JP6725037B1 - Pressure-sensitive adhesive layer, pressure-sensitive adhesive sheet, laminate, and method for manufacturing laminate - Google Patents
Pressure-sensitive adhesive layer, pressure-sensitive adhesive sheet, laminate, and method for manufacturing laminate Download PDFInfo
- Publication number
- JP6725037B1 JP6725037B1 JP2019091396A JP2019091396A JP6725037B1 JP 6725037 B1 JP6725037 B1 JP 6725037B1 JP 2019091396 A JP2019091396 A JP 2019091396A JP 2019091396 A JP2019091396 A JP 2019091396A JP 6725037 B1 JP6725037 B1 JP 6725037B1
- Authority
- JP
- Japan
- Prior art keywords
- pressure
- sensitive adhesive
- adhesive layer
- meth
- adhesive sheet
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Abstract
【課題】低い透湿性を有し、しかも、耐久性にも優れる粘着シートを形成することができる粘着剤層及び該粘着剤層を備える粘着シート、積層体、並びに積層体の製造方法を提供する。【解決手段】本発明の粘着剤層は、ポリオレフィンと、(メタ)アクリル系モノマーと、水素引抜型開始剤とを含有する粘着剤組成物を含み、活性エネルギー線を積算光量が3000mJ/cm2となるように照射して後硬化した場合に下記物性(1)、(2)を満たす。物性(1):引張速度10mm/minの引張試験測定において、破断伸度が1200%以上であり、かつ、ひずみ1000%での応力が0.40N/mm2以上である。物性(2):100μmの厚みでの透湿度が50g/m2・24hr以下である。【選択図】なしProvided are a pressure-sensitive adhesive layer capable of forming a pressure-sensitive adhesive sheet having low moisture permeability and excellent durability, a pressure-sensitive adhesive sheet including the pressure-sensitive adhesive layer, a laminate, and a method for producing the laminate. .. SOLUTION: The pressure-sensitive adhesive layer of the present invention contains a pressure-sensitive adhesive composition containing a polyolefin, a (meth)acrylic monomer, and a hydrogen abstraction-type initiator, and has an active energy ray accumulated light amount of 3000 mJ/cm2. The following physical properties (1) and (2) are satisfied when post-curing is performed by irradiating the above materials. Physical properties (1): In a tensile test measurement at a tensile speed of 10 mm/min, the breaking elongation is 1200% or more, and the stress at a strain of 1000% is 0.40 N/mm 2 or more. Physical property (2): Moisture permeability at a thickness of 100 μm is 50 g/m2·24 hr or less. [Selection diagram] None
Description
本発明は、粘着剤層、粘着シート及び積層体並びに積層体の製造方法に関する。 The present invention relates to a pressure-sensitive adhesive layer, a pressure-sensitive adhesive sheet, a laminate, and a method for producing a laminate.
従来、液晶表示装置等の画像表示装置においては、光学部材を貼り合せるために粘着シートが使用されている。このような画像表示装置は、水分等の影響によって品質が低下しやすくなることから、粘着シートにも水分等を透過させない特性を付与すること、つまり、低透湿性の粘着シートが求められている。 2. Description of the Related Art Conventionally, in image display devices such as liquid crystal display devices, an adhesive sheet has been used to bond optical members. Since such an image display device is liable to deteriorate in quality due to the influence of moisture or the like, it is required to provide a pressure-sensitive adhesive sheet with a property of not allowing moisture to permeate, that is, a low moisture-permeable pressure-sensitive adhesive sheet. ..
例えば、特許文献1及び2には、ポリイソブチレン、及び、水素引抜型光重合開始剤を含むゴム系粘着剤組成物を用いて低透湿性の粘着シートを得る技術が開示されている。また、特許文献3には、多分散度(重量平均分子量/数平均分子量)が4以下のイソブチレン系ポリマーを含むゴム系粘着剤組成物を用いて低透湿性の粘着シートを得る技術が開示されている。 For example, Patent Documents 1 and 2 disclose a technique of obtaining a low moisture-permeable pressure-sensitive adhesive sheet using a rubber-based pressure-sensitive adhesive composition containing polyisobutylene and a hydrogen abstraction type photopolymerization initiator. Further, Patent Document 3 discloses a technique for obtaining a low moisture-permeable pressure-sensitive adhesive sheet using a rubber-based pressure-sensitive adhesive composition containing an isobutylene-based polymer having a polydispersity (weight average molecular weight/number average molecular weight) of 4 or less. ing.
