JPH10188345A - Optical recording medium - Google Patents
Optical recording mediumInfo
- Publication number
- JPH10188345A JPH10188345A JP34189696A JP34189696A JPH10188345A JP H10188345 A JPH10188345 A JP H10188345A JP 34189696 A JP34189696 A JP 34189696A JP 34189696 A JP34189696 A JP 34189696A JP H10188345 A JPH10188345 A JP H10188345A
- Authority
- JP
- Japan
- Prior art keywords
- parts
- weight
- protective layer
- recording medium
- optical recording
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【0001】[0001]
【発明の属する技術分野】本発明は、光記録媒体、特に
表面に筆記用具やインクジェットプリンターや昇華型プ
リンターで書き込みができる光記録媒体に関する。BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to an optical recording medium, and more particularly to an optical recording medium whose surface can be written with a writing instrument, an ink jet printer or a sublimation printer.
【0002】[0002]
【従来の技術】現在広く一般に普及しているコンパクト
ディスク(CD)やレーザーディスク(LD)のような
再生専用型の光記録媒体は、通常スタンパと呼ばれる原
盤を基にして射出成形法によって情報を持つ基板を製造
する。この方法では、同じ情報を持つ媒体を安価にかつ
大量に製造することは可能であるが、スタンパが非常に
高価なため少量の媒体を作成するには向いていない。ま
た、近年の情報化社会の進展に伴い、磁気記録媒体より
も高密度記録が切望されてきた。そこで少量の情報記録
媒体を作成するため、あるいは利用者が自由にデータを
記録、保存を行なうための光記録媒体が開発されてきて
いる。2. Description of the Related Art A read-only optical recording medium such as a compact disk (CD) or a laser disk (LD), which has been widely and widely used at present, stores information by an injection molding method based on a master usually called a stamper. To manufacture substrates with According to this method, it is possible to produce a medium having the same information at low cost and in large quantities, but it is not suitable for producing a small amount of a medium because the stamper is very expensive. Further, with the progress of the information society in recent years, there has been a growing demand for higher density recording than magnetic recording media. Therefore, an optical recording medium has been developed for creating a small amount of information recording medium or for allowing a user to freely record and store data.
【0003】光記録媒体には、情報の記録及び再生が可
能な追記型と、記録後データの消去が可能な書換型の二
種類に分けられる。その中で、単板構造の追記型コンパ
クトディスクはCD−Rと呼ばれ、通常の再生専用CD
と互換性をもつことから徐々に利用者が増えてきてい
る。このCD−Rはデータの入っていない媒体を購入し
たのち利用者がデータを書き込むために、媒体にどんな
情報が記録されているか何らかの方法でわかるようにし
なければならない。[0003] Optical recording media are classified into two types: a write-once type, in which information can be recorded and reproduced, and a rewritable type, in which data can be erased after recording. Among them, a single-recordable write-once compact disc is called a CD-R, which is a normal read-only CD.
Users are gradually increasing because of compatibility with. After the CD-R has been purchased, it is necessary for the user to know what information is recorded on the medium in some way so that the user can write the data after purchasing the medium.
【0004】一般にタイトル等を表示する方法には、油
性フェルトペンで表面に手で書く方法がとられるが、C
D−Rにデータを入れたのちに末端ユーザーに媒体を販
売する場合には手書きは好まれない。一方、プロッピー
ディスクのような紙やフィルムのラベルを貼る方法はプ
リンターできれいにデザインされた文字や絵をプリント
できる利点があるが、ディスク全面に文字を入れたい場
合、大きな面積のドーナツ型のラベルを用いる必要があ
り、位置を合わせて貼るのは非常に難しい。また、剥が
れかかった場合、装置内で剥離しひっかかる恐れがある
ため、他の方法が望まれてきた。In general, a method of displaying a title or the like is a method of manually writing on a surface with an oil-based felt pen.
Handwriting is not preferred when selling media to end users after data has been entered into the DR. On the other hand, a method of attaching a paper or film label such as a proppy disc has the advantage of printing well-designed characters and pictures on a printer, but if you want to put letters on the entire surface of the disc, a large area donut-shaped label And it is very difficult to stick them together. In addition, when the film is peeled, there is a possibility that the film may be peeled and caught in the apparatus, and thus another method has been desired.
【0005】[0005]
【発明が解決しようとする課題】これらの用途から、媒
体の光入射面と反対側に親水性のコート層を施し、イン
クジェットプリンター等を用いて記録内容等をプリント
する方法が実用化され、これに対応した特殊な表面を有
するCD−R媒体が市販されている。From these uses, a method of printing a recorded content using an ink jet printer or the like by applying a hydrophilic coating layer on the side opposite to the light incident surface of the medium has been put into practical use. A CD-R medium having a special surface corresponding to is available on the market.
【0006】しかし、インクジェットプリンター等によ
り記録内容等をプリントした場合、プリント部がにじん
だり、はじいたりして解像度が十分でなくプリントされ
るという問題があった。本発明は、このような問題を解
消する光記録媒体、及びこれに適したインクを提供する
ことを目的とするものである。However, when recording contents and the like are printed by an ink-jet printer or the like, there is a problem that the print portion is blurred or repelled, resulting in insufficient resolution and printing. An object of the present invention is to provide an optical recording medium that solves such a problem and an ink suitable for the medium.
【0007】[0007]
【課題を解決するための手段】本発明者らは、上記問題
点に鑑み、鋭意検討を行なった結果、記録層、金属反射
層、2層以上の保護層を順次積層してなる光記録媒体に
おいて、表面に露出している保護層を、親水性ポリマー
及び親水性モノマー及び共重合可能モノマー及びラジカ
ル開始剤からなる硬化性組成物に、さらにカチオンモノ
マーを添加し、これとフィラーとの混練物をUV硬化せ
しめて得られたものとすることにより、上記問題が解決
できることを見いだし、本発明に至った。Means for Solving the Problems In view of the above problems, the present inventors have conducted intensive studies and as a result, have found that an optical recording medium comprising a recording layer, a metal reflective layer, and two or more protective layers sequentially laminated. In, the protective layer exposed on the surface, a curable composition comprising a hydrophilic polymer and a hydrophilic monomer and a copolymerizable monomer and a radical initiator, a cationic monomer is further added, kneaded product of this and a filler Was found to be able to solve the above problem by being obtained by UV curing, and the present invention was achieved.
