JPH0789220A - Production of cast coated paper for ink jet recording, cast coated paper and recording method using the same - Google Patents
Production of cast coated paper for ink jet recording, cast coated paper and recording method using the sameInfo
- Publication number
- JPH0789220A JPH0789220A JP6132323A JP13232394A JPH0789220A JP H0789220 A JPH0789220 A JP H0789220A JP 6132323 A JP6132323 A JP 6132323A JP 13232394 A JP13232394 A JP 13232394A JP H0789220 A JPH0789220 A JP H0789220A
- Authority
- JP
- Japan
- Prior art keywords
- cast
- coated paper
- paper
- coating layer
- ink jet
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
Description
【0001】[0001]
【産業上の利用分野】本発明は、インクジェット記録用
キャスト塗被紙に関し、特に優れた白紙表面光沢を有
し、かつ優れたインクジェット記録(印字)適性を備え
たキャスト塗被紙の製造方法、キャスト塗被紙、及びそ
のキャスト塗被紙を用いたインクジェット記録方法に関
する。BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a cast coated paper for ink jet recording, and particularly to a method for producing a cast coated paper having an excellent white paper surface gloss and excellent ink jet recording (printing) suitability. The present invention relates to a cast coated paper and an inkjet recording method using the cast coated paper.
【0002】[0002]
【従来の技術】近年、インクジェットプリンタによる記
録が、騒音が少なく、高速記録が可能であり、かつ、多
色化が容易なために多方面で利用されている。インクジ
ェット記録用紙としては、インク吸収性に富むように工
夫された上質紙や、表面に多孔性顔料を塗工した塗被紙
等が適用されている。ところで、これらの用紙はすべて
表面光沢の低い、所謂マット調のインクジェット記録用
紙が主体である。2. Description of the Related Art In recent years, recording by an ink jet printer has been used in various fields because of its low noise, high speed recording, and easy multicoloring. As the ink jet recording paper, high-quality paper designed so as to have high ink absorbability, coated paper having a surface coated with a porous pigment, or the like is applied. By the way, all of these papers are mainly so-called matte ink jet recording papers having low surface gloss.
【0003】しかしながら、最近、インクジェット記録
の高速化、記録画像の高精細化、フルカラー化といった
用途の拡大に伴い、表面光沢の高い、優れた外観を持つ
インクジェット記録用紙が希求されている。一般に、表
面光沢の高い用紙としては、表面に板状顔料を塗被し、
さらに、必要に応じてキャレンダー処理を施した高光沢
を有する塗被紙、あるいは湿潤塗被層を鏡面を有する加
熱ドラム面に圧着、乾燥することにより、その鏡面を写
し取ることによって得られる、所謂キャスト塗被紙等が
知られている。However, recently, with the expansion of applications such as high-speed ink jet recording, high definition of recorded images, and full-color ink jet recording, an ink jet recording paper having a high surface gloss and an excellent appearance has been desired. Generally, for paper with high surface gloss, apply a plate-like pigment on the surface,
Further, it is obtained by copying the mirror surface of the coated paper having a high gloss, which has been subjected to a calendering treatment, or a wet coating layer, by pressing and drying it on a heating drum surface having a mirror surface, if necessary. Cast coated paper and the like are known.
【0004】このキャスト塗被紙はスーパーキャレンダ
ー仕上げされた通常の塗工紙に比較して高い表面光沢と
より優れた表面平滑性を有し、優れた印刷効果が得られ
ることから、高級印刷物等の用途に専ら利用されている
が、インクジェット記録用紙に利用した場合、種々の難
点を抱えている。This cast coated paper has high surface gloss and more excellent surface smoothness as compared with a normal coated paper which has been subjected to a super calender finish, and an excellent printing effect can be obtained. However, when used as an ink jet recording sheet, it has various difficulties.
【0005】即ち、一般に従来のキャスト塗被紙は、例
えばUS5275846号に開示されている。その塗被
層を構成する顔料組成物中の接着剤等の成膜性物質がキ
ャストコーターの鏡面ドラム表面を写し取ることにより
高い光沢を得ている。他方、この成膜性物質の存在によ
って塗被層の多孔性が失われ、インクジェット記録時の
インキの吸収を極端に低下させる等の問題を抱えてい
る。そして、このインキ吸収性を改善するには、キャス
ト塗被層がインキを容易に吸収できるようにポーラスに
してやることが重要であり、そのためには成膜性物質の
量を減ずることが必要となるが、成膜性物質の量を減ら
すことにより、結果として白紙光沢が低下する。That is, a conventional cast coated paper is generally disclosed in, for example, US Pat. No. 5,275,846. A film-forming substance such as an adhesive in the pigment composition constituting the coating layer gives a high gloss by copying the mirror surface of the cast coater. On the other hand, the presence of the film-forming substance causes a problem that the coating layer loses its porosity and the ink absorption during ink jet recording is extremely reduced. In order to improve the ink absorbability, it is important to make the cast coating layer porous so that the ink can be easily absorbed, and for that purpose, it is necessary to reduce the amount of the film-forming substance. However, by reducing the amount of film-forming substance, the glossiness of white paper is reduced as a result.
【0006】以上の如く、キャスト塗被紙の表面光沢と
インクジェット記録(印字)適性の両方を同時に満足さ
せることが極めて困難であるのが現状である。As described above, at present, it is extremely difficult to satisfy both the surface gloss of cast coated paper and the suitability for ink jet recording (printing) at the same time.
【0007】[0007]
【発明が解決しようとする課題】上記より、本発明者等
はキャスト塗被紙が本来有する高表面平滑性および高光
沢を維持し、かつインクジェット記録(印字)適性に優
れたキャスト塗被紙を得るべく鋭意研究を重ねた。その
結果、下塗り塗被層を設けた原紙上にある特定のガラス
転移点を持つ重合体を含有するキャスト用塗被液を塗被
して、キャスト仕上げすることにより、極めて優れたイ
ンクジェット印字記録適性を示し、かつキャスト塗被紙
本来の高光沢を維持し、従来のキャスト塗被紙では得る
ことのできなかった優れたインクジェット(印字)記録
適性を備えたキャスト塗被紙が得られることを見出した
のである。From the above, the inventors of the present invention have found a cast coated paper which maintains the high surface smoothness and high gloss originally possessed by the cast coated paper and is excellent in ink jet recording (printing) suitability. We have earnestly studied to obtain it. As a result, by applying a coating liquid for casting containing a polymer having a specific glass transition point on a base paper provided with an undercoat coating layer and performing a cast finish, extremely excellent inkjet printability In addition, it was found that a cast-coated paper that exhibits the excellent glossiness of inkjet-coated paper while maintaining the original high gloss of cast-coated paper and that has not been obtained with conventional cast-coated paper can be obtained. It was.
【0008】[0008]
【課題を解決するための手段】本発明は、以下の実施の
態様を含むがこれらのみに限らない。The present invention includes, but is not limited to, the following embodiments.
【0009】〔1〕 顔料および接着剤を含有する下塗
り塗被層を設けた原紙上に、エチレン性不飽和結合を有
するモノマーを重合させてなる40℃以上のガラス転移
点を有する重合体を含有する塗被液を塗被してキャスト
用塗被層を形成せしめ、該キャスト用塗被層が湿潤状態
にある間に、加熱された鏡面ドラムに圧接、乾燥して仕
上げるインクジェット記録用キャスト塗被紙の製造方
法。[1] A polymer having a glass transition point of 40 ° C. or higher obtained by polymerizing a monomer having an ethylenically unsaturated bond is contained on a base paper provided with an undercoating layer containing a pigment and an adhesive. The coating liquid for coating is applied to form a coating layer for casting, and while the coating layer for casting is in a wet state, it is pressed against a heated mirror surface drum and dried to finish. Paper manufacturing method.
【0010】〔2〕 鏡面ドラム表面の温度を重合体の
ガラス転移点未満の温度条件下で乾燥仕上げする〔1〕
記載のインクジェット記録用キャスト塗被紙の製造方
法。[2] The surface of the mirror drum surface is dried and finished under the temperature condition below the glass transition point of the polymer [1].
A method for producing the cast-coated paper for inkjet recording described.
【0011】〔3〕 顔料および接着剤を含有する下塗
り塗被層を設けた原紙上に、エチレン性不飽和結合を有
するモノマーを重合させてなる40℃以上のガラス転移
点を有する重合体を含有する塗被液を塗被してキャスト
用塗被層を形成せしめ、該キャスト用塗被層が湿潤状態
にある間に、加熱された鏡面ドラムに圧接、乾燥して仕
上げてなるインクジェット記録用キャスト塗被紙。[3] A polymer having a glass transition point of 40 ° C. or higher, which is obtained by polymerizing a monomer having an ethylenically unsaturated bond, on a base paper provided with an undercoat coating layer containing a pigment and an adhesive. An ink jet recording cast which is formed by applying a coating liquid to form a coating layer for casting, and while the coating layer for casting is in a wet state, is pressed against a heated mirror surface drum and dried to finish. Coated paper.
【0012】〔4〕 キャスト塗被紙の透気度が(JI
S−P−8117)300秒/100cc以下であるこ
とを特徴とする〔3〕記載のインクジェット記録用キャ
スト塗被紙。[4] The air permeability of the cast coated paper is (JI
SP-8117) 300 sec / 100 cc or less, The cast coated paper for inkjet recording according to [3].
【0013】〔5〕 下塗り塗被層中にカチオン樹脂を
含有せしめた〔3〕記載のインクジェット記録用キャス
ト塗被紙。[5] The cast coated paper for ink jet recording according to [3], wherein a cationic resin is contained in the undercoat coating layer.
【0014】〔6〕 顔料及び接着剤を含有する下塗り
塗被層を設けた原紙上に、エチレン性不飽和結合を有す
るモノマーを重合させてなる40℃以上のガラス転移点
を有する重合体を含有する表面塗被層を設けてなるイン
クジェット記録用強光沢紙に対して、微細孔から水性イ
ンクを吐出させて画像を形成することを特徴とするイン
クジェット記録方法。 〔7〕 水性インクに熱エネルギーを作用させてインク
を吐出させる〔6〕記載のインクジェット記録方法。[6] A polymer having a glass transition point of 40 ° C. or higher obtained by polymerizing a monomer having an ethylenically unsaturated bond is contained on a base paper provided with an undercoat coating layer containing a pigment and an adhesive. An ink jet recording method, characterized in that an image is formed by ejecting a water-based ink from fine pores on a strong glossy paper for ink jet recording having a surface coating layer. [7] The inkjet recording method according to [6], wherein thermal energy is applied to the water-based ink to eject the ink.
【0015】〔8〕 該光沢紙の表面塗被紙の透気度が
300秒/100cc以下である〔6〕記載のインクジ
ェット記録方法。[8] The ink jet recording method according to [6], wherein the coated paper of the glossy paper has an air permeability of 300 sec / 100 cc or less.
〔9〕 該光沢紙の下塗り塗被層がカチオン性樹脂を含
有する〔6〕記載のインクジェット記録方法。 〔10〕 該光沢紙の表面塗被層がコロイダルシリカを
含有する〔6〕記載のインクジェット記録方法。 〔11〕 該光沢紙の下塗り塗被層がアルミナ又はシリ
カを含有する〔6〕記載のインクジェット記録方法。[9] The inkjet recording method according to [6], wherein the undercoat coating layer of the glossy paper contains a cationic resin. [10] The inkjet recording method according to [6], wherein the surface coating layer of the glossy paper contains colloidal silica. [11] The inkjet recording method according to [6], wherein the undercoat coating layer of the glossy paper contains alumina or silica.
【0016】[0016]
【作用】前記したように、本発明の1つの態様では、顔
料および接着剤を含有する下塗り塗被層を設けた原紙上
に、特定のガラス転移点をもつ特定の樹脂を含有する塗
被組成物を塗被し、キャスト仕上げすることにより、本
発明の所望とする優れた表面光沢を維持し、かつ優れた
インクジェット記録(印字)適性を兼ね備えたインクジ
ェット記録用キャスト塗被紙を得るものである。As described above, in one embodiment of the present invention, a coating composition containing a specific resin having a specific glass transition point on a base paper provided with an undercoat coating layer containing a pigment and an adhesive. The object is to obtain a cast coated paper for inkjet recording, which has excellent surface gloss desired by the present invention and excellent aptitude for inkjet recording (printing) by coating and casting finish. .