しかしながら、従来のようなゴム系粘着剤組成物を用いて得られる粘着シートは、低い透湿性を有するものの、耐久性が十分ではなく、貼り合わせ後に接着面に気泡が生じたり、あるいは、剥がれが生じたりする問題を有していた。このような観点から、画像表示装置等で使用される粘着シートにおいては、低透湿性に加えて、優れた耐久性を有することが求められていた。 However, a pressure-sensitive adhesive sheet obtained using a conventional rubber-based pressure-sensitive adhesive composition has low moisture permeability, but is not sufficiently durable, and bubbles are generated on the adhesive surface after bonding, or peeling occurs. There was a problem that occurred. From such a viewpoint, the pressure-sensitive adhesive sheet used in an image display device or the like has been required to have excellent durability in addition to low moisture permeability.
本発明は、上記に鑑みてなされたものであり、低い透湿性を有し、しかも、耐久性にも優れる粘着シートを形成することができる粘着剤層及び該粘着剤層を備える粘着シート、積層体、並びに積層体の製造方法を提供することを目的とする。 The present invention has been made in view of the above, and has a low moisture permeability, and a pressure-sensitive adhesive layer capable of forming a pressure-sensitive adhesive sheet having excellent durability, and a pressure-sensitive adhesive sheet including the pressure-sensitive adhesive layer, a laminate An object of the present invention is to provide a method for manufacturing a body and a laminated body.
本発明者らは、上記目的を達成すべく鋭意研究を重ねた結果、ポリオレフィンと(メタ)アクリル系モノマーとを含む粘着剤組成物を使用し、かつ、該粘着剤組成物の後硬化後の力学物性を特定の範囲内とすることにより、上記目的を達成できることを見出し、本発明を完成するに至った。 The present inventors have conducted extensive studies to achieve the above object, and as a result, use a pressure-sensitive adhesive composition containing a polyolefin and a (meth)acrylic monomer, and after post-curing the pressure-sensitive adhesive composition. The inventors have found that the above object can be achieved by setting the mechanical properties within a specific range, and have completed the present invention.
すなわち、本発明は、例えば、以下の項に記載の主題を包含する。
項1
ポリオレフィンと、(メタ)アクリル系モノマーと、水素引抜型開始剤とを含有する粘着剤組成物を含み、
活性エネルギー線を積算光量が3000mJ/cm2となるように照射して後硬化した場合に下記物性(1)及び(2)
物性(1):引張速度10mm/minの引張試験測定において、破断伸度が1200%以上であり、かつ、ひずみ1000%での応力が0.40N/mm2以上である、
物性(2):100μmの厚みでの透湿度が50g/m2・24hr以下である、
を満たす、粘着剤層。
項2
前記ポリオレフィンは、エチレン−プロピレン共重合体である、項1に記載の粘着剤層。
項3
前記粘着剤組成物に含まれる前記(メタ)アクリル系モノマーは、前記ポリオレフィン100質量部に対して1〜25質量部である、項1又は2に記載の粘着剤層。
項4
前記(メタ)アクリル系モノマーが、分子内に重合性官能基を2つ以上有する多官能モノマーと、分子内に重合性官能基を1つのみ有する単官能モノマーとの混合物である、項1〜3のいずれか1項に記載の粘着剤層。
項5
比誘電率が3.0以下である、項1〜4のいずれか1項に記載の粘着剤層。
項6
厚さが5〜200μmである、項1〜5のいずれか1項に記載の粘着剤層。
項7
項1〜6のいずれか1項に記載の粘着剤層を備える、粘着シート。
項8
項7に記載の粘着シート又はその硬化物を備える、積層体。
項9
項7に記載の粘着シートの少なくとも一方の面側に被着体を積層する工程、及び前記粘着シートの粘着剤層に活性エネルギー線を照射することにより前記粘着剤層を後硬化させる工程を順に有する、積層体の製造方法。
That is, the present invention includes the subject matter described in the following sections, for example.
Item 1
Including a pressure-sensitive adhesive composition containing a polyolefin, a (meth)acrylic monomer, and a hydrogen abstraction-type initiator,
The following physical properties (1) and (2) when irradiated with active energy rays so that the integrated light amount becomes 3000 mJ/cm 2 and post-cured
Physical properties (1): In a tensile test measurement at a tensile speed of 10 mm/min, a breaking elongation is 1200% or more, and a stress at a strain of 1000% is 0.40 N/mm 2 or more,
Physical properties (2): Water vapor permeability at a thickness of 100 μm is 50 g/m 2 ·24 hr or less,
Adhesive layer that fills.
