Nothing Special   »   [go: up one dir, main page]

CN1106433A - Resin rubber anti-corrosive and waterproof paint - Google Patents

Resin rubber anti-corrosive and waterproof paint Download PDF

Info

Publication number
CN1106433A
CN1106433A CN 94111417 CN94111417A CN1106433A CN 1106433 A CN1106433 A CN 1106433A CN 94111417 CN94111417 CN 94111417 CN 94111417 A CN94111417 A CN 94111417A CN 1106433 A CN1106433 A CN 1106433A
Authority
CN
China
Prior art keywords
corrosive
powder
epoxy
resins
mixed solvent
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN 94111417
Other languages
Chinese (zh)
Other versions
CN1056397C (en
Inventor
黄爱江
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN94111417A priority Critical patent/CN1056397C/en
Publication of CN1106433A publication Critical patent/CN1106433A/en
Application granted granted Critical
Publication of CN1056397C publication Critical patent/CN1056397C/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

The anticorrosion, water-proof paint for building material is prepared with resin, rubber and others by proportional mixing and features high adhesion, not layering, and quick drying.

Description

Resin rubber anti-corrosive and waterproof paint
The present invention relates to a kind of coating, particularly a kind of anti-corrosive and waterproof paint that prevents metallic corrosion and building materials percolating water.
Prevent that in the coating of metallic corrosion, epoxy resin series coating exists easily crisp critical defect, the hydroxyl in the novolac systems coating easily and alkali have an effect not enough, the easy aliquation of chlorosulphonation polyene paint adhesion.Above-mentioned these coating all are two-component materials, and levelling is not smooth, and construction is extremely inconvenient.
In the middle of the waterproof paint, coating such as synthetic rubber series, sponge structure series, emulsified bitumen series exist high temperature and are prone to the trickling phenomenon, and became uneven, low temperature easily produce crack performance.Though more novel cold subsides coiled material can adapt to difference variation, but because bottom surface structure difference, it is synthetic because of the velocity of variation disunity, very easily separates, lose protective effect, especially very easily produce phenomenons such as seepage and gas pickling at handing-over mouthful, edge lines such as parapet bears down on one, outfall sewer mouth, expansion joint.
Deposed polystyrene is big public hazards that influence environment, pollute.Though existing utilize deposed polystyrene resin synthetic paint, exist following defective: curing cycle is long, easily crisp, and the oil silk is long and can not spray, levelling is difficult to overcome, aromaticity content is too high, and can only be used for waterproof, and can not be used to prevent metallic corrosion, application is restricted.
Purpose of the present invention will overcome above-mentioned defective exactly, develops a kind of coating that prevents metallic corrosion, building materials percolating water.
Technical scheme of the present invention:
Pressing column weight amount per-cent by following composition forms:
A, anti-corrosive type
Mixed solvent 46-48
Deposed polystyrene 11-14
Resins, epoxy 7-10
Viscose material 8-11
Film coalescence aid 5-8
Pigment 5-9
Zinc oxide 0.4-1.4
Talcum powder 2.7-4.3
Mica powder 1.3-3.4
Mishmetal siccative 0.4-0.9
B, waterproof type
Mixed solvent 46-48
Deposed polystyrene 11-14
Resins, epoxy 2.0-3.5
Viscose material 5-7.5
Pitch 9-12
Film coalescence aid 2.5-4.5
Asbestos powder 4.5-7.5
Barium sulfate 5-8
Silicon-dioxide 0.5-3.0
Superiority of the present invention is to make full use of deposed polystyrene, defectives such as curing cycle is long, easily crisp, oil silk is long have been solved, can spray, aromaticity content reduces, overcome levelling, and not only can be used for the building materials waterproof, and also can be used for preventing metallic corrosion, do not exist the defective of common metal protective system yet.
Embodiment 1:
A, anti-corrosive type
Mixed solvent 47.4
Deposed polystyrene 13.0
Resins, epoxy 8.6
Viscose material 8.8
Film coalescence aid 7.4
Pigment 7.8
Zinc oxide 1.1
Talcum powder 3.1
Mica powder 2.1
Mix alkene soil siccative 0.7
Wherein, mixed solvent is that No. 200 chemical solventss account for 80%, and dimethylbenzene accounts for 20%, and deposed polystyrene is exactly useless foamed resin, and Resins, epoxy adopts 6101, and viscose material is JX-23, and pigment is oxide pigment or titanium dioxide.Be mixed in proportion separately, stir, promptly get protective system with the thinner dilution again.
B, waterproof type
Pigment in a anti-corrosive type, zinc oxide, talcum powder, mica powder, mishmetal siccative are changed to pitch, asbestos powder, barium sulfate, silicon-dioxide.
Mixed solvent 47.4
Deposed polystyrene 13
Resins, epoxy 3.0
Viscose material 7.0
Pitch 10.6
Film coalescence aid 4.0
Asbestos powder 6.0
Barium sulfate 7.0
Silicon-dioxide 2.0
Its medium pitch adopts No. 10 petroleum pitch, mixes according to the above ratio, stirs, and gets final product with the thinner dilution again.
Through detecting, data are as follows:
Appearance of film: smooth, color and luster is even; Time of drying: surface drying 1h, do solid work 2h, viscosity s:110, sticking power (%): 100; Opacifying power: 78(g/m); Shock strength: 50(kg, cm); Hardness: 0.50; High thermal resistance; 150c.4h it is no abnormal to film; Winter hardiness :-20 ℃, 6h is normal; Acid resistance 48h, normal (40%HCl solution); Normal (40%NaOH) solution of alkali resistance 48h); Water tolerance: 48h is normal.Detect through Jiangsu Province's health and epidemic prevention inspection center, belong to nontoxic type coating.
Embodiment 2:
A, anti-corrosive type
Mixed solvent 47.4
Deposed polystyrene 13.0
Resins, epoxy 8.2
Viscose material 8.6
Film coalescence aid 7.5
Pigment 8.1
Zinc oxide 1.2
Talcum powder 3.3
Mica powder 2.0
Mishmetal siccative 0.7
Surplus all with embodiment 1.
B, waterproof type
Mixed solvent 47.4
Deposed polystyrene 13.0
Resins, epoxy 3.1
Viscose material 7.2
Pitch 10.2
Film coalescence aid 4.0
Asbestos powder 6.3
Barium sulfate 7.0
Silica 1 .8
Surplus all with embodiment 1.

