちい
ずれかの請求項に記載の積層シート。8. The adhesive according to claim 1, wherein the adhesive of the adhesive layer has adhesiveness to an ABS resin (acrylonitrile butadiene styrene resin). Laminated sheet.
着剤であることを特徴とする請求項1から請求項8のう
ちいずれかの請求項に記載の積層シート。9. The laminated sheet according to claim 1, wherein the adhesive agent of the adhesive layer is a hot melt adhesive agent.
は、ポリエステル系のものであることを特徴とする請求
項9に記載の積層シート。10. The laminated sheet according to claim 9, wherein the hot melt adhesive which is the adhesive is a polyester adhesive.
かの請求項に記載の積層シートと、この積層シートの裏
面側にある接着層に対し直接的に接触させて一体化した
熱可塑性樹脂組成物からなる成形体とからなることを特
徴とする積層体。11. A thermoplastic resin which is integrated by directly contacting the laminated sheet according to any one of claims 1 to 10 with an adhesive layer on the back side of the laminated sheet. A laminated body comprising a molded body made of the composition.
成物はABS樹脂(アクリルニトリルブタジエンスチレ
ン樹脂)を含むことを特徴とする請求項11に記載の積
層体。12. The laminate according to claim 11, wherein the thermoplastic resin composition forming the molded body contains an ABS resin (acrylonitrile butadiene styrene resin).
かの請求項に記載の積層シートからその一部を切り抜い
て成形用積層シートとし、 前記成形用積層シートの表面側にある木質層を成形型の
キャビティの内面に沿うように当てがってこの成形用積
層シートをこの成形型に位置決めし、 前記キャビティで前記成形用積層シートの裏面側にある
接着層に面する成形空間に対し溶融状態の熱可塑性樹脂
組成物を供給してこの接着層に対し直接的に接触させ、
この熱可塑性樹脂組成物からなる成形体とこの成形用積
層シートとを一体化した積層体を製造することを特徴と
する積層体の製造方法。13. A laminated sheet for molding, which is obtained by cutting out a part of the laminated sheet according to any one of claims 1 to 10 to form a wood layer on the front surface side of the laminated sheet for molding. The molding laminated sheet is positioned so as to fit along the inner surface of the cavity of the molding die in the molding die, and melted in the molding space facing the adhesive layer on the back side of the molding laminated sheet in the cavity. The thermoplastic resin composition in the state is supplied to directly contact the adhesive layer,
A method for producing a laminated body, comprising producing a laminated body in which a formed body made of the thermoplastic resin composition and the forming laminated sheet are integrated.
かの請求項に記載の積層シートに対し予備賦形を施した
後にこの積層シートからその一部を切り抜いて成形用積
層シートとするか、または、請求項1から請求項10の
うちいずれかの請求項に記載の積層シートからその一部
を切り抜いて成形用積層シートとした後にこの成形用積
層シートに対し予備賦形を施し、 前記成形用積層シートの表面側にある木質層を成形型の
キャビティの内面に沿うように当てがってこの成形用積
層シートをこの成形型に位置決めし、 前記キャビティで前記成形用積層シートの裏面側にある
接着層に面する成形空間に対し溶融状態の熱可塑性樹脂
組成物を供給してこの接着層に対し直接的に接触させ、
この熱可塑性樹脂組成物からなる成形体とこの成形用積
層シートとを一体化した積層体を製造することを特徴と
する積層体の製造方法。14. A laminated sheet for molding according to any one of claims 1 to 10, which is obtained by subjecting the laminated sheet according to any one of claims 1 to 10 to preliminary shaping and then cutting out a part of the laminated sheet. Alternatively, a part of the laminated sheet according to any one of claims 1 to 10 is cut out to form a laminated sheet for molding, and then preliminary shaping is performed on the laminated sheet for molding, The wood layer on the front surface side of the molding laminated sheet is applied along the inner surface of the cavity of the molding die to position this molding laminated sheet in the molding die, and the back surface side of the molding laminated sheet in the cavity. The thermoplastic resin composition in a molten state is supplied to the molding space facing the adhesive layer to directly contact the adhesive layer,
A method for producing a laminated body, comprising producing a laminated body in which a formed body made of the thermoplastic resin composition and the forming laminated sheet are integrated.
め成形し、 請求項1から請求項10のうちいずれかの請求項に記載
の積層シートの裏面側にある接着層をこの成形体に対し
直接的に接触させてこの積層シートを熱成形し、この成
形体とこの積層シートとを一体化した積層体を製造する
ことを特徴とする積層体の製造方法。15. A molded body is molded in advance with a thermoplastic resin composition, and an adhesive layer on the back surface side of the laminated sheet according to claim 1 is attached to this molded body. A method for producing a laminated body, which comprises directly forming a thermoform of the laminated sheet by directly contacting with each other to produce a laminated body in which the formed body and the laminated sheet are integrated.
(アクリルニトリルブタジエンスチレン樹脂)を含むこ
とを特徴とする請求項13または請求項14または請求
項15に記載の積層体の製造方法。16. The method for producing a laminated body according to claim 13, 14 or 15, wherein the thermoplastic resin composition contains an ABS resin (acrylonitrile butadiene styrene resin).