【0017】ここに、キャスト塗被液としては、エチレ
ン性不飽和結合を有するモノマーを重合させてなる40
℃以上のガラス転移点を有する重合体を含有する塗被組
成物を使用するものである。Here, the cast coating liquid is obtained by polymerizing a monomer having an ethylenically unsaturated bond.
A coating composition containing a polymer having a glass transition point of not less than 0 ° C. is used.
【0018】即ち、本発明において、キャスト用塗被組
成物(キャスト塗被液)に含有されるエチレン性不飽和
結合を有するモノマー(以下エチレン性モノマーとい
う)を重合してなる重合体としては、例えばメチルアク
リレート、エチルアクリレートブチルアクリレート、2
エチルヘキシルアクリレート、ラウリルアクリレート、
2−ヒドロキシエチルアクリレート、グリシジルアクリ
レート等のアルキル基炭素数が1〜18個のアクリル酸
エステル、メチルメタクリレート、エチルメタクリレー
ト、2−ヒドロキシエチルメタクリレート、2−ヒドロ
キシプロピルメタクリレート、グリシジルメタクリレー
ト等のアルキル基炭素数が1〜18個のメタクリル酸エ
ステル、スチレン、α−メチルスチレン、ビニルトルエ
ン、アクリロニトリル、塩化ビニル、塩化ビニリデン、
酢酸ビニル、プロピオン酸ビニル、アクリルアミド、N
−メチロールアクリルアミド、エチレン、ブタジエン等
のエチレン性モノマーを重合して得られる重合体であ
る。本発明の効果を阻害しない範囲で他のモノマーを重
合させることも出来る。上記の中でも、特にスチレン−
アクリル酸エステル共重合体、スチレン−メタクリル酸
エステル共重合体が好ましい。That is, in the present invention, as a polymer obtained by polymerizing a monomer having an ethylenically unsaturated bond (hereinafter referred to as an ethylenic monomer) contained in a coating composition for casting (cast coating liquid), For example, methyl acrylate, ethyl acrylate butyl acrylate, 2
Ethylhexyl acrylate, lauryl acrylate,
Alkyl group such as 2-hydroxyethyl acrylate, glycidyl acrylate, etc. having 1 to 18 carbon atoms, alkyl group such as methyl methacrylate, ethyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, glycidyl methacrylate, etc. Of 1 to 18 methacrylic acid ester, styrene, α-methylstyrene, vinyltoluene, acrylonitrile, vinyl chloride, vinylidene chloride,
Vinyl acetate, vinyl propionate, acrylamide, N
A polymer obtained by polymerizing ethylenic monomers such as methylol acrylamide, ethylene and butadiene. Other monomers may be polymerized within the range that does not impair the effects of the present invention. Among the above, styrene-
Acrylic acid ester copolymers and styrene-methacrylic acid ester copolymers are preferred.
【0019】なお、重合体は、必要に応じて2種類以上
のエチレン性モノマーを併用した共重合体であっても良
いし、さらに、これら重合体あるいは共重合体の置換誘
導体でも良い。因みに、置換誘導体としては、例えばカ
ルボキシル基化したもの、またはそれをアルカリ反応性
にしたもの等が例示される。また、上記のエチレン性モ
ノマーをコロイダルシリカの存在下で重合させ、Si−
O−R(R:重合体成分)結合によって複合体になった
形で使用することも可能である。The polymer may be a copolymer in which two or more kinds of ethylenic monomers are used in combination, if necessary, and may be a substituted derivative of these polymers or copolymers. Incidentally, examples of the substituted derivative include, for example, those having a carboxyl group or those having an alkali reactivity. Further, the above-mentioned ethylenic monomer is polymerized in the presence of colloidal silica to obtain Si-
It is also possible to use it in the form of a complex by OR (R: polymer component) bond.
【0020】既述した如く、上記のエチレン性モノマー
を重合してなる重合体は、そのガラス転移点が40℃以
上のものが必要であり、より好ましくは約50℃〜約1
00℃の範囲であるものが望ましい。最も好ましくは約
70℃〜約90℃である。ガラス転移点は例えばエチレ
ン性モノマーの種類や重合体の架橋度合いにより調整す
ることができる。例えば比較的にガラス転移点を高くす
るスチレン等のモノマーを50重量%以上含有させるこ
とによりガラス転移点を高くすることが出来る。キャス
ト用塗被組成物中には、上記重合体の他にコロイダルシ
リカ等の顔料を配合することができ、通常その量は重合
体100重量部に対し約0重量部〜約200重量部が好
ましい。As mentioned above, the polymer obtained by polymerizing the above-mentioned ethylenic monomer is required to have a glass transition point of 40 ° C. or higher, more preferably about 50 ° C. to about 1 ° C.
It is preferably in the range of 00 ° C. Most preferably, it is about 70 ° C to about 90 ° C. The glass transition point can be adjusted by, for example, the type of ethylenic monomer or the degree of crosslinking of the polymer. For example, it is possible to raise the glass transition point by including 50% by weight or more of a monomer such as styrene which relatively raises the glass transition point. In the coating composition for casting, a pigment such as colloidal silica may be blended in addition to the above-mentioned polymer, and the amount thereof is usually about 0 parts by weight to about 200 parts by weight with respect to 100 parts by weight of the polymer. .
【0021】即ち、従来のキャスト塗被紙においては、
優れた表面光沢を得るために、キャスト仕上げを行う
際、塗被液内の樹脂分を十分成膜させ、キャスト光沢を
得ていた。しかし、このような方法では、キャスト塗被
紙表面の多孔性が減少し、結果として、インクジェット
記録時のインキの吸収を低下させるので好ましくない。
本発明では、このインクの吸収を低下させないために、
ガラス転移点が高い重合体を使用しているため、重合体
組成物が完全に成膜を起こさない状態でキャスト仕上げ
される。従ってキャスト塗被紙表面の多孔性の減少が軽
微であり、インキの吸収は低下せず、しかも優れた光沢
面を有するキャスト塗被面を得ることができる。重合体
のガラス転移点が40℃未満であると、キャストドラム
表面の熱によって、樹脂分の成膜化が必要以上に進み易
く、キャスト塗被紙表面の多孔性が減少し、インク吸収
性が低下してしまう。That is, in the conventional cast coated paper,
In order to obtain an excellent surface gloss, the resin content in the coating liquid was sufficiently formed into a film during the cast finish to obtain the cast gloss. However, such a method is not preferable because the porosity of the surface of the cast coated paper is reduced and, as a result, the absorption of ink during inkjet recording is reduced.
In the present invention, in order not to reduce the absorption of this ink,
Since a polymer having a high glass transition point is used, the polymer composition is cast-finished in a state where film formation does not occur completely. Therefore, the decrease in the porosity of the surface of the cast coated paper is slight, the absorption of the ink does not decrease, and a cast coated surface having an excellent glossy surface can be obtained. When the glass transition point of the polymer is lower than 40 ° C., the heat of the surface of the cast drum facilitates the film formation of the resin component more than necessary, the porosity of the surface of the cast coated paper is reduced, and the ink absorbency is reduced. Will fall.
【0022】本発明は、前述の如き特定のガラス転移点
を有する重合体だけでキャスト塗被層用の組成物を得る
ことができるが、必要に応じて離型性改良のために、離
型剤がカゼイン、大豆蛋白等を併用することもできる。
さらに、インクジェット印字後のインキ定着性や耐水性
を向上させる目的で、3級アミノ基や、4級アンモニウ
ム基を含有したカチオン性の樹脂等が併用される。その
他、白色度、粘度、流動性等を調節するために、一般の
印刷用塗被紙やインクジェット用紙に使用されている顔
料、分散剤、増粘剤、消泡剤、着色剤、帯電防止剤、防
腐剤等の各種助剤が適宜添加される。In the present invention, the composition for cast coating layer can be obtained only by the polymer having the specific glass transition point as described above. The agent can be used in combination with casein, soybean protein and the like.
Further, a cationic resin containing a tertiary amino group or a quaternary ammonium group is used in combination for the purpose of improving ink fixability and water resistance after inkjet printing. In addition, pigments, dispersants, thickeners, defoamers, colorants, antistatic agents used for general printing coated papers and inkjet papers to adjust whiteness, viscosity, fluidity, etc. , Various auxiliaries such as preservatives are appropriately added.
【0023】次に、本発明の方法は上記の上塗り用塗液
(キャスト用塗液又は特定の重合体組成物ともよぶ)を
支持体(主に原紙)上に予め設けた下塗り塗被層上に塗
被することが必要である。原紙上に直接塗被して、キャ
スト仕上げを行った場合、原紙の表面平滑が下塗りした
ものに比べ著しく劣るため、所謂ピンホール等の表面欠
陥が生じる。本発明の別の態様ではキャスト塗被紙のJ
IS−P−8117に準拠して測定した透気度を300
秒/100cc以下に調整することにより優れたインク
吸収性を得ている。JIS−P−8117に準拠して測
定した透気度が300秒/100ccを越えると、イン
キの吸収性が低下する傾向がある。透気度の下限は特に
限定しないが通常約5秒/100cc以上が好ましい。
透気度はより好ましくは約10秒/100cc〜約20
0秒/100ccである。Next, in the method of the present invention, the above-mentioned top coating solution (also referred to as a casting coating solution or a specific polymer composition) is preliminarily provided on a support (mainly base paper) on an undercoat coating layer. It is necessary to coat it. When the base paper is directly coated and cast-finished, the surface smoothness of the base paper is remarkably inferior to that of the undercoat, so that surface defects such as so-called pinholes occur. In another aspect of the invention, the cast coated paper J
The air permeability measured according to IS-P-8117 is 300.
Excellent ink absorbency is obtained by adjusting the time to not more than 100 sec / sec. If the air permeability measured according to JIS-P-8117 exceeds 300 seconds / 100 cc, the ink absorbency tends to decrease. The lower limit of the air permeability is not particularly limited, but usually about 5 seconds / 100 cc or more is preferable.
The air permeability is more preferably about 10 seconds / 100 cc to about 20.
It is 0 second / 100 cc.
【0024】キャスト塗被層を形成した後に上記のよう
なJIS−P−8117に従う透気度が300秒/10
0ccのキャスト塗被紙を得るための1つの手段として
は、下塗り塗被層を設けた後の基紙の塗被面のガーレー
高圧型透気度試験機による測定値(ASTM−D−72
6 B法)で、30秒/10cc以下(値が低い方が透
気性が良い)、好ましくは20秒/10cc以下である
ように調整することが挙げられる。因みに30秒/10
ccを越えるとインクジェットのインク吸収性が低下す
る傾向があり、キャスト操業性も低下する。After forming the cast coating layer, the air permeability according to JIS-P-8117 as described above is 300 seconds / 10.
One means for obtaining 0 cc of cast coated paper is a value measured by a Gurley high pressure type air permeability tester (ASTM-D-72) on the coated surface of the base paper after providing an undercoat coating layer.
6 B method), it may be adjusted to 30 seconds / 10 cc or less (the lower the value, the better the air permeability), preferably 20 seconds / 10 cc or less. By the way, 30 seconds / 10
If it exceeds cc, the ink absorbency of the inkjet tends to decrease, and the cast operability also decreases.
【0025】下塗り塗被層に含有される顔料と接着剤に
ついて述べる。即ち、顔料としては、例えばカオリン、
クレー、焼成クレー、無定形シリカ、酸化亜鉛、酸化ア
ルミニウム、水酸化アルミニウム、炭酸カルシウム、サ
チンホワイト、珪酸アルミニウム、スメクタイト、珪酸
マグネシウム、炭酸マグネシウム、酸化マグネシウム、
珪藻土、スチレン系プラスチックピグメント、尿素樹脂
系プラスチックピグメント、ベンゾグアナミン系プラス
チックピグメント等、一般塗被紙製造分野で公知公用の
各種顔料が使用できる。The pigment and adhesive contained in the undercoat coating layer will be described. That is, as the pigment, for example, kaolin,
Clay, calcined clay, amorphous silica, zinc oxide, aluminum oxide, aluminum hydroxide, calcium carbonate, satin white, aluminum silicate, smectite, magnesium silicate, magnesium carbonate, magnesium oxide,
Various publicly known pigments used in the general coated paper manufacturing field such as diatomaceous earth, styrene-based plastic pigments, urea resin-based plastic pigments, and benzoguanamine-based plastic pigments can be used.