Item 2
Item 2. The pressure-sensitive adhesive layer according to Item 1, wherein the polyolefin is an ethylene-propylene copolymer.
Item 3
Item 3. The pressure-sensitive adhesive layer according to Item 1 or 2, wherein the (meth)acrylic monomer contained in the pressure-sensitive adhesive composition is 1 to 25 parts by mass with respect to 100 parts by mass of the polyolefin.
Item 4
Item 1. The (meth)acrylic monomer is a mixture of a polyfunctional monomer having two or more polymerizable functional groups in the molecule and a monofunctional monomer having only one polymerizable functional group in the molecule. The pressure-sensitive adhesive layer according to any one of 3 above.
Item 5
Item 5. The pressure-sensitive adhesive layer according to any one of Items 1 to 4, which has a relative dielectric constant of 3.0 or less.
Item 6
Item 6. The pressure-sensitive adhesive layer according to any one of items 1 to 5, which has a thickness of 5 to 200 µm.
Item 7
A pressure-sensitive adhesive sheet comprising the pressure-sensitive adhesive layer according to any one of items 1 to 6.
Item 8
A laminate comprising the pressure-sensitive adhesive sheet according to item 7 or a cured product thereof.
Item 9
Item 7. The step of laminating an adherend on at least one surface side of the pressure-sensitive adhesive sheet according to item 7, and the step of post-curing the pressure-sensitive adhesive layer by irradiating the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet with active energy rays in order. A method for producing a laminated body having.
本発明に係る粘着剤層は、低い透湿性を有し、しかも、耐久性にも優れる粘着シートを形成することができる。 The pressure-sensitive adhesive layer according to the present invention can form a pressure-sensitive adhesive sheet having low moisture permeability and excellent durability.
以下、本発明の実施形態について詳細に説明する。なお、本明細書中において、「含有」及び「含む」なる表現については、「含有」、「含む」、「実質的にからなる」及び「のみからなる」という概念を含む。 Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expressions "containing" and "including" include the concepts of "containing", "including", "consisting essentially of" and "consisting only".
1.粘着剤層
本発明の粘着剤層は、ポリオレフィンと、(メタ)アクリル系モノマーと、水素引抜型開始剤とを含有する粘着剤組成物を含み、活性エネルギー線を積算光量が3000mJ/cm2となるように照射して後硬化した場合に下記物性(1)及び(2)を満たす。
物性(1):引張速度10mm/minの引張試験測定において、破断伸度が1200%以上であり、かつ、ひずみ1000%での応力が0.40N/mm2以上である。
物性(2):100μmの厚みでの透湿度が50g/m2・24hr以下である。
1. Pressure-sensitive adhesive layer The pressure-sensitive adhesive layer of the present invention contains a pressure-sensitive adhesive composition containing a polyolefin, a (meth)acrylic monomer, and a hydrogen abstraction-type initiator, and has an active energy ray accumulated light amount of 3000 mJ/cm 2 . The following physical properties (1) and (2) are satisfied when post-curing is performed by irradiating so that
Physical Properties (1): In a tensile test measurement at a tensile speed of 10 mm/min, the breaking elongation is 1200% or more, and the stress at a strain of 1000% is 0.40 N/mm 2 or more.
Physical properties (2): Water vapor permeability at a thickness of 100 μm is 50 g/m 2 ·24 hr or less.
(粘着剤組成物)
粘着剤層は、後記するように、粘着剤組成物を用いて形成することができる。当該粘着剤組成物は、少なくともポリオレフィンと、(メタ)アクリル系モノマーと、水素引抜型開始剤とを含有する。
(Adhesive composition)
The pressure-sensitive adhesive layer can be formed using a pressure-sensitive adhesive composition, as described below. The pressure-sensitive adhesive composition contains at least a polyolefin, a (meth)acrylic monomer, and a hydrogen abstraction initiator.
粘着剤組成物において、ポリオレフィンの種類は特に限定されず、例えば、公知のポリオレフィンを広く採用することができる。粘着剤組成物がポリオレフィンを含むことで、粘着剤層は物性(2)を満たすことができ、低い透湿性を有することができる。 In the pressure-sensitive adhesive composition, the type of polyolefin is not particularly limited, and, for example, known polyolefins can be widely adopted. When the pressure-sensitive adhesive composition contains polyolefin, the pressure-sensitive adhesive layer can satisfy the physical property (2) and can have low moisture permeability.