【0008】すなわち、本発明は (1) 透明基板上に記録層、金属反射層、2層以上の保護
層を順次積層してなる光記録媒体において、表面に露出
している保護層が、親水性ポリマー、親水性モノマー、
カチオンモノマー、共重合可能なモノマー及びラジカル
開始剤からなる硬化性組成物とフィラーとの混練物をU
V硬化せしめて得られたものからなり、該保護層表面を
プリンタブルに構成することを特徴とする光記録媒体で
あり、また、(2) 表面に露出しているUV硬化樹脂から
なる保護層が、a)親水性ポリマー1〜80重量部、b)
親水性モノマー20〜88重量部、c)カチオンモノマー10
〜70重量部、d)共重合可能モノマー1〜40重量部、及
びe)ラジカル開始剤 0.1〜10重量部からなる硬化性組
成物とフィラーとの混練物をUV硬化せしめて得られた
ものからなり、該保護層表面をプリンタブルに構成する
ことを特徴とする上記(1)に記載の光記録媒体であり、
また、 (3) 前記の表面に露出しているUV硬化樹脂からなる保
護層が、a)親水性ポリマー10〜70重量部、b)親水性
モノマー20〜78重量部、c)カチオンモノマー10〜50重
量部、d)共重合可能モノマー1〜20重量部、及びe)
ラジカル開始剤1〜8重量部からなる硬化性組成物とフ
ィラーとの混練物をUV硬化せしめて得られたものから
なり、該保護層表面をプリンタブルに構成することを特
徴とする上記(1) に記載の光記録媒体であり、また、 (4) カチオンモノマーがアミド基及び/又はアミノ基を
有することを特徴とする上記 (1)〜(3) のいずれかに記
載の光記録媒体であり、また、 (5) 表面に露出しているUV硬化樹脂からなる保護層に
含まれるフィラーが、吸水性及び/又は吸油性を有する
有機フィラー及び/又は無機フィラーを含有するUV硬
化樹脂からなり、フィラーの合計量が表面に露出してい
るUV硬化樹脂 100重量部に対し、1〜80重量部である
ことを特徴とする上記 (1)〜(4) のいずれかに記載の光
記録媒体であり、また、 (6) 表面に露出しているUV硬化樹脂からなる保護層に
含まれるフィラーが吸水性及び/又は吸油性を有する有
機フィラー及び/又は無機フィラーを含有するUV硬化
樹脂からなり、フィラーの合計量が表面に露出している
UV硬化樹脂 100重量部に対し、5〜50重量部であるこ
とを特徴とする上記(5) に記載の光記録媒体であり、ま
た、 (7) 記録層が有機色素からなる上記 (1)〜(6) のいずれ
かに記載の光記録媒体であり、また、 (8) 表面に露出している保護層に水性又は油性インクで
プリントを施した上記 (1)〜(7) のいずれかに記載の光
記録媒体であり、また、 (9) 吸水性及び/又は吸油性を有する有機フィラー及び
/又は無機フィラーと、上記 (2)〜(6) のいずれかに記
載のUV硬化性組成物からなるプリンタブルな保護層を
形成するに適したUV硬化型インクである。That is, the present invention provides (1) an optical recording medium comprising a recording layer, a metal reflection layer, and two or more protective layers sequentially laminated on a transparent substrate, wherein the protective layer exposed on the surface is hydrophilic. Polymer, hydrophilic monomer,
A kneaded product of a curable composition comprising a cationic monomer, a copolymerizable monomer and a radical initiator and a filler is prepared by
V. An optical recording medium comprising a material obtained by curing and having the surface of the protective layer printable, and (2) a protective layer made of a UV-curable resin exposed on the surface. , A) 1 to 80 parts by weight of a hydrophilic polymer, b)
20 to 88 parts by weight of hydrophilic monomer, c) cationic monomer 10
To 70 parts by weight, d) 1 to 40 parts by weight of a copolymerizable monomer and e) 0.1 to 10 parts by weight of a radical initiator. Wherein the optical recording medium according to the above (1), wherein the protective layer surface is configured to be printable,
(3) The protective layer made of a UV-curable resin exposed on the surface comprises: a) 10 to 70 parts by weight of a hydrophilic polymer, b) 20 to 78 parts by weight of a hydrophilic monomer, c) 10 to 70 parts by weight of a cationic monomer. 50 parts by weight, d) 1 to 20 parts by weight of a copolymerizable monomer, and e)
The kneaded product of a curable composition comprising 1 to 8 parts by weight of a radical initiator and a filler is obtained by UV-curing, and the surface of the protective layer is configured to be printable (1). (4) The optical recording medium according to any one of the above (1) to (3), wherein the cationic monomer has an amide group and / or an amino group. And (5) the filler contained in the protective layer made of a UV curable resin exposed on the surface is made of a UV curable resin containing an organic filler and / or an inorganic filler having water absorbency and / or oil absorbency, The optical recording medium according to any one of (1) to (4), wherein the total amount of the filler is 1 to 80 parts by weight with respect to 100 parts by weight of the UV curable resin exposed on the surface. Yes, and (6) UV hard exposed on the surface The UV curable resin in which the filler contained in the protective layer made of a resin is a UV curable resin containing an organic filler and / or an inorganic filler having water absorbency and / or oil absorbency, and the total amount of the filler is exposed on the surface. The optical recording medium according to the above (5), which is 5 to 50 parts by weight relative to parts by weight, and (7) the above (1) to (6), wherein the recording layer is made of an organic dye. (8) The optical recording medium according to any one of (1) to (7) above, wherein the protective layer exposed on the surface is printed with an aqueous or oil-based ink. A printable medium comprising: (9) an organic filler and / or an inorganic filler having a water absorbing property and / or an oil absorbing property; and the UV-curable composition according to any one of the above (2) to (6). UV curable ink suitable for forming a simple protective layer.
【0009】[0009]
【発明の実施の形態】本発明において用いられるの光記
録媒体の構成は、透明基板、記録層、金属反射層、2層
以上の保護層からなり、特性を向上させるために下地層
やさらに保護層を積層させてもよい。DESCRIPTION OF THE PREFERRED EMBODIMENTS The construction of an optical recording medium used in the present invention comprises a transparent substrate, a recording layer, a metal reflective layer, and two or more protective layers. Layers may be stacked.
【0010】本発明において用いられる基板は光によっ
て再生記録を行なうため、透明ならばいかなる材質でも
使用できる。例えばポリカーボネート樹脂、アクリル樹
脂、ポリスチレン樹脂、塩化ビニル樹脂、エポキシ樹
脂、ポリエステル樹脂、ポリオレフィン等の高分子材
料、ガラスなどの無機材料等が例示できるが、これらに
限定されるものではない。これらの中で、基板の機械的
強度、グルーブや再生専用信号などの付与のしやすさ、
及び経済性等の点からポリカーボネート樹脂、アクリル
樹脂、ポリオレフィン樹脂を用いるのが望ましく、特に
ポリカーボネート樹脂がより望ましい。Since the substrate used in the present invention performs reproduction and recording by light, any transparent material can be used. Examples thereof include, but are not limited to, polycarbonate resin, acrylic resin, polystyrene resin, vinyl chloride resin, epoxy resin, polyester resin, polymer materials such as polyolefin, and inorganic materials such as glass. Among these, the mechanical strength of the substrate, the ease of providing grooves and read-only signals, etc.,
It is preferable to use a polycarbonate resin, an acrylic resin, or a polyolefin resin from the viewpoint of economy and economical efficiency, and more preferable is a polycarbonate resin.
【0011】これらの基板の形状は板状でもフィルム状
でもよく、また、円形やカード状でもよい。また、これ
らの基板表面には記録位置を表す案内溝やピット、一部
再生専用の情報等のためのピットを有していてもよい。
これらの溝やピット等は、通常スタンパを用い、公知の
方法にて形成される。The shape of these substrates may be plate-like or film-like, and may be circular or card-like. Further, these substrate surfaces may have guide grooves and pits indicating recording positions, and pits for partially read-only information.