【0026】なお、上記の顔料の中でも、とりわけ無定
形シリカ、アルミナ等のポーラスな顔料を用いると、イ
ンクジェット記録時のインク吸収性、印字発色濃度が改
善されるので特によい。その理由は無定形シリカやアル
ミナが非常にポーラスな構造を持つために、塗被層中に
多量の空隙が得られ、結果として透気度も下がり、イン
ク吸収性が改善される。Among the above pigments, it is particularly preferable to use a porous pigment such as amorphous silica or alumina because the ink absorbability during ink jet recording and the print color density are improved. The reason is that since amorphous silica and alumina have a very porous structure, a large amount of voids are obtained in the coating layer, and as a result, air permeability is lowered and ink absorption is improved.
【0027】さらに、この顔料は高い透明性を持つため
に、塗被層中に吸収されたインク染料の発色を妨げない
ために、結果的に印字発色性が向上させられる。また、
ポーラスな顔料の添加量は顔料として、少なくとも50
重量%以上含有させることが望ましい。Further, since this pigment has high transparency, it does not interfere with the color development of the ink dye absorbed in the coating layer, and as a result, the color development of the print is improved. Also,
The amount of porous pigment added is at least 50 as a pigment.
It is desirable that the content be at least wt%.
【0028】次に、下塗り塗被層の接着剤としては、カ
ゼイン、大豆蛋白、合成蛋白等の蛋白質類、澱粉や酸化
澱粉等の各種澱粉類、ポリビニルアルコール、カルボキ
シメチルセルロースやメチルセルロース等のセルロース
誘導体、スチレン−ブタジエン共重合体、メチルメタク
リレート−ブタジエン共重合体の共役ジエン系重合体ラ
テックス、アクリル系重合体ラテックス、エチレン−酢
酸ビニル共重合体等のビニル系重合体ラテックス、等一
般に塗被紙用として用いられている従来公知の接着剤が
単独、あるいは併用して用いられる。なお接着剤の配合
量は顔料に対し、5〜50重量%、より好ましくは10
〜30重量%の範囲で調節される。Next, as an adhesive for the undercoat layer, proteins such as casein, soybean protein and synthetic protein, various starches such as starch and oxidized starch, polyvinyl alcohol, cellulose derivatives such as carboxymethyl cellulose and methyl cellulose, Styrene-butadiene copolymer, methyl methacrylate-butadiene copolymer conjugated diene polymer latex, acrylic polymer latex, vinyl polymer latex such as ethylene-vinyl acetate copolymer, etc. Generally for coated paper The conventionally known adhesives used can be used alone or in combination. The amount of the adhesive compounded is 5 to 50% by weight, more preferably 10% by weight, based on the pigment.
It is adjusted in the range of ˜30% by weight.
【0029】本発明の更に別の態様ではキャスト塗被紙
の製造に際し、キャスト塗被液(上塗り層用塗被液)に
含有される重合体のガラス転移点未満の温度条件でキャ
スト塗被層を乾燥仕上げすることにより、好ましい結果
が得られる。尚、鏡面ドラム温度の下限については特に
限定されないが、好ましくは約40℃以上である。より
好ましくは約50℃〜約90℃である。支持体(原紙)
に下塗り層を設け、更に前記特定のガラス転移点を有す
る重合体を含有するキャスト塗被組成物層を形成し、キ
ャストドラムに圧接して、キャスト仕上げするに際し、
特にその重合体のガラス転移点未満のドラム表面温度で
乾燥を行うことが好ましい。上記により、重合体組成物
が完全な皮膜を形成しない状態でキャスト仕上げを行う
ことにより、キャスト塗被層表面の多孔性を維持した状
態で、強光沢を有するキャスト塗被層面を得ることがで
きるわけである。In still another embodiment of the present invention, in the production of cast coated paper, the cast coated layer is formed at a temperature condition below the glass transition point of the polymer contained in the cast coating liquid (coating liquid for the overcoat layer). Drying of the gives good results. The lower limit of the mirror surface drum temperature is not particularly limited, but it is preferably about 40 ° C. or higher. More preferably, it is about 50 ° C to about 90 ° C. Support (base paper)
To provide a subbing layer, further to form a cast coating composition layer containing a polymer having the specific glass transition point, press-contacted to the cast drum, when cast finish,
It is particularly preferable to carry out the drying at a drum surface temperature below the glass transition point of the polymer. According to the above, by performing the cast finish in a state in which the polymer composition does not form a complete film, it is possible to obtain a cast coating layer surface having high gloss while maintaining the porosity of the cast coating layer surface. That is why.
【0030】逆にキャスト塗被層の乾燥温度を高くする
と、これらの重合体はそのガラス転移点以上で成膜が行
われ、結果的に、高分子皮膜によりキャスト塗被層表面
の多孔性が阻害されるのでインクジェット記録時のイン
キの吸収を低下させる傾向がある。特にガラス転移点を
20℃以上越えるドラム表面温度は好ましくない。On the contrary, when the drying temperature of the cast coating layer is increased, these polymers are formed at a temperature not lower than their glass transition point, and as a result, the porosity of the surface of the cast coating layer is increased by the polymer film. Since they are hindered, they tend to reduce the ink absorption during inkjet recording. Particularly, a drum surface temperature exceeding the glass transition point by 20 ° C. or more is not preferable.
【0031】因みに、重合体のガラス転移点が40℃未
満の場合、それ以下の表面温度でキャスト仕上げするこ
とになり、結果としてキャスト塗被組成物の乾燥スピー
ドが著しく遅くなり、生産性の低下が避けられない。By the way, when the glass transition point of the polymer is less than 40 ° C., the casting is finished at a surface temperature lower than that, and as a result, the drying speed of the cast coating composition is remarkably slowed and the productivity is lowered. Is inevitable.
【0032】而して、下塗り塗被層用組成物は、一般に
固形分濃度を1〜65重量%程度に調整し、米坪が約2
0〜400g/m2 程度の原紙上に乾燥重量で2〜50
g/m2 、より好ましくは5〜20g/m2 程度になる
ようにブレードコーター、エアーナイフコーター、ロー
ルコーター、ブラシコーター、チャンプレックスコータ
ー、バーコーター、グラビアコーター等の各種公知公用
の塗被装置により塗被、乾燥される。さらに、必要に応
じて下塗り塗被層の乾燥後にスーパーキャレンダー、ブ
ラシ掛け、キャスト仕上げ等の平滑化処理を施すことも
できる。Thus, the composition for the undercoat layer generally has a solid content concentration adjusted to about 1 to 65% by weight, and has a basis weight of about 2%.
2 to 50 dry weight on base paper of 0 to 400 g / m 2
g / m 2, more preferably a blade coater so that the order of 5 to 20 g / m 2, an air knife coater, roll coater, brush coater, champflex coater, a bar coater, various known and used coated device such as a gravure coater Is coated and dried. Further, if necessary, smoothing treatment such as super calendering, brushing, and cast finishing can be performed after drying the undercoat layer.
【0033】なお、ベースとなる原紙としては、特に限
定されるものではなく、一般の塗被紙に使用される酸性
紙、あるいは中性紙等が適宜使用される。また印字品質
に合わせてサイズ度や填料を適宜調整できる。かくして
得られた下塗り塗被紙の塗被面に、前述した特定の重合
体組成物よりなるキャスト塗被液を、ブレードコータ
ー、エアーナイフコーター、ロールコーター、ブラシコ
ーター、チャンプレックスコーター、バーコーター、グ
ラビアコーター等の各種公知の塗被装置により塗被し、
前述したように塗被層が湿潤状態にある間に、加熱され
た鏡面ドラムに圧接、乾燥してキャスト仕上げを行うこ
とになる。この場合のキャスト塗被液の塗被量は、乾燥
固形分で0.2〜30g/m2 、好ましくは、1〜10
g/m2 である。The base paper to be the base is not particularly limited, and acid paper or neutral paper used for general coated paper is appropriately used. Further, the sizing degree and the filler can be appropriately adjusted according to the print quality. The coating surface of the thus obtained undercoat coated paper, a cast coating liquid consisting of the specific polymer composition described above, a blade coater, an air knife coater, a roll coater, a brush coater, a Chanplex coater, a bar coater, Coating with various known coating devices such as gravure coater,
As described above, while the coating layer is in the wet state, it is pressed against the heated mirror surface drum and dried to perform the cast finish. The coating amount of the cast coating liquid in this case is 0.2 to 30 g / m 2 in terms of dry solid content, preferably 1 to 10
It is g / m 2 .
【0034】キャスト塗被液中には白色度、粘度、流動
性等を調節するために、一般の印刷用塗被紙やインクジ
ェット用紙に使用されている顔料、分散剤、増粘剤、消
泡剤、着色剤、帯電防止剤、防腐剤等の各種助剤を適宜
添加することが出来る。In the cast coating liquid, pigments, dispersants, thickeners and defoaming agents used for general coated papers for printing and ink jet papers are used for controlling whiteness, viscosity, fluidity and the like. Various auxiliaries such as agents, colorants, antistatic agents and preservatives can be appropriately added.
【0035】尚、従来インクジェット用紙については、
その耐水性や印字発色濃度を向上させる目的でカチオン
性樹脂を塗被層中に添加することが知られている。しか
しながら、これらのカチオン性樹脂を、従来の一般キャ
スト塗被液に添加すると、表面光沢の低下やインク吸収
性の低下をもたらすため好ましくない。他方、カチオン
性樹脂を下塗り塗被層用塗被液に添加することは、表面
光沢やインク吸収性を低下させることなく、耐水性や印
字発色濃度を良好にすることができるものである。さら
に、カチオン性樹脂を下塗り層用塗被液に添加すること
は前述した重合体組成物を主成分とするキャスト用塗被
組成物を上塗りとして塗被した際に、カチオン性樹脂が
キャスト用塗被組成物の凝集を促進させるため、下塗り
層への過度の浸透を防ぎ、結果として、光沢むらやピン
ホールの少ない均一で光沢の高いキャスト塗被表面を得
ることができる。Regarding conventional ink jet paper,
It is known to add a cationic resin to the coating layer for the purpose of improving the water resistance and the color density of printing. However, it is not preferable to add these cationic resins to conventional general cast coating liquids, because they lower the surface gloss and the ink absorbency. On the other hand, addition of a cationic resin to the undercoat coating layer coating liquid can improve water resistance and print color density without lowering surface gloss and ink absorbency. Furthermore, the addition of a cationic resin to the coating liquid for the undercoat layer means that when the coating composition for casting containing the above-mentioned polymer composition as a main component is coated as the top coating, the cationic resin is coated for casting. Since the aggregation of the composition is promoted, excessive penetration into the undercoat layer can be prevented, and as a result, a uniform and high-gloss cast coating surface with less uneven gloss and pinholes can be obtained.
【0036】なお、この場合のカチオン性樹脂として
は、例えばポリエチレンポリアミンやポリプロピレンポ
リアミンなどのポリアルキレンポリアミン類、またはそ
の誘導体、第3級アミノ基や第4級アンモニウム基を有
するアクリル樹脂、ジアクリルアミン等が使用される。The cationic resin in this case is, for example, a polyalkylene polyamine such as polyethylene polyamine or polypropylene polyamine, or a derivative thereof, an acrylic resin having a tertiary amino group or a quaternary ammonium group, a diacrylamine. Etc. are used.
【0037】さらに、カチオン性樹脂の添加量として
は、顔料100重量部に対し、1〜30重量部、より好
ましくは5〜20重量部の範囲で調節される。その他、
一般塗被紙の製造において使用される分散剤、増粘剤、
消泡剤、着色剤、帯電防止剤、防腐剤等の各種助剤が適
宜添加される。Further, the addition amount of the cationic resin is adjusted in the range of 1 to 30 parts by weight, more preferably 5 to 20 parts by weight, relative to 100 parts by weight of the pigment. Other,
Dispersants, thickeners, used in the production of general coated paper,
Various auxiliaries such as defoaming agents, colorants, antistatic agents and preservatives are appropriately added.
【0038】かくして得られるインクジェット記録用キ
ャスト塗被紙を用いた本発明のインクジェット記録方法
は、インクをノズルより効果的に離脱させて、射程体で
ある記録媒体にインクを付与し得る方式であれば、いか
なる方式でもよいが、特に、特開昭54−59936号
公報に記載されている方法で、熱エネルギーの作用を受
けたインクが急激な体積変化を生じ、この状態変化によ
る作用力によって、インクをノズルより吐出させるイン
クジェット記録方式が有効に使用できるものである。The ink jet recording method of the present invention using the thus obtained cast coated paper for ink jet recording may be a system capable of effectively separating the ink from the nozzle to apply the ink to the recording medium as a range. Any method may be used, but in particular, in the method described in JP-A-54-59936, the ink subjected to the action of thermal energy undergoes a rapid volume change, and the action force due to this state change causes An inkjet recording method in which ink is ejected from nozzles can be effectively used.