ポリオレフィンとしては、例えば、ポリエチレン、ポリプロピレン、エチレン−プロピレン共重合体等を挙げることができる。得られる粘着剤層が低い透湿性を有し、しかも、耐久性にも優れやすいという観点から、ポリオレフィンは、エチレン−プロピレン共重合体であることが好ましい。ポリオレフィンにおいて、ポリオレフィン主鎖には、本発明の効果が阻害されない限り、オレフィン以外の単量体単位を含むこともできる。 Examples of the polyolefin include polyethylene, polypropylene, ethylene-propylene copolymer and the like. The polyolefin is preferably an ethylene-propylene copolymer from the viewpoint that the obtained pressure-sensitive adhesive layer has low moisture permeability and is easily excellent in durability. In the polyolefin, the polyolefin main chain may contain a monomer unit other than the olefin as long as the effect of the present invention is not impaired.
粘着剤組成物に含まれるポリオレフィンは1種のみであってもよいし、異なる2種以上であってもよい。 The number of polyolefins contained in the pressure-sensitive adhesive composition may be only one, or may be two or more different types.
ポリオレフィンの製造方法は特に限定されず、例えば、公知の製造方法によって、ポリオレフィンを製造することができる。あるいは、ポリオレフィンは、市販品等から入手することもできる。ポリオレフィンの市販品としては、例えば、JSR社製T7241、EP33、EP35、EP331、EP342、EP251、EP65等を挙げることができる。 The method for producing the polyolefin is not particularly limited, and for example, the polyolefin can be produced by a known production method. Alternatively, the polyolefin can be obtained from a commercially available product or the like. Examples of commercially available polyolefin products include T7241, EP33, EP35, EP331, EP342, EP251 and EP65 manufactured by JSR.
粘着剤組成物に含まれる(メタ)アクリル系モノマーの種類は特に限定されず、例えば、公知の(メタ)アクリル系モノマーを広く採用することができる。なお、本明細書において、「(メタ)アクリル」とは「アクリル」または「メタクリル」を、「(メタ)アクリレート」とは「アクリレート」または「メタクリレート」を意味する。 The type of the (meth)acrylic monomer contained in the pressure-sensitive adhesive composition is not particularly limited, and for example, known (meth)acrylic monomers can be widely adopted. In addition, in this specification, "(meth)acryl" means "acryl" or "methacryl", and "(meth)acrylate" means "acrylate" or "methacrylate".
特に(メタ)アクリル系モノマーは、分子内に重合性官能基を2つ以上有する多官能モノマーと、分子内に重合性官能基を1つのみ有する単官能モノマーとの混合物であることが好ましい。この場合、得られる粘着剤層は、低い透湿性を維持しつつ、優れた耐久性を有することができる。 In particular, the (meth)acrylic monomer is preferably a mixture of a polyfunctional monomer having two or more polymerizable functional groups in the molecule and a monofunctional monomer having only one polymerizable functional group in the molecule. In this case, the obtained pressure-sensitive adhesive layer can have excellent durability while maintaining low moisture permeability.
ここで、重合性官能基とは、例えば、ラジカル重合をすることが可能な官能基を意味し、具体的には重合性二重結合であり、より具体的には重合性二重結合として(メタ)アクリロイル基を挙げることができる。 Here, the polymerizable functional group means, for example, a functional group capable of radical polymerization, specifically a polymerizable double bond, and more specifically as a polymerizable double bond ( An example is a (meth)acryloyl group.
前記多官能モノマーにおいて、分子内の重合性官能基の数は特に限定されないが、得られる粘着剤層の耐久性が優れるという点で、1分子中の重合性二重結合の数は2個以上5個以下とすることができ、2個以上3個以下とすることが好ましく、2個であることが特に好ましい。 In the polyfunctional monomer, the number of polymerizable functional groups in the molecule is not particularly limited, but the number of polymerizable double bonds in one molecule is 2 or more in terms of excellent durability of the obtained adhesive layer. The number may be 5 or less, preferably 2 or more and 3 or less, and particularly preferably 2.