These grooves and pits are usually formed by a known method using a stamper.
【0012】本発明に用いられる記録層は、シアニン
系、フタロシアニン系、アゾ系などの有機色素を用いる
のが一般的である。これらの色素は溶剤に対する溶解性
のためや記録特性等のために各種の置換基で置換されて
いてもよい。また、これらの色素は1種類又は2種類以
上を混合して用いることもできる。The recording layer used in the present invention generally uses an organic dye such as a cyanine-based, phthalocyanine-based, or azo-based dye. These dyes may be substituted with various substituents for solubility in a solvent or recording characteristics. These dyes may be used alone or in combination of two or more.
【0013】前記した色素を含有する記録層は通常スピ
ンコート、スプレーコート、ディップコート等の塗布方
法によって成膜することができる。上記色素を塗布法に
より成膜する際は樹脂基板にダメージを与えない溶剤、
すなわち基板用樹脂を実質的に溶解しない溶剤に色素を
溶解して塗布すればよい。The recording layer containing the dye described above can be generally formed by a coating method such as spin coating, spray coating or dip coating. Solvent that does not damage the resin substrate when forming the above dye by coating method,
That is, the dye may be dissolved in a solvent that does not substantially dissolve the resin for the substrate and then applied.
【0014】本発明において記録層の膜厚は通常50〜20
0 nmが好ましい。色素を含有する記録層を成膜する際
には前記した色素の他にニトロセルロース、エチルセル
ロース、アクリル樹脂、ポリスチレン樹脂、ウレタン樹
脂等の樹脂やレベリング剤、消泡剤等を本発明の効果を
損なわない範囲において併用することもできる。記録層
としては、主に有機色素を含有するものについて記述し
ているが、本発明は無機物やポリマーあるいは金属を記
録層として用いた媒体についても適用できることは明か
である。In the present invention, the thickness of the recording layer is usually 50 to 20.
0 nm is preferred. When forming a recording layer containing a dye, in addition to the above-described dye, nitrocellulose, ethyl cellulose, acrylic resin, polystyrene resin, a resin such as a urethane resin, a leveling agent, an antifoaming agent, etc. impair the effects of the present invention. It can also be used together in a range that does not exist. Although a recording layer mainly containing an organic dye is described, it is apparent that the present invention can be applied to a medium using an inorganic substance, a polymer, or a metal as the recording layer.
【0015】本発明における記録層の上に設けられた反
射層としては、金、銀、アルミニウムあるいはこれらの
合金のような高反射率の金属膜が用いられる。これらの
金属の反射層は蒸着、スパッタ等の方法で成膜すること
ができる。また、これらの反射層の膜厚は通常 500〜20
00Å程度が好ましい。反射層は多層積層することも可能
である。As the reflective layer provided on the recording layer in the present invention, a metal film having a high reflectivity such as gold, silver, aluminum or an alloy thereof is used. These metal reflective layers can be formed by a method such as vapor deposition or sputtering. The thickness of these reflective layers is usually 500 to 20.
It is preferably about 00 °. The reflective layer can be formed by multilayering.
【0016】上記の反射層上に保護層を設ける。例えば
アクリレート系やメタクリレート系の一般的なラジカル
反応で重合するもの、エポキシ系のように光でカチオン
重合を行なうもの等がある。これらの樹脂は単独で重合
させてもよいしモノマー、オリゴマーを混合させてもよ
い。また、溶剤で希釈して塗布することも可能である。
その中でも作業性の点からUV硬化型が望ましい。保護
層を形成する際、スピンコート、ディップコート、バー
コート、スクリーン印刷等の方法で行われるが、作業性
の面からスピンコート法がとられる場合が多い。これら
の膜厚は1μmから 100μm の膜厚で使われるが、1〜2
0μm が望ましい。A protective layer is provided on the reflective layer. For example, there are those which polymerize by a general radical reaction of acrylate or methacrylate, and those which perform cationic polymerization by light such as epoxy. These resins may be polymerized singly or as a mixture of monomers and oligomers. It is also possible to dilute with a solvent and apply.
Among them, a UV curable type is desirable from the viewpoint of workability. When the protective layer is formed, it is performed by a method such as spin coating, dip coating, bar coating, screen printing, etc. In many cases, the spin coating method is used from the viewpoint of workability. These film thicknesses are used in a thickness of 1 μm to 100 μm.
0 μm is desirable.
【0017】保護層は、1層だけでなく、例えばその耐
スクラッチ性を向上させるために2層以上の保護層を積
層してもよい。また、保護層の上に全面あるいは部分的
にスクリーン印刷等でレーベル等の印刷を行なうことも
可能である。Not only one protective layer but also two or more protective layers may be laminated, for example, to improve the scratch resistance. It is also possible to print a label or the like entirely or partially on the protective layer by screen printing or the like.
【0018】本発明の表面に露出している保護層は、イ
ンクジェットプリンターのインクを十分に吸収、定着さ
せるためのものであり、特には、親水性ポリマー及び親
水性モノマー及びカチオンモノマー及び共重合可能モノ
マー及びラジカル開始剤からなる硬化性組成物とフィラ
ーとの混練物をUV硬化せしめて得られたものからなる
UV硬化樹脂で作成することにより、インクの吸収速度
が増し、良好な吸収、定着性、解像度が得られる。The protective layer exposed on the surface of the present invention is used to sufficiently absorb and fix the ink of an ink jet printer, and particularly, a hydrophilic polymer, a hydrophilic monomer and a cationic monomer, and a copolymerizable polymer. By forming a kneaded product of a curable composition comprising a monomer and a radical initiator and a filler with a UV-curable resin obtained by UV-curing, the ink absorption speed is increased, and good absorption and fixing properties are obtained. , Resolution is obtained.
【0019】前記の表面に露出しているUV硬化樹脂か
らなる保護層に含まれるフィラーとしては吸水性及び/
又は吸油性を有する有機フィラー及び/又は無機フィラ
ーを用いる。The filler contained in the protective layer made of a UV-curable resin exposed on the surface includes water-absorbing and / or
Alternatively, an organic filler and / or an inorganic filler having an oil absorbing property is used.
【0020】有機フィラーの具体例としてはアクリル樹
脂、ポリアクリル酸エステル、ポリメタクリル酸エステ
ル、スチレン樹脂、ポリエステル、ポリカーボネート、
変性メラミン樹脂微粒子、ポリビニルアルコール、ポリ
アクリルアミド、ポリビニルピロリドン、ゴム等の微粒
子、又はこれらポリマーの架橋微粒子、さらにリグニ
ン、プロテイン、セルロースの粉末等が挙げられる。こ
の際油性ペンや水性ペンのインクがはじかないようにす
るため、添加するフィラーは吸水性や吸油性の高いもの
が必要である。この点からはリグニン、プロテイン、セ
ルロースの粉末が好ましい。インクジェットプリンター
のインクのように乾きにくい溶剤を含む場合は特に効果
的である。Specific examples of the organic filler include acrylic resin, polyacrylate, polymethacrylate, styrene resin, polyester, polycarbonate,
Modified melamine resin fine particles, fine particles of polyvinyl alcohol, polyacrylamide, polyvinylpyrrolidone, rubber and the like, cross-linked fine particles of these polymers, and powders of lignin, protein, cellulose and the like are also included. At this time, in order to prevent the ink of the oil-based pen or the water-based pen from repelling, it is necessary that the filler to be added has a high water-absorbing or oil-absorbing property. From this viewpoint, lignin, protein, and cellulose powders are preferred. It is particularly effective when it contains a solvent that does not easily dry, such as ink for an ink jet printer.