【0039】本発明のインクジェット記録方法に好適な
一例のインクジェット記録装置を以下に説明する。その
装置の主要部である、ヘッド構成例を図1、図2及び図
3に示す。即ち、ヘッド13はインクを通す溝14を有
するガラス、セラミックまたはプラスチック板等を、感
熱記録に用いられる発熱ヘッド15(図ではヘッドが示
されているが、これに限定されるものではない)とを接
着して得られる。発熱ヘッド15は酸化シリコン等で形
成される保護膜16、アルミニウム電極17−1、17
−2、ニクロム等で形成される発熱抵抗体層18、蓄熱
層19、アルミナ等の放熱性の良い基板20よりなって
いる。An example of an inkjet recording apparatus suitable for the inkjet recording method of the present invention will be described below. An example of the head structure, which is the main part of the apparatus, is shown in FIGS. 1, 2 and 3. That is, the head 13 is made of glass, ceramic, plastic plate, or the like having a groove 14 through which ink passes, and a heating head 15 (a head is shown in the drawing, but not limited to this) used for thermal recording. It is obtained by bonding. The heating head 15 includes a protective film 16 made of silicon oxide or the like and aluminum electrodes 17-1 and 17.
-2, a heating resistor layer 18 made of nichrome or the like, a heat storage layer 19, and a substrate 20 having a good heat dissipation property such as alumina.
【0040】インク21は吐出オリフィス(微細孔)2
2まで来ており、圧力Pによりメニスカス23を形成し
ている。The ink 21 has a discharge orifice (fine hole) 2
2, the meniscus 23 is formed by the pressure P.
【0041】いま、電極17−1、17−2に電気信号
が加わると、発熱ヘッド15のnで示される領域が急激
に発熱し、ここに接しているインク21に気泡が発生
し、その圧力でメニスカス23が突出し、インク21が
吐出し、オリフィス22より記録小滴24となり、記録
シート25に向かって飛翔する。図3には図1に示すヘ
ッドを多数並べたマルチヘッドの外観図を示す。該マル
チヘッドはマルチ溝26を有するガラス板27と、図1
に説明したものと同様な発熱ヘッド28を密着して製作
されている。Now, when an electric signal is applied to the electrodes 17-1 and 17-2, the area indicated by n of the heating head 15 rapidly generates heat, and bubbles are generated in the ink 21 in contact therewith, and the pressure thereof is generated. At this point, the meniscus 23 is projected, the ink 21 is ejected, becomes a recording droplet 24 from the orifice 22, and flies toward the recording sheet 25. FIG. 3 shows an external view of a multi-head in which many heads shown in FIG. 1 are arranged. The multi-head includes a glass plate 27 having multi-grooves 26, and FIG.
The heating head 28 similar to that described in FIG.
【0042】なお、図1はインク流路に沿ったヘッド1
3の断面図であり、図2は図1のA−B線での切断図で
ある。FIG. 1 shows the head 1 along the ink flow path.
3 is a sectional view of FIG. 3, and FIG. 2 is a sectional view taken along the line AB of FIG. 1.
【0043】図4に、かかるヘッドを、組み込んだイン
クジェット記録装置の1例を示す。図4において、61
はワイピング部材としてのブレードであり、その一端は
ブレード保持部材によって保持されて固定端となり、カ
ンチレバーの形態をなす。ブレード61は記録ヘッドに
より記録領域に隣接した位置に配設され、また、本例の
場合、記録ヘッドの移動経路中に突出した形態で保持さ
れる。62はキャップであり、ブレード61に隣接する
ホームポジションに配設され、記録ヘッドの移動方向と
垂直な方向に移動して吐出口面と当接し、キャッピング
を行う構成を備える。さらに、63はブレード61に隣
接して設けられるインク吸収体であり、ブレード61と
同様に記録ヘッドの移動経路中に突出した形態で保持さ
れる。上記ブレード61、キャップ62、吸収体63に
よって吐出回復部64が構成され、ブレード61及び吸
収体63によってインク吐出口面に水分、塵埃等の除去
が行われる。FIG. 4 shows an example of an ink jet recording apparatus incorporating such a head. In FIG. 4, 61
Is a blade serving as a wiping member, one end of which is held by a blade holding member to be a fixed end, which is in the form of a cantilever. The blade 61 is arranged at a position adjacent to the recording area by the recording head, and in the case of this example, is held in a form protruding in the movement path of the recording head. Reference numeral 62 denotes a cap, which is disposed at a home position adjacent to the blade 61, and has a configuration in which it moves in a direction perpendicular to the moving direction of the recording head and contacts the ejection port surface to perform capping. Further, 63 is an ink absorber provided adjacent to the blade 61, and is held in a form projecting in the movement path of the recording head like the blade 61. The blade 61, the cap 62, and the absorber 63 form an ejection recovery unit 64, and the blade 61 and the absorber 63 remove water, dust, and the like from the ink ejection port surface.
【0044】65は吐出エネルギー発生手段を有し、吐
出口を配した吐出口面に対向する記録媒体にインクを吐
出して記録を行う記録ヘッド、66は記録ヘッド65を
搭載して記録ヘッド65の移動を行う為のキャリッジで
ある。キャリッジ66はガイド軸67と摺動可能に係合
し、キャリッジ66の一部はモーター68によって駆動
されるベルト69と接続(不図示)している。これによ
り、キャリッジ66はガイド軸67に沿った移動が可能
となり、記録ヘッド65による記録領域及びそれに隣接
して領域の移動が可能となる。Reference numeral 65 denotes a recording head having ejection energy generating means for ejecting ink to a recording medium facing the ejection port surface where the ejection port is arranged for recording, and 66 a recording head 65 having the recording head 65 mounted thereon. It is a carriage for moving the. The carriage 66 slidably engages with a guide shaft 67, and a part of the carriage 66 is connected (not shown) to a belt 69 driven by a motor 68. Accordingly, the carriage 66 can move along the guide shaft 67, and the recording area by the recording head 65 and the area adjacent thereto can be moved.
【0045】51は記録媒体を挿入する為の給紙部、5
2は不図示のモーターにより駆動される紙送りローラー
である。これらの構成によって記録ヘッドの吐出口面と
対向する位置へ記録媒体が給紙され、記録が進行するに
つれて排紙ローラー53を介して排紙される。Reference numeral 51 designates a paper feed section for inserting a recording medium, and 5
A paper feed roller 2 is driven by a motor (not shown). With these configurations, the recording medium is fed to a position facing the ejection opening surface of the recording head, and is ejected via the ejection roller 53 as the recording progresses.
【0046】上記の構成において、記録ヘッド65が記
録終了等でホームポジションに戻る際、ヘッド回復部6
4のキャップ62は記録ヘッド65の移動経路から退避
しているが、ブレード61は移動経路中に突出してい
る。その結果、記録ヘッド65の吐出口面がワイピング
される。なお、キャップ62が記録ヘッド65の突出面
に当接してキャッピングを行う場合、キャップ62は記
録ヘッドの移動経路中に突出するように移動する。In the above structure, when the recording head 65 returns to the home position after recording is completed, the head recovery unit 6
The fourth cap 62 is retracted from the movement path of the recording head 65, but the blade 61 is projected in the movement path. As a result, the ejection port surface of the recording head 65 is wiped. When the cap 62 comes into contact with the protruding surface of the recording head 65 to perform capping, the cap 62 moves so as to protrude into the movement path of the recording head.
【0047】記録ヘッド65がホームポジションから記
録開始位置へ移動する場合、キャップ62及びブレード
61は上述したワイピング時の位置と同一の位置にあ
る。その結果、その移動においても記録ヘッド65の突
出口面はワイピングされる。When the recording head 65 moves from the home position to the recording start position, the cap 62 and the blade 61 are in the same positions as the above wiping positions. As a result, the protruding opening surface of the recording head 65 is wiped even during the movement.
【0048】上述の記録ヘッドのホームポジションへの
移動は、記録終了時や吐出回復時ばかりでなく、記録ヘ
ッドが記録のために記録領域を移動する間に所定の間隔
で記録領域に隣接したホームポジションへ移動し、その
移動に伴って、上記ワイピングが行われる。The above-mentioned movement of the recording head to the home position is performed not only at the end of recording and at the time of ejection recovery, but also at the home adjacent to the recording area at a predetermined interval while the recording head moves in the recording area for recording. After moving to the position, the wiping is performed in accordance with the movement.
【0049】一方、本発明のインクジェット記録方法で
使用されるインクとしては、像を形成する為の色素と該
色素を溶解または分散する為の液媒体を必須成分とし、
必要に応じて各種の分散剤、界面活性剤、粘度調整剤、
比抵抗調整剤、pH調整剤、防黴剤、記録剤の溶解(ま
たは分散)安定化剤等を添加して調製される。On the other hand, in the ink used in the ink jet recording method of the present invention, a dye for forming an image and a liquid medium for dissolving or dispersing the dye are essential components,
If necessary, various dispersants, surfactants, viscosity modifiers,
It is prepared by adding a specific resistance adjusting agent, a pH adjusting agent, an antifungal agent, a dissolution (or dispersion) stabilizer of a recording agent, and the like.
【0050】インクに使用される記録剤としては直接染
料、酸性染料、塩基性染料、反応性染料、食用色素、分
散染料、油性染料および各種顔料等が挙げられるが、従
来公知のものは特に制限なく使用することができる。こ
のような色素の含有量は、液媒体成分の種類、インクに
要求される特性等に依存して決定されるが、本発明にお
けるインクの場合も、従来のインク中におけるような配
合、即ち、0.1〜20重量%程度の割合になるような
使用で特に問題はない。The recording agents used in the ink include direct dyes, acid dyes, basic dyes, reactive dyes, food dyes, disperse dyes, oil dyes and various pigments, but conventionally known ones are not particularly limited. Can be used without. The content of such a dye is determined depending on the type of liquid medium component, the properties required for the ink, etc., but in the case of the ink of the present invention, the formulation as in the conventional ink, that is, There is no particular problem when used in a proportion of about 0.1 to 20% by weight.
【0051】本発明で用いられるインクとしては、上記
の如き色素を溶解または分散させてなる液溶媒であっ
て、水または水と水溶性有機溶剤として、インクの乾燥
防止効果を有する多価アルコールを含有するものが使用
される。The ink used in the present invention is a liquid solvent prepared by dissolving or dispersing the above-mentioned dye, and is water or water and a water-soluble organic solvent, and a polyhydric alcohol having an ink drying preventing effect. What is contained is used.
【実施例】以下に実施例を挙げて、本発明をより具体的
に説明するが、勿論これらに限定されるものではない。
また、例中の部および%は特に断らない限り、それぞれ
重量部および重量%を示す。特に断らない限り重量部は
水を除いた固形分のみの重量部を示す。キャスト塗被層
形成後の透気度はJIS−P−8117により測定し、
秒/100ccの単位で表示した。下塗り層形成後の原
紙の透気度はガーレー高圧型透気度試験機を用い、AS
TM−D−726 B法に従い、秒/10ccで表示し
た。The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples.
Unless otherwise specified, parts and% in the examples represent parts by weight and% by weight, respectively. Unless stated otherwise, parts by weight refer to parts by weight of solids only, excluding water. The air permeability after forming the cast coating layer is measured according to JIS-P-8117,
Displayed in units of seconds / 100 cc. The air permeability of the base paper after forming the undercoat layer was measured by AS
Displayed in seconds / 10 cc according to the TM-D-726B method.
【0052】実施例1−1 顔料として無定形シリカ100部を使用し、接着剤とし
てポリビニルアルコール20部、カチオン樹脂として4
級アンモニウム塩含有アクリル系樹脂5部、分散剤とし
てポリ燐酸ソーダ0.5部を添加し、固形分濃度が20
%の下塗り用塗被液を調製した。この下塗り用塗被液
を、米坪100g/m2 の原紙に乾燥重量で10g/m
2 になるように、エアーナイフコーターで塗被、乾燥し
て下塗り原紙を得た。この下塗り原紙の透気度をガーレ
ー高圧型透気度試験機で測定したところ、5秒/10c
cであった。Example 1-1 100 parts of amorphous silica was used as a pigment, 20 parts of polyvinyl alcohol was used as an adhesive, and 4 parts was used as a cationic resin.
