Thermanit 22/09

Solid wire, high-alloyed, stainless

Classifications
EN ISO 14343-A EN ISO 14343-B AWS A5.9 Mat. No.
G 22 9 3 N L SS2209 ER2209 ≈1.4462
Characteristics and typical fields of application
Duplex stainless steel; resistant to intercrystalline corrosion and wet corrosion up to 250 °C
(482 °F). Good resistance to stress corrosion cracking in chlorine- and hydrogen sulphide-bearing
environment. High Cr- and Mo-contents provide resistance to pitting corrosion. For joining and
surfacing work with matching and similar austenitc steels / cast steel grades. Attention must be
paidto embrittlement susceptibility of the parent metal.

Base materials
TÜV-certified duplex stainless steels 1.4462 – X2CrNiMoN22-5-3 and others, also combinations of
aforementioned steels and ferritic steels up to
S355J, 16Mo3 and 1.4583 – X10CrNiMoNb18-12 – UNS S31803, S32205

Typical analysis of solid wire (wt.-%)


C Si Mn Cr Mo Ni N
wt-% 0.025 0.5 1.6 23.0 3.0 9.0 0.14
Structure: Austenite/Ferrite
Mechanical properties of all-weld metal
Heat- Yield strength Yield strength Tensile strength Elongation Impact work
treatment R p0.2 R p1.0 Rm A (L 0 =5d 0 ) ISO-V KV J
MPa MPa MPa % +20 °C
aw 510 550 700 25 70
Operating data
Polarity: Shielding gas: ø (mm) Spool:
DC ( + ) (EN ISO 14175) M12, M13 0.8 BS300
1.0 B300
1.2 B300
Welding instruction
Materials Preheating Postweld heat treatment
Matching / similar steels / None Mostly none; if necessary solution
cast steel grades annealing at 1050 °C (1922 °F)/ water
Approvals
TÜV (03342), DB (43.132.36) DNV, GL, CE

All information provided is based upon careful investigation and intensive research. 05/2014
However, we do not assume any liability for correctness and information is subject to change without notice. www.voestalpine.com/welding

You might also like