【0021】無機フィラーの具体例としては、シリカ、
タルク、クレー、炭酸カルシウム、ケイ酸カルシウム、
硫酸バリウム、マイカ、珪藻土シリカ、水酸化アルミニ
ウム、アルミナ、酸化ジルコニウム、水酸化ジルコニウ
ム等が挙げられる。シリカフィラーは破砕によって製造
された場合、吸水性、又は吸油性が低いため十分な効果
が得られない。しかし細かい一次粒子が集まって二次粒
子を形成している合成シリカ等の場合、その二次粒子の
隙間に油性ペンや水性ペンの溶剤が染み込むため効果的
である。Specific examples of the inorganic filler include silica,
Talc, clay, calcium carbonate, calcium silicate,
Examples include barium sulfate, mica, diatomaceous earth silica, aluminum hydroxide, alumina, zirconium oxide, and zirconium hydroxide. When the silica filler is manufactured by crushing, sufficient effects cannot be obtained due to low water absorption or oil absorption. However, in the case of synthetic silica or the like in which fine primary particles are collected to form secondary particles, it is effective because the solvent of the oil-based pen or the aqueous pen penetrates into the gaps between the secondary particles.
【0022】無機フィラーの場合、吸油量が測定されて
いることが多い。一般的にJIS−K−5101法に準
じ、フィラー 100g当たりに吸収されるアマニ油の量で
表されるが、本発明では5ml/100 g(フィラー量)
以上が望ましく、更には15ml/100 g(フィラー量)
以上がより望ましい。吸水量は一般的な測定方法はない
が、フィラーに水を滴下したときに水滴がフィラーに吸
い込まれるものが望ましい。表面がフッ素処理されてい
るようなフィラーの場合、水滴はフィラーに吸収される
ことなく球状になる。このようなフィラーを用いると油
性でも水性インクでも乾燥せずはじいてしまう。In the case of inorganic fillers, the oil absorption is often measured. Generally, it is represented by the amount of linseed oil absorbed per 100 g of filler according to the JIS-K-5101 method. In the present invention, it is 5 ml / 100 g (filler amount).
The above is desirable, and furthermore, 15 ml / 100 g (filler amount)
The above is more desirable. Although there is no general method for measuring the amount of water absorption, it is preferable that the amount of water absorbed into the filler when water is dropped on the filler is used. In the case of a filler whose surface is treated with fluorine, water droplets become spherical without being absorbed by the filler. If such a filler is used, both oily and water-based inks repel without drying.
【0023】有機フィラーや無機フィラーは単独で用い
ることもできるが、書き込み後の乾燥性の改善、インク
の粘度調整、又は色調改良のために併用することが可能
である。この際混合する比率はその目的によっていろい
ろ変えることが可能である。The organic filler and the inorganic filler can be used alone, but can be used together for improving the drying property after writing, adjusting the viscosity of the ink, or improving the color tone. At this time, the mixing ratio can be variously changed depending on the purpose.
【0024】なお、インクの粘度調整のためにアエロジ
ルのように増粘作用のあるフィラーを添加してもよい。
また、その他目的に応じ各種添加剤を用いることができ
る。印刷時のレベリング剤や消泡剤、脱泡剤、増粘剤、
タレ止め剤、沈降防止剤、顔料分散助剤、湿潤剤や分散
助剤等が挙げられる。Incidentally, a filler having a thickening action such as Aerosil may be added for adjusting the viscosity of the ink.
Various additives can be used according to other purposes. Leveling agent, defoamer, defoamer, thickener,
Examples thereof include an anti-sagging agent, an anti-settling agent, a pigment dispersing aid, a wetting agent and a dispersing aid.
【0025】フィラーを含有する樹脂としてはUV硬化
樹脂が好ましい。熱硬化樹脂等の溶剤含有樹脂は、煩雑
な乾燥工程を必要とし、さらに乾燥によって放出された
有機溶剤は作業環境の点で好ましくない。UV硬化樹脂
は通常無溶剤で用いられるが、通常UV硬化樹脂にフィ
ラーを添加する場合粘度上昇のため添加量が限られてい
まう。そのためにインクの乾燥速度が遅くなり本目的に
は好ましくない。この樹脂層の特性をさらに向上させる
ためには樹脂層をさらに工夫することが好ましい。すな
わちこの樹脂層には1種類又は2種類以上の親水性ポリ
マーと1種類又は2種類以上の親水性モノマーと1種類
又は2種類以上の架橋性モノマー1種類又は2種類以上
のカチオンモノマーとラジカル開始剤を含有するUV硬
化樹脂を用いる。As the resin containing the filler, a UV curable resin is preferable. Solvent-containing resins such as thermosetting resins require a complicated drying step, and organic solvents released by drying are not preferable in terms of working environment. The UV-curable resin is usually used without a solvent, but when a filler is added to the UV-curable resin, the amount of addition is limited due to an increase in viscosity. Therefore, the drying speed of the ink becomes slow, which is not preferable for this purpose. In order to further improve the characteristics of the resin layer, it is preferable to further devise the resin layer. That is, this resin layer has one or more hydrophilic polymers, one or more hydrophilic monomers, one or more crosslinkable monomers, one or more cationic monomers, and a radical initiator. UV curable resin containing an agent is used.
【0026】表面に露出している層に親水性ポリマーを
加えることにより表面に付着したインクを定着しやすく
する。親水性ポリマーにはポリビニルアルコール、ヒド
ロキシエチルセルロース、ヒドロキシプロピルセルロー
ス、ポリアクリルアミド、ポリビニルピロリドン、ポリ
エチレンオキサイド等のホモポリマー及びコポリマーが
ある。コポリマーの場合は親水性ポリマーでないものと
の組み合わせでもよい。これは1種類加えてもよいし2
種類以上組み合わせて用いてもよい。多く入れれば入れ
るほどペンやプリンターのインクの定着がよくなるが、
樹脂粘度が高くて成膜できなくなったりポリマーが析出
してしまうため樹脂組成のうち親水性ポリマーの総量が
1〜80重量部になるように加える。望ましくは10〜
70重量部にするのがよい。The addition of the hydrophilic polymer to the layer exposed on the surface facilitates fixing of the ink adhered to the surface. The hydrophilic polymer includes homopolymers and copolymers such as polyvinyl alcohol, hydroxyethyl cellulose, hydroxypropyl cellulose, polyacrylamide, polyvinyl pyrrolidone, and polyethylene oxide. In the case of a copolymer, a combination with a non-hydrophilic polymer may be used. This may be added one kind, 2
You may use in combination of types or more. The more you add, the better the ink of the pen and printer will be fixed,
Since the viscosity of the resin is so high that a film cannot be formed or the polymer is precipitated, the total amount of the hydrophilic polymer in the resin composition is 1 to 80 parts by weight. Desirably 10
It is good to use 70 parts by weight.