5 parts of acrylic resin containing primary ammonium salt and 0.5 part of sodium polyphosphate as a dispersant were added to give a solid content of 20.
% Coating solution for undercoating was prepared. 10 g / m 2 dry weight of this base coating liquid on a base paper of 100 g / m 2
2 was coated with an air knife coater and dried to obtain an undercoat base paper. The air permeability of this undercoat base paper was measured with a Gurley high pressure type air permeability tester and was 5 seconds / 10c.
It was c.
【0053】一方、キャスト塗被液として、ガラス転移
点が80℃のスチレン−2メチルヘキシルアクリレート
共重合体100部、離型剤としてステアリン酸カルシウ
ム10部よりなる固形分濃度が40%の塗被液を調製し
た。このキャスト塗被液を上記の下塗り原紙上にロール
コーターを用いて塗被した後、ただちに表面温度が75
℃の鏡面ドラムに圧接し、乾燥後、離型させ、インクジ
ェット記録用キャスト塗被紙を得た。この時のキャスト
塗被量は固形分重量で、5g/m2 であった。On the other hand, 100 parts of a styrene-2 methylhexyl acrylate copolymer having a glass transition point of 80 ° C. as a cast coating solution and 10 parts of calcium stearate as a releasing agent, a coating solution having a solid content concentration of 40%. Was prepared. This cast coating liquid was coated on the above base coating base paper using a roll coater, and immediately after the surface temperature was raised to 75
It was pressed against a mirror surface drum at ℃, dried, and then released to obtain a cast coated paper for inkjet recording. The cast coating amount at this time was 5 g / m 2 in terms of solid content weight.
【0054】実施例1−2 キャスト塗被液として、ガラス転移点70℃のスチレン
−メチルアクリレート共重合体とコロイダルシリカの複
合体(共重合体とコロイダルシリカの重量比は50:5
0)100部、離型剤としてステアリン酸カルシウム1
0部よりなる固形分濃度が40%の塗被液を調製した。
このキャスト塗被液を実施例1−1の下塗り原紙(下塗
り層を有する原紙)上にロールコーターを用いて塗被し
た後、ただちに表面温度が60℃の鏡面ドラムに圧接
し、乾燥後、離型させ、インクジェット記録用キャスト
塗被紙を得た。この時のキャスト塗被量は固形分重量
で、2g/m2 であった。Example 1-2 As a cast coating liquid, a composite of a styrene-methyl acrylate copolymer having a glass transition point of 70 ° C. and colloidal silica (the weight ratio of the copolymer to the colloidal silica is 50: 5).
0) 100 parts, calcium stearate 1 as a release agent
A coating liquid having a solid content concentration of 0% of 40% was prepared.
This cast coating liquid was applied onto the undercoat base paper (base paper having an undercoat layer) of Example 1-1 by using a roll coater, and immediately thereafter, it was pressed against a mirror surface drum having a surface temperature of 60 ° C., dried, and then separated. The mold was cast to obtain a cast coated paper for inkjet recording. The cast coating amount at this time was 2 g / m 2 in terms of solid content weight.
【0055】実施例1−3 実施例1−1において、鏡面ドラムの表面温度を50℃
とした他は実施例1−1と同じ方法でインクジェット用
キャスト塗被紙を得た。Example 1-3 In Example 1-1, the surface temperature of the mirror surface drum was 50 ° C.
A cast coated paper for inkjet was obtained by the same method as in Example 1-1, except that.
【0056】実施例1−4 キャスト塗被液として、ガラス転移点45℃のアクリル
酸エステル重合体100部、離型剤としてステアリン酸
カルシウム5部よりなる固形分濃度が40%の塗被液を
調製した。この塗被液を実施例1−1で使用した下塗り
原紙と同一の原紙上にロールコーターを用いて塗被した
後、ただちに表面温度が40℃の鏡面ドラムに圧接、乾
燥後、離型させてインクジェット記録用キャスト塗被紙
を得た。この時のキャスト塗被量は固形分重量で3g/
m2 であった。Examples 1-4 As a cast coating liquid, a coating liquid having 100% of an acrylic ester polymer having a glass transition point of 45 ° C. and 5 parts of calcium stearate as a release agent and having a solid content of 40% was prepared. did. This coating liquid was coated on the same base paper as the base paper used in Example 1-1 by using a roll coater, and immediately thereafter, it was pressed against a mirror surface drum having a surface temperature of 40 ° C., dried, and then released. A cast coated paper for inkjet recording was obtained. The amount of cast coating at this time was 3 g / solid weight.
It was m 2 .
【0057】実施例1−5 キャスト塗被液として、ガラス転移点95℃のスチレン
−メチルアクリレート共重合体とコロイダルシリカの複
合体100部、離型剤としてオレイン酸アンモニウム5
部よりなる固形分濃度が35%の塗被液を調製した。こ
の塗被液を実施例1−1で使用した下塗り原紙と同一の
原紙上にロールコーターを用いて塗被した後、ただちに
表面温度が90℃の鏡面ドラムに圧接、乾燥後、離型さ
せてインクジェット記録用キャスト塗被紙を得た。この
時のキャスト塗被量は固形分重量で2g/m2 であっ
た。Example 1-5 100 parts of a composite of a styrene-methyl acrylate copolymer having a glass transition point of 95 ° C. and colloidal silica as a cast coating liquid, and ammonium oleate 5 as a release agent
A coating liquid having a solid content concentration of 35% was prepared. This coating liquid was applied onto the same base paper as the base paper used in Example 1-1 by using a roll coater, immediately followed by pressure contact with a mirror surface drum having a surface temperature of 90 ° C., drying, and release. A cast coated paper for inkjet recording was obtained. At this time, the cast coating amount was 2 g / m 2 in terms of solid content weight.
【0058】実施例1−6 顔料としてカオリン40部、軽質炭酸カルシウム30
部、および重質炭酸カルシウム30部を使用し、接着剤
として澱粉5部、スチレン−ブタジエン共重合体ラテッ
クス10部、カチオン樹脂として4級アンモニウム塩含
有アクリル系樹脂5部、分散剤としてポリ燐酸ソーダ
0.5部を添加し、固形分濃度が55%の下塗り用塗被
液を調製した。この塗被液を、米坪60g/m2 の原紙
に乾燥重量で20g/m2 になるように、ブレードコー
ターで塗被、乾燥して下塗り原紙を得た。この下塗り原
紙の透気度をガーレー高圧型透気度試験機で測定したと
ころ、50秒/10ccであった。この下塗り原紙上に
実施例1−1で用いたキャスト塗被液と同じものを用
い、実施例1−1と同じようにしてインクジェット記録
用キャスト塗被紙を得た。Example 1-6 40 parts of kaolin as a pigment, 30 parts of light calcium carbonate
Parts, and 30 parts of heavy calcium carbonate, 5 parts of starch as an adhesive, 10 parts of styrene-butadiene copolymer latex, 5 parts of a quaternary ammonium salt-containing acrylic resin as a cationic resin, and sodium polyphosphate as a dispersant. 0.5 part was added to prepare an undercoat coating liquid having a solid content concentration of 55%. This coating liquid was applied to a base paper having a basis weight of 60 g / m 2 by a blade coater so as to have a dry weight of 20 g / m 2 , and dried to obtain an undercoat base paper. The air permeability of this base paper was 50 seconds / 10 cc when measured with a Gurley high pressure type air permeability tester. On this undercoat base paper, the same cast coating liquid as used in Example 1-1 was used, and a cast coated paper for inkjet recording was obtained in the same manner as in Example 1-1.
【0059】実施例1−7 実施例1−1において、鏡面ドラムの温度を90℃とし
た以外は、実施例1−1と同じ方法で、インクジェット
記録用キャスト塗被紙を得た。Example 1-7 An ink jet recording cast coated paper was obtained in the same manner as in Example 1-1, except that the temperature of the mirror surface drum was changed to 90 ° C.
【0060】実施例1−8 実施例1−2において、鏡面ドラムの温度を80℃とし
た以外は、実施例1−2と同じ方法で、インクジェット
記録用キャスト塗被紙を得た。Example 1-8 An ink jet recording cast coated paper was obtained in the same manner as in Example 1-2, except that the temperature of the mirror surface drum was changed to 80 ° C.
【0061】比較例1−1 キャスト塗被液として、ガラス転移点が0℃のスチレン
−ブタジエン共重合体を100部、離型剤としてステア
リン酸カルシウム10部よりなる固形分濃度が40%の
塗被液を調製した。このキャスト塗被液を実施例1−1
と同じ下塗り原紙上にロールコーターを用いて塗被した
後、ただちに表面温度が60℃の鏡面ドラムに圧接し、
乾燥後、離型させ、インクジェット記録用キャスト塗被
紙を得た。この時のキャスト塗被量は固形分重量で、2
g/m2 であった。Comparative Example 1-1 100 parts of a styrene-butadiene copolymer having a glass transition point of 0 ° C. as a cast coating liquid and 10 parts of calcium stearate as a release agent, a coating having a solid content concentration of 40%. A liquid was prepared. This cast coating liquid was used in Example 1-1.
After coating with a roll coater on the same undercoat base paper as above, immediately press the surface of the mirror drum with a surface temperature of 60 ℃,
After drying, the mold was released to obtain a cast coated paper for inkjet recording. At this time, the cast coating amount is 2 by solid weight.
It was g / m 2 .
【0062】比較例1−2 顔料として、カオリン50部、重質炭酸カルシウム50
部、接着剤として、酸化澱粉5部、スチレン−ブタジエ
ン共重合体ラテックス12部、分散剤として、ポリアク
リル酸ソーダ0.5部を添加し、固形分濃度60%の下
塗り用塗被液を調製した。この塗被液を、米坪60g/
m2 の原紙に乾燥重量が20g/m2 になるように、ブ
レードコーターで塗被、乾燥して下塗り原紙を得た。こ
の下塗り原紙のガーレー高圧型透気度試験機で、100
秒/10ccであった。一方、キャスト塗被液として、
カオリン100部、カゼイン10部、スチレン−ブタジ
エン共重合体(ガラス転移点10℃)10部、離型剤と
してステアリン酸カルシウム10部よりなる固形分濃度
が45%の塗被液を調製した。このキャスト塗被液を上
記の下塗り原紙上にロールコーターを用いて塗被した
後、ただちに表面温度が75℃の鏡面ドラムに圧接し、
乾燥後、離型させ、インクジェット記録用キャスト塗被
紙を得た。この時のキャスト塗被量は固形分重量で、1
5g/m2 であった。Comparative Example 1-2 As the pigment, 50 parts of kaolin and 50 parts of heavy calcium carbonate were used.
Parts, 5 parts of oxidized starch, 12 parts of styrene-butadiene copolymer latex as an adhesive, and 0.5 parts of sodium polyacrylate as a dispersant are added to prepare a coating liquid for undercoating having a solid content concentration of 60%. did. This coating liquid, 60 g / tsubo
As the base paper on the dry weight of m 2 is 20 g / m 2, coated with a blade coater and dried to obtain an undercoat base paper. The Gurley high pressure type air permeability tester for this undercoat base paper
It was seconds / 10 cc. On the other hand, as a cast coating liquid,
A coating liquid having a solid content concentration of 45% was prepared, which consisted of 100 parts of kaolin, 10 parts of casein, 10 parts of a styrene-butadiene copolymer (glass transition temperature 10 ° C.), and 10 parts of calcium stearate as a release agent. This cast coating liquid was applied onto the above-mentioned undercoat base paper using a roll coater, and immediately thereafter, it was pressed against a mirror surface drum having a surface temperature of 75 ° C.,
After drying, the mold was released to obtain a cast coated paper for inkjet recording. At this time, the cast coating amount was 1 by weight of the solid content.
It was 5 g / m 2 .
【0063】このようにして得られたキャスト塗被紙の
白紙光沢、インクジェットプリンタ記録適性、操業性の
結果を表1に示した。なお、上記の評価については下記
の如き方法で評価を行った。Table 1 shows the results of the white gloss, the ink jet printer recording suitability and the operability of the cast coated paper thus obtained. The above evaluation was carried out by the following method.
【0064】〔白紙光沢〕JIS−P8142に準じて
測定した。[Glossiness of White Paper] It was measured according to JIS-P8142.