前記多官能モノマーの具体例としては、ジ(メタ)アクリル酸エチレングリコール、ジ(メタ)アクリル酸トリエチレングリコール、ジ(メタ)アクリル酸1,3−ブチレングリコール、ジ(メタ)アクリル酸1,4−ブチレングリコール、ジ(メタ)アクリル酸1,9−ノナンジオール、ジアクリル酸1,6−ヘキサンジオール、ジ(メタ)アクリル酸ポリブチレングリコール、ジ(メタ)アクリル酸ネオペンチルグリコール、ジ(メタ)アクリル酸テトラエチレングリコール、ジ(メタ)アクリル酸トリプロピレングリコール、ジ(メタ)アクリル酸ポリプロピレングリコール、トリ(メタ)アクリル酸トリメチロールプロパン、トリ(メタ)アクリル酸ペンタエリスリトール、テトラ(メタ)アクリル酸ペンタエリスリトール等の多価アルコールの(メタ)アクリル酸エステル類;その他、メタクリル酸ビニル、ジメチロールトリシクロデカンジアクリレート等が挙げられる。 Specific examples of the polyfunctional monomer include ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, di(meth)acrylic acid 1, 4-butylene glycol, 1,9-nonanediol di(meth)acrylic acid, 1,6-hexanediol diacrylic acid, polybutylene glycol di(meth)acrylic acid, neopentyl glycol di(meth)acrylic acid, di(meth)acrylic acid ) Tetraethylene glycol acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tetra(meth)acrylic (Meth)acrylic acid esters of polyhydric alcohols such as acid pentaerythritol; vinyl methacrylate, dimethylol tricyclodecane diacrylate, and the like.
前記多官能モノマーとして、市販品を使用できる。市販品の多官能モノマーの例としては、ジメチロールトリシクロデカンジアクリレート(共栄社化学(株)製、ライトアクリレートDCP−A)、ビスフェノールA エチレンオキサイド変性ジアクリレート(東亞合成(株)製、アロニックスM−211B)等が挙げられる。 A commercially available product can be used as the polyfunctional monomer. Examples of commercially available polyfunctional monomers include dimethylol tricyclodecane diacrylate (Kyoeisha Chemical Co., Ltd., light acrylate DCP-A), bisphenol A ethylene oxide modified diacrylate (Toagosei Co., Ltd., Aronix M). -211B) and the like.
前記単官能モノマーは、分子内に1つのみの重合性官能基を有する。単官能モノマーの具体例としては、イソボルニル(メタ)アクリレート、イソステアリル(メタ)アクリレート、メチル(メタ)アクリレート、エチル(メタ)アクリレート、ブチル(メタ)アクリレート等のアルキル(メタ)アクリレート;その他、ベンジル(メタ)アクリレート、N−(メタ)アクリロイルオキシエチルヘキサヒドロフタルイミド、(メタ)アクリルアミド、N,N−ジメチル(メタ)アクリルアミド、N,N−ジエチル(メタ)アクリルアミド、(メタ)アクリロイルモルホリン、ビニルピロリドンなどを挙げることができる。前記単官能モノマーは、アルキル(メタ)アクリレートであることが好ましく、中でもイソボルニルアクリレート及びイソステアリルアクリレートから選択される少なくとも1種であることが好ましく、イソボルニルアクリレートであることがより好ましい。単官能モノマーの市販品の例としては、大阪有機化学工業社製のIBXA、大阪有機化学工業社製のISTA等が挙げられる。 The monofunctional monomer has only one polymerizable functional group in the molecule. Specific examples of monofunctional monomers include alkyl (meth)acrylates such as isobornyl (meth)acrylate, isostearyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate; and benzyl. (Meth)acrylate, N-(meth)acryloyloxyethylhexahydrophthalimide, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, (meth)acryloylmorpholine, vinylpyrrolidone And so on. The monofunctional monomer is preferably an alkyl(meth)acrylate, more preferably at least one selected from isobornyl acrylate and isostearyl acrylate, and more preferably isobornyl acrylate. Examples of commercially available monofunctional monomers include IBXA manufactured by Osaka Organic Chemical Industry, ISTA manufactured by Osaka Organic Chemical Industry, and the like.
前記(メタ)アクリル系モノマーが前記多官能モノマーと前記単官能モノマーとの混合物である場合、両者の混合割合は特に限定されない。例えば、前記多官能モノマー及び前記単官能モノマーの総量に対して前記多官能モノマーの含有割合を1〜99質量%とすることができ、10〜90質量%とすることが好ましく、20〜80質量%とすることがより好ましく、30〜70質量%とすることがさらに好ましく、40〜60質量%とすることが特に好ましい。 When the (meth)acrylic monomer is a mixture of the polyfunctional monomer and the monofunctional monomer, the mixing ratio of both is not particularly limited. For example, the content ratio of the polyfunctional monomer may be 1 to 99% by mass, preferably 10 to 90% by mass, and preferably 20 to 80% by mass, based on the total amount of the polyfunctional monomer and the monofunctional monomer. %, more preferably 30 to 70% by mass, particularly preferably 40 to 60% by mass.