【0027】本発明においては前記親水性ポリマーは極
性の高い親水性モノマーに溶解する。親水性モノマーと
してはヒドロキシ(メタ)アクリレートやヒドロキシプ
ロピル(メタ)アクリレート、ヒドロキシブチル(メ
タ)アクリレート、ヒドロキシペンチル(メタ)アクリ
レート、フェノキシヒドロキシプロピル(メタ)アクリ
レート、クロロヒドロキシプロピル(メタ)アクリレー
ト、ジエチレングリコールモノ(メタ)アクリレート、
トリエチレングリコールモノ(メタ)アクリレート、ポ
リエチレングリコールモノ(メタ)アクリレート、ジプ
ロピレングリコールモノ(メタ)アクリレート、ポリプ
ロピレングリコールモノ(メタ)アクリレート、グリセ
リンモノ(メタ)アクリレート、グリセリンジ(メタ)
アクリレート、ペンタエリスリトールトリ(メタ)アク
リレート、フェニルグリシジルエーテル(メタ)アクリ
レート、ジペンタエリスリトールペンタ(メタ)アクリ
レート、ビスフェノールAエポキシ樹脂のジ(メタ)ア
クリレートのように分子内にOH基を有するもの、また
ジメチル(メタ)アクリルアミドやジエチル(メタ)ア
クリルアミド、アクロイルモルホリン、N−ビニルピロ
リドン、2−エトキシエチル(メタ)アクリレート、2
−メトキシエチル(メタ)アクリレート、エチルカルビ
トール(メタ)アクリレート、グリシジル(メタ)アク
リレートのような極性の高いものが用いられる。単官能
でもよいし2官能以上のモノマーでもよい。In the present invention, the hydrophilic polymer is dissolved in a highly polar hydrophilic monomer. Hydrophilic monomers include hydroxy (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate, hydroxypentyl (meth) acrylate, phenoxyhydroxypropyl (meth) acrylate, chlorohydroxypropyl (meth) acrylate, diethylene glycol mono (Meth) acrylate,
Triethylene glycol mono (meth) acrylate, polyethylene glycol mono (meth) acrylate, dipropylene glycol mono (meth) acrylate, polypropylene glycol mono (meth) acrylate, glycerin mono (meth) acrylate, glycerin di (meth)
Acrylate, pentaerythritol tri (meth) acrylate, phenylglycidyl ether (meth) acrylate, dipentaerythritol penta (meth) acrylate, bisphenol A epoxy resin di (meth) acrylate having an OH group in the molecule, Dimethyl (meth) acrylamide, diethyl (meth) acrylamide, acroylmorpholine, N-vinylpyrrolidone, 2-ethoxyethyl (meth) acrylate,
-Highly polar substances such as methoxyethyl (meth) acrylate, ethyl carbitol (meth) acrylate, and glycidyl (meth) acrylate are used. It may be monofunctional or a difunctional or higher functional monomer.
【0028】これらのモノマーは溶剤のように親水性ポ
リマーを均一に溶解し、さらに有機溶剤や水を多く含ん
だペンやインクジェットプリンターで樹脂層に文字を書
き込んだ場合、にじみやはじきを抑える。特に親水性の
高いポリマーを用いた場合は分子内に水酸基やカルボキ
シル基、アミノ基、アミド基等の極性の高い基を有する
モノマーを用いると親水性ポリマーが溶解し易い。親水
性ポリマーの溶解性を向上させるために水、メタノー
ル、エタノール、プロパノール、ブタノール、ペンタノ
ール、ヘキサノール等のアルコール類、ジメチルエーテ
ル、ジエチルエーテル、メチルエチルエーテル、ジプロ
ピルエーテル等のエーテル類、アセトン、シクロヘキサ
ン等のケトン類、ジクロロエタン、クロロホルム等のハ
ロゲン系等の溶媒を一部使用してもよい。樹脂組成のう
ち親水性モノマーの総量は20〜88重量部加える。望まし
くは20〜78重量部加える。These monomers uniformly dissolve a hydrophilic polymer like a solvent, and when characters are written on a resin layer with a pen or an ink jet printer containing a large amount of an organic solvent or water, bleeding and bleeding are suppressed. In particular, when a polymer having high hydrophilicity is used, the hydrophilic polymer is easily dissolved when a monomer having a highly polar group such as a hydroxyl group, a carboxyl group, an amino group, or an amide group in the molecule is used. In order to improve the solubility of the hydrophilic polymer, water, alcohols such as methanol, ethanol, propanol, butanol, pentanol and hexanol, ethers such as dimethyl ether, diethyl ether, methyl ethyl ether and dipropyl ether, acetone and cyclohexane And some solvents such as ketones such as dichloroethane and halogen such as chloroform. The total amount of the hydrophilic monomer in the resin composition is 20 to 88 parts by weight. Preferably, 20 to 78 parts by weight are added.
【0029】本発明においては、表面に露出している層
にカチオンモノマーを加えることにより、表面に露出し
ている層表面に有機溶剤や水を多く含んだペンやインク
ジェットプリンターで文字等を書き込んだ場合、にじみ
やはじきがさらに抑えられるとともに解像度も大幅に向
上させることができる。特に分子内にアミノ基、アミド
基等の基を有するカチオンモノマーが効果的である。In the present invention, by adding a cationic monomer to the layer exposed on the surface, characters or the like are written on the surface of the layer exposed on the surface with a pen or an ink jet printer containing a large amount of an organic solvent or water. In this case, bleeding and bleeding can be further suppressed, and the resolution can be significantly improved. Particularly, a cationic monomer having a group such as an amino group or an amide group in the molecule is effective.
【0030】アミノ基、アミド基を有するカチオンモノ
マーとしては、ジメチル(メタ)アクリルアミドやジエ
チル(メタ)アクリルアミド、ジメチルアミノメチル
(メタ)アクリレート、ジメチルアミノメチル(メタ)
アクリレート4級塩、ジメチルアミノエチル(メタ)ア
クリレート、ジメチルアミノエチル(メタ)アクリレー
ト4級塩、ジエチルアミノメチル(メタ)アクリレー
ト、ジエチルアミノメチル(メタ)アクリレート4級
塩、ジエチルアミノエチル(メタ)アクリレート、ジエ
チルアミノエチル(メタ)アクリレート4級塩、メチレ
ンビス(メタ)アクリレート、アクリロイルモルホリ
ン、N−ビニルピロリドン等が用いられる。前記親水性
モノマーの一部に含まれるカチオンモノマーの総量は10
〜70重量部になるように加える。望ましくは10〜50重量
部にするのがよい。Examples of the cationic monomer having an amino group or an amide group include dimethyl (meth) acrylamide, diethyl (meth) acrylamide, dimethylaminomethyl (meth) acrylate, and dimethylaminomethyl (meth).