【0065】〔インクジェットプリンタ記録適性/イン
キ吸収性〕シャープ(株)製カラーイメージジェットI
O−735X(インクジェットプリンタ)を用いて印字
を行い、インクの乾燥性を目視で評価した。 ◎:印字直後に指で触れても全く汚れない。 ○:印字直後に指で触れると僅かに汚れるが、ほとんど
乾燥している。 △:印字直後、インク部分がわずかに光っているが、実
用上問題はない。 ×:インクの乾燥不良のため、印字中にインクが流れて
実用的でない。[Inkjet printer recording suitability / ink absorption] Color Image Jet I manufactured by Sharp Corporation
Printing was performed using O-735X (inkjet printer), and the drying property of the ink was visually evaluated. ⊚: There is no stain even if touched with a finger immediately after printing. ◯: Slightly soiled when touched with a finger immediately after printing, but almost dry. Δ: The ink portion is slightly shiny immediately after printing, but there is no problem in practical use. X: Ink is not practical because the ink flows during printing due to poor drying of the ink.
【0066】〔キャスト操業性〕 ○:問題なく操業できた。 △:低速操業となったが、実用上問題なし。 ×:離型性不良により、ドラムピック発生。[Cast operability] ◯: Operation was possible without problems. Δ: The operation was performed at a low speed, but there was no practical problem. X: Drum pick occurs due to poor releasability.
【0067】[0067]
【表1】 [Table 1]
【0068】実施例2−1 顔料として無定形シリカ90部、軽質炭酸カルシウム1
0部、接着剤として、ポリビニルアルコール20部、カ
チオン性樹脂としてジシアンジアミドとホルマリンの縮
合物であるジシアンジアミド系樹脂(商品名:ネオフィ
ックスFY/日華化学工業(株)製)10部、分散剤と
して、ポリ燐酸ソーダ0.5部を添加し、固形分濃度1
5%の下塗り用塗被液を調成した。この下塗り用塗被液
を、米坪100g/m2 の原紙に乾燥重量で12g/m
2 になるように、エアーナイフコーターで塗被、乾燥し
て下塗り原紙を得た。ガーレー高圧型透気度試験機によ
る透気度は4秒/10ccである。Example 2-1 90 parts of amorphous silica as pigment, 1 light calcium carbonate
0 part, 20 parts of polyvinyl alcohol as an adhesive, 10 parts of dicyandiamide-based resin (trade name: Neofix FY / produced by Nika Chemical Industry Co., Ltd.) which is a condensate of dicyandiamide and formalin as a cationic resin, and a dispersant , 0.5 parts of sodium polyphosphate was added to give a solid content of 1
A 5% undercoat coating solution was prepared. 12 g / m 2 dry weight of this undercoat coating liquid on 100 g / m 2 of base paper.
2 was coated with an air knife coater and dried to obtain an undercoat base paper. The air permeability measured by the Gurley high pressure type air permeability tester is 4 seconds / 10 cc.
【0069】一方、キャスト塗被液として、ガラス転移
点80℃のスチレン−2メチルヘキシルアクリレート共
重合体40部、コロイダルシリカ60部、離型剤として
ステアリン酸カルシウム2部よりなる固形分濃度が30
%のキャスト用塗被液を調製した。この塗被液を上記の
下塗り原紙上にロールコーターを用いて塗被した後、た
だちに表面温度が85℃の鏡面ドラムに圧接し、乾燥
後、離型させ、インクジェット記録用キャスト塗被紙を
得た。このときの塗被量は固形分重量で、5g/m2 で
あった。このキャスト塗被紙の透気度(JIS−P−8
117)は、120秒/100ccであった。On the other hand, the cast coating liquid comprises 40 parts of a styrene-2 methylhexyl acrylate copolymer having a glass transition point of 80 ° C., 60 parts of colloidal silica, and 2 parts of calcium stearate as a release agent, which has a solid content concentration of 30.
% Coating solution for casting was prepared. This coating liquid was coated on the above-mentioned undercoat base paper using a roll coater, immediately followed by pressure contact with a mirror surface drum having a surface temperature of 85 ° C., drying and release to obtain a cast coated paper for inkjet recording. It was The coating amount at this time was 5 g / m 2 in terms of solid content weight. Air permeability of this cast coated paper (JIS-P-8
117) was 120 seconds / 100 cc.
【0070】実施例2−2 実施例2−1において、キャスト塗被紙を得るに当た
り、鏡面ドラムの表面温度を85℃から70℃に変更し
た以外は、実施例2−1と同様にしてインクジェット記
録用キャスト塗被紙を得た。このキャスト塗被紙の透気
度は、80秒/100ccであった。Example 2-2 Ink jetting was carried out in the same manner as in Example 2-1 except that the surface temperature of the mirror surface drum was changed from 85 ° C. to 70 ° C. to obtain the cast coated paper in Example 2-1. A cast coated paper for recording was obtained. The cast coated paper had an air permeability of 80 seconds / 100 cc.
【0071】実施例2−3 キャスト塗被液としてガラス転移点が50℃のスチレン
−メチルアクリレート共重合体100部、離型剤として
オレイン酸アンモニウム5部よりなる固形分濃度が35
%のキャスト用塗被液を調製した。この塗被液を実施例
2−1で得た下塗り原紙上にロールコーターを用いて塗
被した後、ただちに表面温度が60℃の鏡面ドラムに圧
接し、乾燥後、離型させ、インクジェット記録用キャス
ト塗被紙を得た。このときの塗被量は固形分重量で、1
g/m2 であった。このキャスト塗被紙の透気度は、1
00秒/100ccであった。Example 2-3 100 parts of a styrene-methyl acrylate copolymer having a glass transition point of 50 ° C. as a cast coating liquid, and 5 parts of ammonium oleate as a releasing agent have a solid content concentration of 35.
% Coating solution for casting was prepared. This coating liquid was applied on the base paper for undercoat obtained in Example 2-1 using a roll coater, and immediately thereafter, it was pressed against a mirror surface drum having a surface temperature of 60 ° C., dried, and then released for inkjet recording. A cast coated paper was obtained. The coating amount at this time is 1 by weight of the solid content.
It was g / m 2 . The air permeability of this cast coated paper is 1
It was 00 seconds / 100 cc.
【0072】実施例2−4 キャスト塗被液として、ガラス転移点70℃のスチレン
−メチルアクリレート共重合体とコロイダルシリカの複
合体100部、離型剤としてオレイン酸アンモニウム3
部よりなる固形分濃度が40%のキャスト用塗被液を調
製した。この塗被液を実施例2−1で得た下塗り原紙上
にロールコーターを用いて塗被した後、ただちに表面温
度が65℃である加熱鏡面ドラムに圧接し、乾燥後、離
型させ、インクジェット記録用キャスト塗被紙を得た。
このときの塗被量は固形分重量で、6g/m2 であっ
た。このキャスト塗被紙の透気度は、75秒/100c
cであった。Example 2-4 100 parts of a composite of a styrene-methyl acrylate copolymer having a glass transition point of 70 ° C. and colloidal silica as a cast coating liquid, and ammonium oleate 3 as a releasing agent.
A coating liquid for casting having a solid content concentration of 40% was prepared. This coating liquid was applied onto the base paper for undercoat obtained in Example 2-1 by using a roll coater, and immediately thereafter, it was pressed against a heating mirror surface drum having a surface temperature of 65 ° C., dried, and then released from the mold to form an inkjet. A cast coated paper for recording was obtained.
The coating amount at this time was 6 g / m 2 in terms of solid content weight. The air permeability of this cast coated paper is 75 seconds / 100c
It was c.
【0073】実施例2−5 下塗り用塗被液の顔料としてMgCO3 70部、重質炭
酸カルシウム30部、接着剤として酸化澱粉5部、スチ
レン−ブタジエン共重合体ラテックス10部、カチオン
樹脂としてジシアンジアミドとホルマリンの縮合物であ
るジシアンジアミド系樹脂(商品名:ネオフィックスF
Y/日華化学工業(株)製)5部、分散剤としてポリ燐
酸ソーダ0.4部を添加し、固形分濃度30%の下塗り
用塗被液を調成した。この下塗り用塗被液を、米坪60
g/m2 の原紙上に乾燥重量で15g/m2 になるよう
に、ブレードコーターで塗被、乾燥して下塗り原紙を得
た。ガーレー高圧型透気度試験機による透気度は10秒
/10ccである。Example 2-5 70 parts of MgCO 3 as a pigment of an undercoating liquid, 30 parts of heavy calcium carbonate, 5 parts of oxidized starch as an adhesive, 10 parts of styrene-butadiene copolymer latex, and dicyandiamide as a cationic resin. And a formalin condensate dicyandiamide resin (trade name: Neofix F
Y / Nika Kagaku Kogyo Co., Ltd. 5 parts and 0.4 parts of sodium polyphosphate as a dispersant were added to prepare an undercoating coating liquid having a solid content concentration of 30%. This undercoat coating liquid
g / m as on the second base paper become 15 g / m 2 by dry weight, coated with a blade coater and dried to obtain an undercoat base paper. The air permeability measured by the Gurley high pressure type air permeability tester is 10 seconds / 10 cc.
【0074】次いで、この下塗り原紙上に実施例2−1
で用いたキャスト用塗被液を塗被し、実施例2−1と同
様の方法でインクジェット記録用キャスト塗被紙を得
た。このキャスト塗被紙の透気度は、220秒/100
ccであった。Then, Example 2-1 was formed on this base paper.
The cast coating liquid used in 1. was applied, and a cast coated paper for inkjet recording was obtained in the same manner as in Example 2-1. The air permeability of this cast coated paper is 220 seconds / 100
It was cc.
【0075】実施例2−6 下塗り用塗被液の顔料としてAl2 O3 70部、無定形
シリカ30部、接着剤として、酸化澱粉5部、ポリビニ
ルアルコール15部、カチオン性樹脂としてポリエチレ
ンポリアミン系樹脂(商品名:ネオフィックスRP−7
0/日華化学工業(株)製)8部、分散剤としてポリ燐
酸ソーダ0.4部を添加し、固形分濃度30%の下塗り
用塗被液を調製した。この下塗り用塗被液を、米坪80
g/m2の原紙に乾燥重量で9g/m2 になるように、
ブレードコーターで塗被、乾燥して下塗り原紙を得た。
ガーレー高圧型透気度試験機による透気度は7秒/10
ccでる。この下塗り原紙上に実施例2−1で用いたキ
ャスト用塗被液を塗被し、実施例2−1と同様の方法で
インクジェット記録用キャスト塗被紙を得た。このキャ
スト塗被紙の透気度は、250秒/100ccであっ
た。Examples 2-6 70 parts of Al 2 O 3 as a pigment of the undercoating liquid, 30 parts of amorphous silica, 5 parts of oxidized starch as an adhesive, 15 parts of polyvinyl alcohol, and a polyethylene polyamine type as a cationic resin. Resin (Brand name: Neofix RP-7
0 / Nippa Kagaku Kogyo Co., Ltd. 8 parts and 0.4 parts of sodium polyphosphate as a dispersant were added to prepare an undercoating coating liquid having a solid content concentration of 30%. This undercoat coating liquid
g / m 2 of the base paper so that the dry weight becomes 9 g / m 2 .
It was coated with a blade coater and dried to obtain an undercoat base paper.
Air permeability by Gurley high pressure type air permeability tester is 7 seconds / 10
It's cc. The base coating paper was coated with the coating liquid for casting used in Example 2-1, and a cast coated paper for inkjet recording was obtained in the same manner as in Example 2-1. The cast coated paper had an air permeability of 250 seconds / 100 cc.