Claims (3)

1, resin rubber anti-corrosive and waterproof paint is characterized in that pressing column weight amount per-cent by following composition forms:
A, anti-corrosive type
Mixed solvent 46-48
Deposed polystyrene 11-14
Resins, epoxy 7-10
Viscose material 8-11
Film coalescence aid 5-8
Pigment 5-19
Zinc oxide 0.4-1.4
Talcum powder 2.7-4.3
Mica powder 1.3-3.4
Mishmetal siccative 0.4-0.9
B, waterproof type
Pigment, zinc oxide, talcum powder, mica powder, mishmetal siccative in (a) are removed, are added pitch, asbestos powder, barium sulfate, silicon-dioxide mixing:
Mixed solvent 46-48
Deposed polystyrene 11-14
Resins, epoxy 2.0-3.5
Viscose material 5-7.5
Pitch 9-12
Film coalescence aid 2.5-4.5
Asbestos powder 4.5-7.5
Barium sulfate 5-8
Silicon-dioxide 0.5-3.0.
2, resin rubber anti-corrosive and waterproof paint according to claim 1 is characterized in that pressing column weight amount per-cent by following composition forms:
A, anti-corrosive type:
Mixed solvent 47.4
Deposed polystyrene 13.0
Resins, epoxy 8.6
Viscose material 8.8
Film coalescence aid 7.4
Pigment 7.8
Zinc oxide 1.1
Talcum powder 3.1
Mica powder 2.1
Mishmetal siccative 0.7
B, waterproof type:
Mixed solvent 47.4
Deposed polystyrene 13.0
Resins, epoxy 3.0
Viscose material 7.0
Pitch 10.6
Film coalescence aid 4.0
Asbestos powder 6.0
Barium sulfate 7.0
Silicon-dioxide 2.0
3, resin rubber anti-corrosive and waterproof paint according to claim 1 is characterized in that pressing column weight amount per-cent by following composition forms:
A, mixed solvent 47.4
Deposed polystyrene 13.0
Resins, epoxy 8.2
Viscose material 8.6
Film coalescence aid 7.5
Pigment 8.1
Zinc oxide 1.2
Talcum powder 3.3
Mica powder 2.0
Mishmetal siccative 0.7
B, waterproof type:
Mixed solvent 47.4
Deposed polystyrene 13.0
Resins, epoxy 3.1
Viscose material 7.2
Pitch 10.2
Film coalescence aid 4.0
Asbestos powder 6.3
Barium sulfate 7.0
Silica 1 .8
CN94111417A 1994-08-18 1994-08-18 Resin rubber anti-corrosive and waterproof paint Expired - Fee Related CN1056397C (en)