Acrylate quaternary salt, dimethylaminoethyl (meth) acrylate, dimethylaminoethyl (meth) acrylate quaternary salt, diethylaminomethyl (meth) acrylate, diethylaminomethyl (meth) acrylate quaternary salt, diethylaminoethyl (meth) acrylate, diethylaminoethyl (Meth) acrylate quaternary salts, methylenebis (meth) acrylate, acryloylmorpholine, N-vinylpyrrolidone and the like are used. The total amount of the cationic monomer contained in a part of the hydrophilic monomer is 10
Add to ~ 70 parts by weight. Preferably, the amount is 10 to 50 parts by weight.
【0031】これらに架橋性モノマーを加える。これら
にはトリメチロールプロパントリ(メタ)アクリレー
ト、アクリル化イソシアヌレート、1,4ブタンジオー
ルジ(メタ)アクリレート、1,6ヘキサンジオールジ
(メタ)アクリレート、ネオペンチルグリコールジ(メ
タ)アクリレート、ジシクロペンタジエニルジ(メタ)
アクリレート、ペンタエリスリトールテトラ(メタ)ア
クリレート等が使われる。なお、上記の親水性モノマー
がグリセリンジ(メタ)アクリレートやペンタエリスリ
トールトリ(メタ)アクリレート、ジペンタエリスリト
ールヘキサ(メタ)アクリレートのように多官能の場合
は必ずしも加える必要がない。架橋性モノマーを加える
ことで表面に露出している保護層の架橋密度が上がり塗
膜硬度が増す。樹脂組成のうち架橋性モノマーの総量は
1〜40重量部加える。望ましくは1〜20重量部加える。To these are added crosslinking monomers. These include trimethylolpropane tri (meth) acrylate, acrylated isocyanurate, 1,4 butanediol di (meth) acrylate, 1,6 hexanediol di (meth) acrylate, neopentyl glycol di (meth) acrylate, dicyclo Pentadienyl di (meth)
Acrylate, pentaerythritol tetra (meth) acrylate and the like are used. In the case where the hydrophilic monomer is polyfunctional such as glycerin di (meth) acrylate, pentaerythritol tri (meth) acrylate, and dipentaerythritol hexa (meth) acrylate, it is not always necessary to add the hydrophilic monomer. By adding the crosslinkable monomer, the crosslink density of the protective layer exposed on the surface is increased, and the coating film hardness is increased. The total amount of the crosslinking monomer in the resin composition is 1 to 40 parts by weight. Preferably, 1 to 20 parts by weight is added.
【0032】UV光で硬化可能な親水性モノマーやカチ
オンモノマー、架橋性モノマーの混合物に親水性ポリマ
ーを添加すると粘度が上昇する。それらの混合物にフィ
ラーを加えればさらに粘度上昇が見られる。そのためモ
ノマーの粘度があまり高いと、フィラー添加後非常に粘
度が上がってしまい塗布できなくなってしまう。本実験
ではUV硬化樹脂にはなるべく粘度の低いものを選ぶ必
要がある。When a hydrophilic polymer is added to a mixture of a hydrophilic monomer, a cationic monomer and a crosslinkable monomer which can be cured by UV light, the viscosity increases. Addition of fillers to these mixtures further increases the viscosity. For this reason, if the viscosity of the monomer is too high, the viscosity becomes very high after the addition of the filler, and the application becomes impossible. In this experiment, it is necessary to select a UV-curable resin having as low a viscosity as possible.
【0033】これらにラジカル開始剤を加える。ラジカ
ル開始剤としては1−ヒドロキシシクロヘキシルフェニ
ルケトンや2−ヒドロキシ−2−メチル−1−フェニル
プロパン−1−オン、2,2−ジエトキシアセトフェノ
ンや4’−フェノキシ−2,2−ジクロロアセトフェノ
ン等のアセトフェノン系、2−ヒドロキシ−2−メチル
プロピオフェノン等のプロピオフェノン系、2−クロロ
アントラキノン等のアントラキノン系、2,4−ジエチ
ルチオキサントン等のチオキサントン系等が挙げられ
る。この際加える量は樹脂分のうち、 0.1〜10重量部混
ぜる。望ましくは1〜8重量部である。この時、光開始
剤は1種類でもよいし2種類以上を組み合わせてもよ
い。To these, a radical initiator is added. Examples of the radical initiator include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2,2-diethoxyacetophenone and 4'-phenoxy-2,2-dichloroacetophenone. Examples include acetophenone type, propiophenone type such as 2-hydroxy-2-methylpropiophenone, anthraquinone type such as 2-chloroanthraquinone, and thioxanthone type such as 2,4-diethylthioxanthone. The amount added at this time is 0.1 to 10 parts by weight of the resin. Preferably, it is 1 to 8 parts by weight. At this time, one photoinitiator may be used, or two or more photoinitiators may be combined.
【0034】フィラーはこの樹脂 100重量部に対して1
〜80重量部添加するが、望ましくは5〜50重量部添加す
る。保存安定性を考えるとディスパー等で均一に撹拌す
るのが望ましい。The filler is used in an amount of 1 to 100 parts by weight of the resin.
8080 parts by weight, preferably 5-50 parts by weight. Considering storage stability, it is desirable to stir uniformly with a disper or the like.
【0035】この表面に露出している層を形成する方法
はバーコート法、ブレードコート法、エアナイフコート
法、ロールコート法、スクリーン印刷法があるが、表面
を凹凸にすることで筆記性をさらに向上させることがで
きるためスクリーン印刷法が特に望ましい。本発明にお
いてはこの樹脂層を形成する際に塗布性を改良するため
にUV硬化樹脂に溶媒を使用することもできる。膜厚1
〜100 μm に設計されるがディスクの反りに対する影響
を考えると1〜20μm が望ましい。なお、反射層上に一
層保護層があればディスク全面に設けても、又は部分的
にこの層を設けてもよい。The method of forming the layer exposed on the surface includes a bar coating method, a blade coating method, an air knife coating method, a roll coating method, and a screen printing method. Screen printing is particularly desirable because it can be improved. In the present invention, a solvent can be used for the UV-curable resin in order to improve the coating property when the resin layer is formed. Film thickness 1
Although it is designed to be about 100 μm, it is preferably 1 to 20 μm in consideration of the influence on the warpage of the disk. If a single protective layer is provided on the reflective layer, the protective layer may be provided on the entire surface of the disk or may be provided partially.
【0036】塗布された樹脂層はUV光で硬化させる
が、UV光をあてて硬化する場合、 150〜2000mJ/c
m2 のエネルギーを与える。好ましくは 250〜1000mJ
/cm 2 あてる。この際、数秒で塗膜が硬化する。硬化
に用いるUVランプは水銀灯、高圧水銀灯、超高圧水銀
灯、メタルハライドランプが望ましい。The applied resin layer is cured by UV light.
When cured by exposure to UV light, 150-2000 mJ / c
mTwoGive energy. Preferably 250-1000mJ
/ Cm TwoDedicate At this time, the coating film hardens in a few seconds. Hardening
UV lamp used for mercury lamp, high pressure mercury lamp, ultra high pressure mercury
Lights and metal halide lamps are desirable.