【0076】実施例2−7 下塗り用塗被液の顔料としてMgO80部、カオリン2
0部、接着剤としてポリビニルアルコール19部、カチ
オン性樹脂としてジアクリルアミンアクリルアミド系樹
脂(商品名:スミレーズレジン1001/住友化学工業
(株)製)8部、分散剤としてポリ燐酸ソーダ0.4部
を添加し、固形分濃度30%の下塗り用塗被液を調製し
た。この塗被液を、米坪80g/m2 の原紙上に乾燥重
量で14g/m2 となるように、ブレードコーターで塗
被、乾燥して下塗り原紙を得た。ガーレー高圧型透気度
試験機による透気度は7秒/10ccであった。この下
塗り原紙上に実施例2−1で用いたキャスト用塗被液を
塗被し、実施例2−1と同様の方法でインクジェット記
録用キャスト塗被紙を得た。このキャスト塗被紙の透気
度は、180秒/100ccであった。Examples 2-7 80 parts of MgO and 2 kaolins as pigments for the undercoating liquid
0 part, polyvinyl alcohol 19 parts as an adhesive, diacrylamine acrylamide resin (trade name: Sumirez Resin 1001 / Sumitomo Chemical Co., Ltd.) 8 parts as a cationic resin, sodium polyphosphate 0.4 as a dispersant Parts were added to prepare an undercoat coating liquid having a solid content concentration of 30%. This coating liquid was applied onto a base paper having a basis weight of 80 g / m 2 by a blade coater so as to have a dry weight of 14 g / m 2, and dried to obtain an undercoat base paper. The air permeability measured by the Gurley high pressure type air permeability tester was 7 seconds / 10 cc. The base coating paper was coated with the coating liquid for casting used in Example 2-1, and a cast coated paper for inkjet recording was obtained in the same manner as in Example 2-1. The cast coated paper had an air permeability of 180 seconds / 100 cc.
【0077】実施例2−8 酸化アルミニウム(アルミナ)80部、無定形シリカ2
0部、ポリビニルアルコール15部、ポリ燐酸ソーダ1
部を添加し、固形分濃度20%の下塗り用塗被液を調成
した。この下塗り用塗被液を、米坪100g/m2 の原
紙に乾燥重量で12g/m2 になるように、エアーナイ
フコーターで塗被、乾燥して下塗り原紙を得た。 ガー
レー高圧型透気度試験機による透気度は15秒/10c
cである。Example 2-8 80 parts of aluminum oxide (alumina), amorphous silica 2
0 parts, polyvinyl alcohol 15 parts, sodium polyphosphate 1
Parts were added to prepare an undercoat coating liquid having a solid content concentration of 20%. This undercoating coating liquid was applied to a base paper having a basis weight of 100 g / m 2 with a dry weight of 12 g / m 2 by an air knife coater and dried to obtain an undercoat base paper. Air permeability by Gurley high pressure type air permeability tester is 15 seconds / 10c
c.
【0078】一方、キャスト塗被液として、ガラス転移
点80℃のスチレン−2メチルヘキシルアクリレート共
重合体50部、コロイダルシリカ50部、離型剤として
ステアリン酸カルシウム2部よりなる固形分濃度が30
%のキャスト用塗被液を調製した。この塗被液を上記の
下塗り原紙上にロールコーターを用いて塗被した後、た
だちに表面温度が85℃の鏡面ドラムに圧接し、乾燥
後、離型させ、インクジェット記録用キャスト塗被紙を
得た。このときの塗被量は固形分重量で、6g/m2 で
あった。このキャスト塗被紙の透気度(JIS−P−8
117)は、400秒/100ccであった。On the other hand, as a cast coating liquid, 50 parts of a styrene-2 methylhexyl acrylate copolymer having a glass transition point of 80 ° C., 50 parts of colloidal silica, and 2 parts of calcium stearate as a release agent have a solid content concentration of 30.
% Coating solution for casting was prepared. This coating liquid was coated on the above-mentioned undercoat base paper using a roll coater, immediately followed by pressure contact with a mirror surface drum having a surface temperature of 85 ° C., drying and release to obtain a cast coated paper for inkjet recording. It was The coating amount at this time was 6 g / m 2 in terms of solid content weight. Air permeability of this cast coated paper (JIS-P-8
117) was 400 seconds / 100 cc.
【0079】実施例2−9 顔料として無定形シリカ100部、接着剤としてポリビ
ニルアルコール15部、分散剤としてポリ燐酸ソーダ
1.0部を添加し、固形分濃度15%の下塗り用塗被液
を調成した。この下塗り用塗被液を、米坪100g/m
2 の原紙に乾燥重量で6g/m2 になるように、エアー
ナイフコーターで塗被、乾燥して下塗り原紙を得た。ガ
ーレー高圧型透気度試験機による透気度は4秒/10c
cである。Example 2-9 100 parts of amorphous silica as a pigment, 15 parts of polyvinyl alcohol as an adhesive, and 1.0 part of sodium polyphosphate as a dispersant were added to prepare an undercoating coating solution having a solid content of 15%. It was prepared. This undercoat coating liquid, 100 g / m 2
Such that the 6 g / m 2 by dry weight to 2 of the base paper, coated with an air knife coater and dried to obtain an undercoat base paper. Air permeability by Gurley high pressure type air permeability tester is 4 seconds / 10c
c.
【0080】一方、キャスト塗被液として、ガラス転移
点80℃のスチレン−2メチルヘキシルアクリレート共
重合体50部、コロイダルシリカ50部、離型剤として
ステアリン酸カルシウム2部よりなる固形分濃度が30
%のキャスト用塗被液を調製した。この塗被液を上記の
下塗り原紙上にロールコーターを用いて塗被した後、た
だちに表面温度が85℃の鏡面ドラムに圧接し、乾燥
後、離型させ、インクジェット記録用キャスト塗被紙を
得た。このときの塗被量は固形分重量で、6g/m2 で
あった。このキャスト塗被紙の透気度(JIS−P−8
117)は、100秒/100ccであった。On the other hand, as a cast coating liquid, 50 parts of styrene-2 methylhexyl acrylate copolymer having a glass transition point of 80 ° C., 50 parts of colloidal silica, and 2 parts of calcium stearate as a releasing agent have a solid content concentration of 30.
% Coating solution for casting was prepared. This coating liquid was coated on the above-mentioned undercoat base paper using a roll coater, immediately followed by pressure contact with a mirror surface drum having a surface temperature of 85 ° C., drying and release to obtain a cast coated paper for inkjet recording. It was The coating amount at this time was 6 g / m 2 in terms of solid content weight. Air permeability of this cast coated paper (JIS-P-8
117) was 100 seconds / 100 cc.
【0081】比較例2−1 キャスト塗被液としてガラス転移点0℃のスチレン−2
メチルヘキシルアクリレート共重合体40部、コロイダ
ルシリカ60部、離型剤としてオレイン酸アンモニウム
5部よりなる固形分濃度が35%のキャスト用塗被液を
調製した。この塗被液を実施例2−1で得た下塗り原紙
上にロールコーターを用いて塗被した後、ただちに表面
温度が60℃の鏡面ドラムに圧接し、乾燥後、離型さ
せ、インクジェット記録用キャスト塗被紙を得た。この
ときの塗被量は固形分重量で、5g/m2 であった。こ
のキャスト塗被紙の透気度は、450秒/100ccで
あった。Comparative Example 2-1 Styrene-2 having a glass transition point of 0 ° C. as a cast coating liquid
A coating liquid for casting having a solid content concentration of 35% was prepared, which was composed of 40 parts of methylhexyl acrylate copolymer, 60 parts of colloidal silica, and 5 parts of ammonium oleate as a release agent. This coating liquid was applied on the base paper for undercoat obtained in Example 2-1 using a roll coater, and immediately thereafter, it was pressed against a mirror surface drum having a surface temperature of 60 ° C., dried, and then released for inkjet recording. A cast coated paper was obtained. The coating amount at this time was 5 g / m 2 in terms of solid content weight. The cast coated paper had an air permeability of 450 seconds / 100 cc.
【0082】比較例2−2 キャスト塗被液としてガラス転移点30℃のスチレン−
ブタジエン共重合体100部、離型剤としてオレイン酸
アンモニウム5部よりなる固形分濃度が35%のキャス
ト用塗被液を調製した。この塗被液を実施例2−1で得
た下塗り原紙上にロールコーターを用いて塗被した後、
ただちに表面温度が80℃の鏡面ドラムに圧接し、乾燥
後、離型させ、インクジェット記録用キャスト塗被紙を
得た。このときの塗被量は固形分重量で、5g/m2 で
あった。このキャスト塗被紙の透気度は、1300秒/
100ccであった。Comparative Example 2-2 Styrene having a glass transition point of 30 ° C. as a cast coating liquid
A coating liquid for casting having a solid content concentration of 35% was prepared, which was composed of 100 parts of a butadiene copolymer and 5 parts of ammonium oleate as a release agent. After this coating liquid was coated on the base paper for undercoat obtained in Example 2-1, using a roll coater,
Immediately, it was pressed against a mirror surface drum having a surface temperature of 80 ° C., dried, and released to obtain a cast coated paper for inkjet recording. The coating amount at this time was 5 g / m 2 in terms of solid content weight. The air permeability of this cast coated paper is 1300 seconds /
It was 100 cc.
【0083】比較例2−3 キャスト塗被液としてガラス転移点0℃のスチレン−ブ
タジエン共重合体100部、離型剤としてオレイン酸ア
ンモニウム5部よりなる固形分濃度が35%のキャスト
用塗被液を調製した。この塗被液を実施例2−1で得た
下塗り原紙上にロールコーターを用いて塗被した後、た
だちに表面温度が60℃の鏡面ドラムに圧接し、乾燥
後、離型させ、インクジェット記録用キャスト塗被紙を
得た。このときの塗被量は固形分重量で、5g/m2 で
あった。このキャスト塗被紙の透気度は、2200秒/
100ccであった。COMPARATIVE EXAMPLE 2-3 Cast coating comprising 100 parts of a styrene-butadiene copolymer having a glass transition point of 0 ° C. as a cast coating liquid and 5 parts of ammonium oleate as a releasing agent and having a solid content of 35%. A liquid was prepared. This coating liquid was applied on the base paper for undercoat obtained in Example 2-1 using a roll coater, and immediately thereafter, it was pressed against a mirror surface drum having a surface temperature of 60 ° C., dried, and then released for inkjet recording. A cast coated paper was obtained. The coating amount at this time was 5 g / m 2 in terms of solid content weight. The air permeability of this cast coated paper is 2200 seconds /
It was 100 cc.
【0084】比較例2−4 キャスト塗被液としてカオリン100部、カゼイン10
部、スチレン−メチルメタアクリレート(ガラス転移点
30℃)10部、離型剤としてステアリン酸カルシウム
10部よりなる固形分濃度が45%のキャスト用塗被液
を調製した。この塗被液を実施例2−1で得た下塗り原
紙上にロールコーターを用いて塗被した後、ただちに表
面温度が75℃の鏡面ドラムに圧接し、乾燥後、離型さ
せ、インクジェット記録用キャスト塗被紙を得た。この
ときのキャスト塗被量は固形分重量で、15g/m2 で
あった。このキャスト塗被紙の透気度は、5000秒/
100ccであった。Comparative Example 2-4 Kaolin 100 parts and casein 10 as a cast coating liquid
Part, styrene-methylmethacrylate (glass transition point 30 ° C.) 10 parts, and 10 parts of calcium stearate as a release agent, a coating liquid for casting having a solid content concentration of 45% was prepared. This coating liquid was applied onto the base paper for undercoat obtained in Example 2-1 by using a roll coater, and immediately thereafter, it was pressed against a mirror surface drum having a surface temperature of 75 ° C., dried, and then released for inkjet recording. A cast coated paper was obtained. The cast coating amount at this time was 15 g / m 2 in terms of solid content weight. The air permeability of this cast coated paper is 5000 seconds /
It was 100 cc.
【0085】比較例2−5 顔料として、カオリン50部、軽質炭酸カルシウム50
部、接着剤として酸化澱粉5部、スチレン−ブタジエン
共重合体ラテックス20部、分散剤としてポリ燐酸ソー
ダ0.5部を添加し、固形分濃度50%の下塗り用塗被
液を調製した。この下塗り用塗被液を、米坪100g/
m2 の原紙に乾燥重量が12g/m2 となるように、エ
アーナイフコーターで塗被、乾燥して下塗り原紙を得
た。ガーレー高圧型透気度試験機による透気度は200
秒/10ccであった。Comparative Example 2-5 As the pigment, 50 parts of kaolin and 50 parts of light calcium carbonate were used.
Parts, 5 parts of oxidized starch as an adhesive, 20 parts of styrene-butadiene copolymer latex, and 0.5 parts of sodium polyphosphate as a dispersant were added to prepare a coating liquid for undercoating having a solid content concentration of 50%. This undercoat coating liquid is 100 g / tsubo
As the base paper on the dry weight of m 2 is 12 g / m 2, coated with an air knife coater and dried to obtain an undercoat base paper. Gurley high pressure type air permeability tester has an air permeability of 200
It was seconds / 10 cc.