前記(メタ)アクリル系モノマーが前記多官能モノマーと前記単官能モノマーとの混合物である場合、当該混合物は、本発明の効果が阻害されない程度であれば、その他の単量体を含むことができる。混合物がその他の単量体を含む場合、その含有量は、混合物全量に対し、10質量%とすることができ、5質量%以下とすることが好ましく、1質量%以下とすることがより好ましく、0.1質量%以下とすることが特に好ましい。 When the (meth)acrylic monomer is a mixture of the polyfunctional monomer and the monofunctional monomer, the mixture may contain other monomers as long as the effects of the present invention are not impaired. .. When the mixture contains other monomers, the content thereof may be 10% by mass, preferably 5% by mass or less, more preferably 1% by mass or less, based on the total amount of the mixture. Is particularly preferably 0.1% by mass or less.
前記粘着剤組成物に含まれる前記(メタ)アクリル系モノマーの含有量は低い透湿性が維持される限りは特に制限されない。例えば、前記粘着剤組成物に含まれる前記(メタ)アクリル系モノマーは、前記ポリオレフィン100質量部に対して1〜25質量部とすることができる。この場合、得られる粘着剤層は、性(1)及び物性(2)の両方を満たしやすく、結果として、低い透湿性を維持しつつ、優れた耐久性を有することができる。前記粘着剤組成物に含まれる前記(メタ)アクリル系モノマーの下限は、前記ポリオレフィン100質量部に対して2質量部とすることが好ましく、3質量部とすることがより好ましく、5質量部とすることが特に好ましい。前記粘着剤組成物に含まれる前記(メタ)アクリル系モノマーの上限は、前記ポリオレフィン100質量部に対して20質量部とすることが好ましく、18質量部とすることがより好ましく、15質量部とすることが特に好ましい。 The content of the (meth)acrylic monomer contained in the pressure-sensitive adhesive composition is not particularly limited as long as low moisture permeability is maintained. For example, the (meth)acrylic monomer contained in the pressure-sensitive adhesive composition may be 1 to 25 parts by mass with respect to 100 parts by mass of the polyolefin. In this case, the obtained pressure-sensitive adhesive layer can easily satisfy both the property (1) and the physical property (2), and as a result, it can have excellent durability while maintaining low moisture permeability. The lower limit of the (meth)acrylic monomer contained in the pressure-sensitive adhesive composition is preferably 2 parts by mass, more preferably 3 parts by mass, and more preferably 5 parts by mass with respect to 100 parts by mass of the polyolefin. Is particularly preferable. The upper limit of the (meth)acrylic monomer contained in the pressure-sensitive adhesive composition is preferably 20 parts by mass, more preferably 18 parts by mass, and 15 parts by mass with respect to 100 parts by mass of the polyolefin. Is particularly preferable.
粘着剤組成物に含まれる水素引抜型開始剤としては特に限定されず、例えば、公知の水素引抜型開始剤を広く使用することができる。水素引抜型光重合開始剤とは、後記する活性エネルギー線を照射することで、開始剤自身は開裂することなく、前記アクリル変性ポリオレフィン又は後記1,2−ビニル基を有するジエン系重合体より水素を引き抜き、ポリマーに反応点を作ることができる性質を有する重合開始剤をいう。当該反応点形成により、ポリマーの架橋反応が形成される。 The hydrogen abstraction type initiator contained in the pressure-sensitive adhesive composition is not particularly limited, and for example, known hydrogen abstraction type initiators can be widely used. The hydrogen abstraction type photopolymerization initiator, by irradiating with an active energy ray described below, the initiator itself is not cleaved, hydrogen from the acrylic modified polyolefin or a diene polymer having a 1,2-vinyl group described below. It is a polymerization initiator having a property of being capable of drawing out a reaction point in the polymer. Due to the formation of the reaction points, a crosslinking reaction of the polymer is formed.