【0037】文字を書き込んだりプリントしたりする部
分以外にさらに部分的に層を重ねてもよい。例えばそれ
ぞれの媒体で異なるタイトルやナンバーや日付等を書く
ところ以外の部分は共通の社名やマーク、媒体商品名や
中に記録するソフト名等を表記する場合がある。そのよ
うな場合、スクリーン印刷やオフセット印刷等でさらに
何層か重ねてもよい。Layers may be further partially overlapped with portions where characters are written or printed. For example, portions other than where different titles, numbers, dates, and the like are written in each medium may be described with a common company name, mark, medium product name, software name recorded in the medium, and the like. In such a case, several layers may be further stacked by screen printing, offset printing, or the like.
【0038】このように構成された表面に露出している
保護層に書き込む場合、油性ペンや水、水溶性有機溶剤
を含む水性ペン、油性スタンプ、水性スタンプを用いる
ことができる。また、油性、又は水性インクを用いたイ
ンクジェットプリンター、昇華型プリンター、熱転写型
プリンターを使用することもできる。When writing on the protective layer exposed on the surface configured as described above, an oil-based pen, an aqueous pen containing water and a water-soluble organic solvent, an oil-based stamp, and an aqueous stamp can be used. In addition, an ink jet printer, a sublimation printer, or a thermal transfer printer using an oil-based or water-based ink can also be used.
【0039】[0039]
【実施例】以下、実施例により本発明を具体的に説明す
るが、本発明の実施の態様はこれにより限定されるもの
ではない。EXAMPLES The present invention will be described below in more detail with reference to examples, but embodiments of the present invention are not limited thereto.
【0040】実施例1 厚さ 1.2mm、直径 120mmのスパイラル状のグルーブ(深
さ 140nm、幅 0.5μm 、ピッチ 1.6μm )を有する射
出成形ポリカーボネート樹脂基板にフタロシアニン色素
からなる記録層をオクタン溶液を用いたスピンコート法
により成膜した。この記録層の上に反射層として厚さ 1
00nmのAu薄膜をスパッタリングにより成膜した。こ
の上に紫外線硬化樹脂ダイキュアクリアSD−17(大
日本インキ化学工業株式会社製)をスピンコートした
後、紫外線を照射し、6μm の第1保護層を成膜した。
その上にポリビニルピロリドン−酢酸ビニルコポリマー
(7:3、50%エタノール溶液、東京化成株式会社
製)30重量部、2−ヒドロキシプロピルアクリレート30
重量部、ジメチルアクリルアミド25重量部、トリメチロ
ールプロパントリアクリレート15重量部、ラジカル開始
剤ダロキュア1173を5重量部を混ぜ合わせた樹脂 1
00重量部に対し、合成シリカのTOKUSIL GU
(徳山曹達株式会社製)を20重量部混ぜ、ディスパーで
混練した。それをスクリーン印刷を行なったのち、紫外
線を照射して硬化し、20μm の親水性表面層を形成して
CD−R媒体とした。この親水性表面層にインクジェッ
トプリンターで文字を直接この樹脂層にプリントしたと
ころ、プリント部がにじんだり、はじいたりすることな
く、十分な解像度が得られた。EXAMPLE 1 A recording layer made of a phthalocyanine dye was applied to an injection molded polycarbonate resin substrate having a spiral groove (depth 140 nm, width 0.5 μm, pitch 1.6 μm) having a thickness of 1.2 mm and a diameter of 120 mm by using an octane solution. A film was formed by spin coating. Thickness 1 as a reflective layer on this recording layer
An Au thin film of 00 nm was formed by sputtering. After spin-coating an ultraviolet-curable resin, Die Cure Clear SD-17 (manufactured by Dainippon Ink and Chemicals, Inc.), the film was irradiated with ultraviolet rays to form a 6 μm-thick first protective layer.
30 parts by weight of polyvinylpyrrolidone-vinyl acetate copolymer (7: 3, 50% ethanol solution, manufactured by Tokyo Chemical Industry Co., Ltd.), 2-hydroxypropyl acrylate 30
1 part by weight, 25 parts by weight of dimethylacrylamide, 15 parts by weight of trimethylolpropane triacrylate, and 5 parts by weight of Darocur 1173, a radical initiator.
00 parts by weight of synthetic silica TOKUSIL GU
20 parts by weight (manufactured by Tokuyama Soda Co., Ltd.) were mixed and kneaded with a disper. After screen printing, it was cured by irradiating ultraviolet rays to form a 20 μm hydrophilic surface layer to obtain a CD-R medium. When characters were directly printed on this resin layer by an ink jet printer on the hydrophilic surface layer, a sufficient resolution was obtained without the printed portion bleeding or bleeding.
【0041】実施例2 実施例1のように記録層、反射層を形成後、さらにこの
反射層上に紫外線硬化樹脂ダイキュアクリアSD−17
(大日本インキ化学工業株式会社製)をスピンコート
後、紫外線を照射し、6μm の第1保護層を成膜した。
その上にウレタンアクリレートオリゴマー20重量部、ヒ
ドロキシエチルアクリレート40重量部、メチレンビスア
クリルアミド20重量部、1,4−ブタンジオールジアク
リレート15重量部、ラジカル開始剤ダロキュア1173
を5重量部を混ぜ合わせた樹脂 100重量部に対し、プロ
テインを主成分とする有機フィラー(平均粒径10μm )
を10重量部混ぜ、ディスパーで混練した。それをスクリ
ーン印刷を行なったのち、紫外線を照射して硬化し、15
μm の親水性表面層を形成してCD−R媒体とした。こ
の親水性表面層にインクジェットプリンターで文字を直
接この樹脂層にプリントしたところ、プリント部がにじ
んだり、はじいたりすることなく、十分な解像度が得ら
れた。Example 2 After forming a recording layer and a reflective layer as in Example 1, an ultraviolet-curable resin Die Cure Clear SD-17 was further formed on this reflective layer.
(Dai Nippon Ink Chemical Industry Co., Ltd.) was spin-coated and irradiated with ultraviolet light to form a 6 μm-thick first protective layer.
20 parts by weight of a urethane acrylate oligomer, 40 parts by weight of hydroxyethyl acrylate, 20 parts by weight of methylenebisacrylamide, 15 parts by weight of 1,4-butanediol diacrylate, and a radical initiator Darocure 1173
To 5 parts by weight of resin and 100 parts by weight of organic filler containing protein as the main component (average particle size 10 μm)
Was mixed with 10 parts by weight and kneaded with a disper. After screen-printing it, it is cured by irradiating ultraviolet rays,
A CD-R medium was formed by forming a hydrophilic surface layer of μm. When characters were directly printed on this resin layer by an ink jet printer on this hydrophilic surface layer, a sufficient resolution was obtained without the printed portion bleeding or bleeding.