【0086】一方、比較例2−4のキャスト用塗被液
を、上記の下塗り原紙上にロールコーターを用いて塗被
した後、ただちに表面温度が85℃の鏡面ドラムに圧接
し、乾燥後、離型させ、インクジェット記録用キャスト
塗被紙を得た。このときの塗被量は固形分重量で、15
g/m2 であった。このキャスト塗被紙の透気度は、1
0000秒/100ccであった。On the other hand, the casting coating liquid of Comparative Example 2-4 was applied onto the above-mentioned undercoat base paper using a roll coater, and immediately thereafter, it was pressed against a mirror surface drum having a surface temperature of 85 ° C. and dried, The mold was released to obtain a cast coated paper for inkjet recording. The coating amount at this time is 15% by weight of solid content.
It was g / m 2 . The air permeability of this cast coated paper is 1
It was 0000 seconds / 100 cc.
【0087】このようにして得られたキャスト塗被紙の
白紙光沢、インクジェット記録適性、および操業性の結
果を表2に纏めて示した。なお、上記の評価については
下記の如き方法で評価を行った。The results of white gloss, ink jet recording suitability and operability of the cast coated paper thus obtained are summarized in Table 2. The above evaluation was carried out by the following method.
【0088】〔白紙光沢〕JIS−P8142に準じて
測定した。[Glossiness of White Paper] It was measured according to JIS-P8142.
【0089】〔インクジェット記録適性〕 (インクジェット記録用インクの吸収性)シャープ
(株)製のカラーイメージジェットIO−735X(イ
ンクジェット記録用装置)にて印字を行ない、インキの
乾燥性を目視で評価した。 ◎:印字直後に指で触れてもまったく汚れない。 ○:印字直後に指で触れると僅かに汚れるが、ほとんど
乾燥している。 △:印字直後、インク部分がわずかに光っているが、実
用上問題はない。 △’:印字直後、インク部分が光っているが、約10秒
後には乾燥し、インク量の少ない図柄では実用上問題の
ないレベル。 ×:インクの乾燥不良により、印字中にインクが流れて
実用に耐えない。[Inkjet Recording Suitability] (Absorbability of Inkjet Recording Ink) Printing was performed with Color Image Jet IO-735X (inkjet recording apparatus) manufactured by Sharp Corporation, and the drying property of the ink was visually evaluated. . ⊚: No stain at all when touched with a finger immediately after printing. ◯: Slightly soiled when touched with a finger immediately after printing, but almost dry. Δ: The ink portion is slightly shiny immediately after printing, but there is no problem in practical use. Δ ': The ink portion is shining immediately after printing, but it is dried after about 10 seconds, and there is no problem in practical use for a pattern with a small amount of ink. X: Due to poor drying of the ink, the ink flows during printing and cannot be used practically.
【0090】(インクジェット記録用インクの記録後の
発色性)シャープ(株)製のカラーイメージジェットI
O−735Xにて印字を行ない、インクの濃度を目視で
評価した。 ○:発色濃度が良好である。 △:発色濃度がやや薄いが実用上問題のないレベルであ
る。 ×:発色濃度が薄く実用に耐えない。(Coloring property of ink jet recording ink after recording) Color Image Jet I manufactured by Sharp Corporation
Printing was performed with O-735X, and the density of the ink was visually evaluated. ◯: Color density is good. Δ: The color density is slightly low, but there is no practical problem. X: The color density is too low to be practical.
【0091】〔キャスト操業性〕 ○:問題なく操業できた。 △:低スピードではあるが、操業可能なレベル。 ×:離型性不良により、ドラムピックが発生し、操業不
可。[Cast operability] ◯: Operation was possible without problems. △: Low speed but at a level at which operation is possible. ×: Drum pick occurs due to poor releasability and operation is impossible.
【0092】[0092]
【表2】 [Table 2]
【0093】水性インクに熱エネルギーを作用させてイ
ンクを吐出させるインクジェットプリンタ(BJC−8
20J:商品名、キャノン(株)製)を用いて、実施例
2−1から実施例2−9のキャスト塗被紙にインクジェ
ット記録を行ったが、表2と同様な結果が得られた。Inkjet printer (BJC-8) for ejecting ink by applying thermal energy to water-based ink
Ink jet recording was performed on the cast coated papers of Example 2-1 to Example 2-9 using 20J: trade name, manufactured by Canon Inc., and the same results as in Table 2 were obtained.
【0094】[0094]
【発明の効果】表1,表2の結果から明らかなように、
本発明のキャスト塗被紙は表面光沢度、インクジェット
記録適性に優れ、かつ効率良く生産することができた。As is clear from the results shown in Tables 1 and 2,
The cast coated paper of the present invention was excellent in surface gloss and suitability for inkjet recording, and could be efficiently produced.
【図1】インクジェット記録装置のヘッド部の縦断面
図。FIG. 1 is a vertical sectional view of a head portion of an inkjet recording apparatus.
【図2】インクジェット記録装置のヘッド部の横断面
図。FIG. 2 is a cross-sectional view of a head portion of an inkjet recording device.
【図3】図1に示したヘッドをマルチ化したヘッドの外
観斜視図。3 is an external perspective view of a head in which the head shown in FIG.
【図4】インクジェット記録装置の一例を示す斜視図。FIG. 4 is a perspective view showing an example of an inkjet recording apparatus.
13 : ヘッド 14 : インクを通す溝 15 : 発熱ヘッド 16 : 保護膜 17−1: アルミニウム電極 17−2: アルミニウム電極 18 : 発熱抵抗体層 19 : 蓄熱層 20 : 基板 21 : インク 22 : オリフィス 23 : メニスカス 24 : 記録小滴 25 : 記録シート 26 : マルチ溝 27 : ガラス板 28 : 発熱ヘッド 51 : 給紙部 52 : 紙送りローラー 53 : 排紙ローラー 61 : ブレード 62 : キャップ 63 : インク吸収体 64 : 吐出回復部 65 : 記録ヘッド 66 : キャリッジ 67 : ガイド軸 68 : モ−ター 69 : ベルト 13: Head 14: Groove through which ink is passed 15: Heating head 16: Protective film 17-1: Aluminum electrode 17-2: Aluminum electrode 18: Heating resistor layer 19: Heat storage layer 20: Substrate 21: Ink 22: Orifice 23: Meniscus 24: Recording small droplet 25: Recording sheet 26: Multi-groove 27: Glass plate 28: Heating head 51: Paper feeding section 52: Paper feeding roller 53: Paper discharging roller 61: Blade 62: Cap 63: Ink absorber 64: Discharge recovery unit 65: Recording head 66: Carriage 67: Guide shaft 68: Motor 69: Belt
───────────────────────────────────────────────────── フロントページの続き (72)発明者 近藤 博雅 兵庫県尼崎市常光寺4丁目3番1号 新王 子製紙株式会社神崎工場内 (72)発明者 野島 一博 兵庫県尼崎市常光寺4丁目3番1号 新王 子製紙株式会社神崎工場内 (72)発明者 今別府 勝善 兵庫県尼崎市常光寺4丁目3番1号 新王 子製紙株式会社神崎工場内 ─────────────────────────────────────────────────── ─── Continuation of the front page (72) Inventor Hiromasa Kondo 4-3-1, Jokoji, Amagasaki City, Hyogo Prefecture Shinko Paper Manufacturing Co., Ltd. Kanzaki Mill (72) Inventor Kazuhiro Nojima 4-chome, Jokoji Temple, Amagasaki City, Hyogo Prefecture No. 1 Shin-Oji Paper Co., Ltd. Kanzaki Mill (72) Inventor Katsuyoshi Imabefu 4-3-1, Jokoji, Amagasaki City, Hyogo Prefecture Shin-Oji Paper Mill Kanzaki Mill
Claims (14)
層を設けた原紙上に、エチレン性不飽和結合を有するモ
ノマーを重合させてなる40℃以上のガラス転移点を有
する重合体を含有する塗被液を塗被してキャスト用塗被
層を形成せしめ、該キャスト用塗被層が湿潤状態にある
間に、加熱された鏡面ドラムに圧接、乾燥して仕上げる
インクジェット記録用キャスト塗被紙の製造方法。1. A polymer having a glass transition point of 40 ° C. or higher, which is obtained by polymerizing a monomer having an ethylenically unsaturated bond, on a base paper provided with an undercoat coating layer containing a pigment and an adhesive. A cast coated paper for ink jet recording, which is formed by applying a coating liquid to form a cast coating layer, and while the cast coating layer is in a wet state, press-contacts a heated mirror surface drum and finishes by drying. Manufacturing method.
転移点未満として乾燥仕上げする請求項1記載のインク
ジェット記録用キャスト塗被紙の製造方法。2. The method for producing cast coated paper for ink-jet recording according to claim 1, wherein the mirror-finished drum surface is dried to a temperature below the glass transition point of the polymer.
−8117)300秒/100cc以下とすることを特
徴とする請求項1または2記載のインクジェット記録用
キャスト塗被紙の製造方法。3. The air permeability of the cast coated paper is defined by (JIS-P
-8117) 300 seconds / 100 cc or less, The manufacturing method of the cast coated paper for inkjet recording of Claim 1 or 2 characterized by the above-mentioned.
せしめた請求項1,2,または3記載のインクジェット
記録用キャスト塗被紙の製造方法。4. The method for producing a cast coated paper for ink jet recording according to claim 1, 2 or 3, wherein a cationic resin is contained in the undercoat coated layer.
層を設けた原紙上に、エチレン性不飽和結合を有するモ
ノマーを重合させてなる40℃以上のガラス転移点を有
する重合体を含有する塗被液を塗被してキャスト用塗被
層を形成せしめ、該キャスト用塗被層が湿潤状態にある
間に、加熱された鏡面ドラムに圧接、乾燥して仕上げて
なるインクジェット記録用キャスト塗被紙。5. A polymer having a glass transition point of 40 ° C. or higher, which is obtained by polymerizing a monomer having an ethylenically unsaturated bond, on a base paper provided with an undercoat coating layer containing a pigment and an adhesive. A cast coating for inkjet recording, which is formed by applying a coating liquid to form a coating layer for casting, and pressing and drying the coating layer for heating while the coating layer for casting is in a wet state and drying. Paper.
−8117)300秒/100cc以下であることを特
徴とする請求項5記載のインクジェット記録用キャスト
塗被紙。6. The air permeability of the cast coated paper is (JIS-P
-8117) 300 sec / 100 cc or less, The cast coated paper for inkjet recording according to claim 5.
せしめた請求項5または6記載のインクジェット記録用
キャスト塗被紙。7. The cast coated paper for ink jet recording according to claim 5, wherein a cationic resin is contained in the undercoat coated layer.
転移点未満として乾燥仕上げしてなる請求項5,6,ま
たは7記載のインクジェット記録用キャスト塗被紙。8. The cast coated paper for ink jet recording according to claim 5, 6, or 7, which is dried and finished with the temperature of the surface of the mirror surface drum being lower than the glass transition point of the polymer.
を設けた原紙上に、エチレン性不飽和結合を有するモノ
マーを重合させてなる40℃以上のガラス転移点を有す
る重合体を含有する表面塗被層を設けてなるインクジェ
ット記録用強光沢紙に対して、微細孔から水性インクを
吐出させて画像を形成することを特徴とするインクジェ
ット記録方法。9. A polymer having a glass transition point of 40 ° C. or higher, which is obtained by polymerizing a monomer having an ethylenically unsaturated bond, on a base paper provided with an undercoat coating layer containing a pigment and an adhesive. An inkjet recording method, wherein an image is formed by ejecting a water-based ink from fine pores on a strong glossy paper for inkjet recording having a surface coating layer.
てインクを吐出させる請求項9記載のインクジェット記
録方法。10. The ink jet recording method according to claim 9, wherein heat energy is applied to the water-based ink to eject the ink.
0秒/100cc以下である請求項9記載のインクジェ
ット記録方法。11. An air permeability of the coated paper of the glossy paper is 30.
The ink jet recording method according to claim 9, which is 0 second / 100 cc or less.
樹脂を含有する請求項9記載のインクジェット記録方
法。12. The ink jet recording method according to claim 9, wherein the undercoat coating layer of the glossy paper contains a cationic resin.
リカを含有する請求項9記載のインクジェット記録方
法。13. The ink jet recording method according to claim 9, wherein the surface coating layer of the glossy paper contains colloidal silica.
はシリカを含有する請求項9記載のインクジェット記録
方法。14. The ink jet recording method according to claim 9, wherein the undercoat coating layer of the glossy paper contains alumina or silica.