水素引抜型光重合開始剤としては、例えば、ベンゾイルギ酸メチル;4−メチルベンゾフェノン、アセトフェノン、ベンゾフェノン、O−ベンゾイル安息香酸メチル−4−フェニルベンゾフェノン、4,4’−ジクロロベンゾフェノン、ヒドロキシベンゾフェノン、4,4’−ジメトキシベンゾフェノン、4,4’−ジクロルベンゾフェノン、4,4’−ジメチルベンゾフェノン、4−ベンゾイル−4’−メチル−ジフェニルサルファイド、アクリル化ベンゾフェノン、3,3’,4,4’−テトラ(t−ブチルペルオキシカルボニル)ベンゾフェノン、3,3’−ジメチル−4−メトキシベンゾフェノン等のベンゾフェノン系化合物;2−イソプロピルチオキサントン、2,4−ジメチルチオキサントン、2,4−ジエチルチオキサントン、2,4−ジクロロチオキサントン等のチオキサントン系化合物;4,4’−ビス(ジメチルアミノ)ベンゾフェノン、4,4’−ジエチルアミノベンゾフェノン等のアミノベンゾフェノン系化合物;10−ブチル−2−クロロアクリドン、2−エチルアンスラキノン、9,10−フェナンスレンキノン、カンファーキノン等;アセトナフトン、1−ヒドロキシシクロヘキシルフェニルケトン等の芳香族ケトン化合物;テレフタルアルデヒド等の芳香族アルデヒド、メチルアントラキノン等のキノン系芳香族化合物が挙げられる。これらは1種単独で、又は、2種以上を混合して用いることができる。これらの中でも、反応性の点から、ベンゾフェノン系化合物が好ましく、4−メチルベンゾフェノンがより好ましい。 Examples of the hydrogen abstraction type photopolymerization initiator include methyl benzoylformate; 4-methylbenzophenone, acetophenone, benzophenone, methyl-4-phenylbenzophenone O-benzoylbenzoate, 4,4′-dichlorobenzophenone, hydroxybenzophenone, 4, 4'-dimethoxybenzophenone, 4,4'-dichlorobenzophenone, 4,4'-dimethylbenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, acrylated benzophenone, 3,3',4,4'-tetra Benzophenone compounds such as (t-butylperoxycarbonyl)benzophenone and 3,3′-dimethyl-4-methoxybenzophenone; 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichloro. Thioxanthone compounds such as thioxanthone; 4,4′-bis(dimethylamino)benzophenone, aminobenzophenone compounds such as 4,4′-diethylaminobenzophenone; 10-butyl-2-chloroacridone, 2-ethylanthraquinone, 9 , 10-phenanthrenequinone, camphorquinone and the like; aromatic ketone compounds such as acetonaphthone and 1-hydroxycyclohexyl phenyl ketone; aromatic aldehydes such as terephthalaldehyde and quinone-based aromatic compounds such as methylanthraquinone. These may be used alone or in combination of two or more. Among these, benzophenone compounds are preferable, and 4-methylbenzophenone is more preferable, from the viewpoint of reactivity.
粘着剤組成物において、(メタ)アクリル系モノマーと水素引抜型開始剤の含有割合は特に限定されない。例えば、粘着剤組成物中、(メタ)アクリル系モノマー100質量部に対し、水素引抜型開始剤の含有量を0.05〜30質量部とすることができ、0.1〜25質量部とすることが好ましく、0.2〜20質量部とすることがより好ましい。 In the pressure-sensitive adhesive composition, the content ratios of the (meth)acrylic monomer and the hydrogen abstraction initiator are not particularly limited. For example, in the pressure-sensitive adhesive composition, the content of the hydrogen abstraction initiator can be 0.05 to 30 parts by mass, and 0.1 to 25 parts by mass with respect to 100 parts by mass of the (meth)acrylic monomer. It is preferable that the amount is 0.2 to 20 parts by mass.
粘着剤組成物は、ポリオレフィン、(メタ)アクリル系モノマー及び水素引抜型開始剤の他、その他の成分を含有することができる。例えば、粘着剤組成物は、1,2−ビニル基を有するジエン系重合体をさらに含有することもできる。 The pressure-sensitive adhesive composition may contain other components in addition to the polyolefin, the (meth)acrylic monomer and the hydrogen abstraction initiator. For example, the pressure-sensitive adhesive composition can further contain a diene polymer having a 1,2-vinyl group.
1,2−ビニル基を有するジエン系重合体としては特に限定されず、1,2−ビニル基を有する限り、公知のジエン系重合体を広く採用することができる。特に、1,2−ビニル基を有するジエン系重合体は、分子内に非共役ジエン構造を有する重合体であることが好ましい。このようなジエン系重合体としては、ポリブタジエン等を挙げることができる。1,2−ビニル基を有するジエン系重合体は共重合体であってもよく、例えば、アクリロニトリルとブタジエンの共重合体、スチレンとブタジエンの共重合体、イソプレンとブタジエンの共重合体、イソブチレンとブタジエンの共重合体等が挙げられる。 The diene polymer having a 1,2-vinyl group is not particularly limited, and known diene polymers can be widely adopted as long as they have a 1,2-vinyl group. Particularly, the diene polymer having a 1,2-vinyl group is preferably a polymer having a non-conjugated diene structure in the molecule. Examples of such a diene polymer include polybutadiene and the like. The diene-based polymer having a 1,2-vinyl group may be a copolymer, for example, a copolymer of acrylonitrile and butadiene, a copolymer of styrene and butadiene, a copolymer of isoprene and butadiene, and isobutylene. Examples thereof include a butadiene copolymer.