【0042】比較例1 実施例1において、ジメチルアクリルアミドを削除した
以外は、実施例1と同様にしてCD−R媒体を作成し
た。この親水性表面層にインクジェットプリンターで文
字を直接この樹脂層にプリントしたところ、細かな抜き
文字部がにじんでしまい、十分な解像度は得られなかっ
た。Comparative Example 1 A CD-R medium was prepared in the same manner as in Example 1 except that dimethylacrylamide was omitted. When characters were directly printed on the hydrophilic surface layer with an ink jet printer on the resin layer, finely drawn character portions were blurred, and sufficient resolution could not be obtained.
【0043】比較例2 実施例2において、メチレンビスアクリルアミドを削除
した以外は、実施例2と同様にしてCD−R媒体を作成
した。この親水性表面層にインクジェットプリンターで
文字を直接この樹脂層にプリントしたところ、細かな抜
き文字部がにじんでしまい、十分な解像度は得られなか
った。Comparative Example 2 A CD-R medium was prepared in the same manner as in Example 2, except that methylenebisacrylamide was omitted. When characters were directly printed on the hydrophilic surface layer with an ink jet printer on the resin layer, finely drawn character portions were blurred, and sufficient resolution could not be obtained.
【0044】[0044]
【発明の効果】実施例及び比較例の結果からも明らかな
ように、本発明によれば、インクがにじんだり、はじい
たりすることなくインクジェットプリンターで文字等を
書き込むことのできる光記録媒体を提供することができ
る。As is apparent from the results of the examples and comparative examples, according to the present invention, an optical recording medium on which characters and the like can be written by an ink jet printer without ink bleeding or repelling is provided. can do.
───────────────────────────────────────────────────── フロントページの続き (72)発明者 川本 誠之 千葉県茂原市東郷1900番地 三井東圧化学 株式会社内 (72)発明者 加納 泰作 千葉県茂原市東郷1900番地 三井東圧化学 株式会社内 ──────────────────────────────────────────────────の Continuing on the front page (72) Inventor: Masayuki Kawamoto 1900 Togo, Mogo-shi, Chiba Mitsui Toatsu Chemical Co., Ltd.
Claims (9)
以上の保護層を順次積層してなる光記録媒体において、
表面に露出している保護層が、親水性ポリマー、親水性
モノマー、カチオンモノマー、共重合可能なモノマー及
びラジカル開始剤からなる硬化性組成物とフィラーとの
混練物をUV硬化せしめて得られたものからなり、該保
護層表面をプリンタブルに構成することを特徴とする光
記録媒体。An optical recording medium comprising a recording layer, a metal reflection layer, and two or more protective layers sequentially laminated on a transparent substrate.
A protective layer exposed on the surface was obtained by UV-curing a kneaded product of a filler and a curable composition comprising a hydrophilic polymer, a hydrophilic monomer, a cationic monomer, a copolymerizable monomer and a radical initiator. An optical recording medium comprising a protective layer and a surface of the protective layer being printable.
る保護層が、a)親水性ポリマー1〜80重量部、b)親
水性モノマー20〜88重量部、c)カチオンモノマー10〜
70重量部、d)共重合可能モノマー1〜40重量部、及び
e)ラジカル開始剤 0.1〜10重量部からなる硬化性組成
物とフィラーとの混練物をUV硬化せしめて得られたも
のからなり、該保護層表面をプリンタブルに構成するこ
とを特徴とする請求項1に記載の光記録媒体。2. The protective layer comprising a UV-curable resin exposed on the surface comprises: a) 1 to 80 parts by weight of a hydrophilic polymer, b) 20 to 88 parts by weight of a hydrophilic monomer, c) 10 to 10 parts by weight of a cationic monomer.
A kneaded product of a curable composition comprising 70 parts by weight, d) 1 to 40 parts by weight of a copolymerizable monomer, and e) 0.1 to 10 parts by weight of a radical initiator, and a filler obtained by UV curing. 2. The optical recording medium according to claim 1, wherein said protective layer surface is printable.
からなる保護層が、a)親水性ポリマー10〜70重量部、
b)親水性モノマー20〜78重量部、c)カチオンモノマ
ー10〜50重量部、d)共重合可能モノマー1〜20重量
部、及びe)ラジカル開始剤1〜8重量部からなる硬化
性組成物とフィラーとの混練物をUV硬化せしめて得ら
れたものからなり、該保護層表面をプリンタブルに構成
することを特徴とする請求項1に記載の光記録媒体。3. The protective layer made of a UV-curable resin exposed on the surface comprises: a) 10 to 70 parts by weight of a hydrophilic polymer,
b) a curable composition comprising 20 to 78 parts by weight of a hydrophilic monomer, c) 10 to 50 parts by weight of a cationic monomer, d) 1 to 20 parts by weight of a copolymerizable monomer, and e) 1 to 8 parts by weight of a radical initiator. 3. The optical recording medium according to claim 1, wherein the surface of the protective layer is made printable, which is obtained by UV-curing a kneaded product of a binder and a filler.
アミノ基を有することを特徴とする請求項1〜3のいず
れかに記載の光記録媒体。4. The optical recording medium according to claim 1, wherein the cationic monomer has an amide group and / or an amino group.
る保護層に含まれるフィラーが、吸水性及び/又は吸油
性を有する有機フィラー及び/又は無機フィラーを含有
するUV硬化樹脂からなり、フィラーの合計量が表面に
露出しているUV硬化樹脂 100重量部に対し、1〜80重
量部であることを特徴とする請求項1〜4のいずれかに
記載の光記録媒体。5. The filler contained in a protective layer made of a UV curable resin exposed on the surface is made of a UV curable resin containing an organic filler and / or an inorganic filler having water absorbency and / or oil absorbency. The optical recording medium according to any one of claims 1 to 4, wherein the total amount is 1 to 80 parts by weight based on 100 parts by weight of the UV curable resin exposed on the surface.
る保護層に含まれるフィラーが吸水性及び/又は吸油性
を有する有機フィラー及び/又は無機フィラーを含有す
るUV硬化樹脂からなり、フィラーの合計量が表面に露
出しているUV硬化樹脂 100重量部に対し、5〜50重量
部であることを特徴とする請求項5に記載の光記録媒
体。6. The filler contained in a protective layer made of a UV-curable resin exposed on the surface is made of a UV-curable resin containing an organic filler and / or an inorganic filler having a water absorbing property and / or an oil absorbing property. The optical recording medium according to claim 5, wherein the total amount is 5 to 50 parts by weight based on 100 parts by weight of the UV curable resin exposed on the surface.
のいずれかに記載の光記録媒体。7. The recording layer according to claim 1, wherein the recording layer comprises an organic dye.
The optical recording medium according to any one of the above.
性インクでプリントを施した請求項1〜7のいずれかに
記載の光記録媒体。8. The optical recording medium according to claim 1, wherein the protective layer exposed on the surface is printed with an aqueous or oil-based ink.
ィラー及び/又は無機フィラーと、請求項2〜6のいず
れかに記載のUV硬化性組成物からなるプリンタブルな
保護層を形成するに適したUV硬化型インク。9. A printable protective layer comprising an organic filler and / or an inorganic filler having a water absorbing property and / or an oil absorbing property and the UV curable composition according to any one of claims 2 to 6. UV curable ink.