粘着剤組成物に含まれる1,2−ビニル基を有するジエン系重合体は1種のみであってもよいし、異なる2種以上であってもよい。 The diene-based polymer having a 1,2-vinyl group contained in the pressure-sensitive adhesive composition may be only one type, or may be two or more different types.
1,2−ビニル基を有するジエン系重合体を製造する方法は特に限定されず、例えば、公知の製造方法によって、1,2−ビニル基を有するジエン系重合体を得ることができる。あるいは、1,2−ビニル基を有するジエン系重合体は市販品等から入手することもできる。このような1,2−ビニル基を有するジエン系重合体としては、例えば、ポリブタジエンとして、TOTAL社製のRICON130、RICON131、RICON134、RICON142、RICON150、RICON152、RICON153、RICON154、RICON154、RICON156、RICON157、RICON P30D等を挙げることができる。 The method for producing the 1,2-vinyl group-containing diene polymer is not particularly limited, and for example, a 1,2-vinyl group-containing diene polymer can be obtained by a known production method. Alternatively, the diene polymer having a 1,2-vinyl group can be obtained from a commercial product or the like. Examples of such a diene polymer having a 1,2-vinyl group include, as polybutadiene, RICON130, RICON131, RICON134, RICON142, RICON150, RICON152, RICON153, RICON154, RICON154, RICON156, RICON157, RICON manufactured by TOTAL. P30D etc. can be mentioned.
粘着剤組成物が1,2−ビニル基を有するジエン系重合体を含む場合、アクリル変性ポリオレフィン、水素引抜型開始剤及び1,2−ビニル基を有するジエン系重合体の含有割合は特に限定されない。例えば、粘着剤組成物において、前記ポリオレフィン100質量部に対し、1,2−ビニル基を有するジエン系重合体の含有量の下限は0.1質量部とすることができ、0.5質量部とすることが好ましく、1.0質量部とすることがより好ましい。また、粘着剤組成物において、ポリオレフィン100質量部に対し、1,2−ビニル基を有するジエン系重合体の含有量の上限は15質量部とすることができ、10質量部とすることが好ましく、8質量とすることがより好ましい。 When the pressure-sensitive adhesive composition contains a diene polymer having a 1,2-vinyl group, the content ratios of the acrylic modified polyolefin, the hydrogen abstraction initiator and the diene polymer having a 1,2-vinyl group are not particularly limited. .. For example, in the pressure-sensitive adhesive composition, the lower limit of the content of the diene-based polymer having a 1,2-vinyl group can be 0.1 parts by mass, and 0.5 parts by mass with respect to 100 parts by mass of the polyolefin. And preferably 1.0 part by mass. In the pressure-sensitive adhesive composition, the upper limit of the content of the diene polymer having a 1,2-vinyl group may be 15 parts by mass, preferably 10 parts by mass, based on 100 parts by mass of the polyolefin. , 8 mass is more preferable.
粘着剤組成物は、粘着剤層の粘着性及び耐久性を高めるために、さらに粘着付与剤を含むことも好ましい。粘着付与剤の種類は特に限定されず、例えば、粘着シートにおいて使用されている公知の粘着付与剤を広く使用することができる。 The pressure-sensitive adhesive composition preferably further contains a tackifier in order to enhance the tackiness and durability of the pressure-sensitive adhesive layer. The type of tackifier is not particularly limited, and for example, known tackifiers used in pressure-sensitive adhesive sheets can be widely used.
粘着付与剤としては、芳香族系粘着付与剤、テルペン骨格を含む粘着付与剤、ロジン骨格を含む粘着付与剤、及び石油樹脂系粘着付与剤等を挙げることができる。粘着剤組成物が粘着付与剤を含む場合、その種類は1種のみとすることができ、あるいは、2種以上とすることもできる。 Examples of the tackifier include an aromatic tackifier, a tackifier containing a terpene skeleton, a tackifier containing a rosin skeleton, and a petroleum resin tackifier. When the pressure-sensitive adhesive composition contains a tackifier, the type thereof may be only one type, or may be two or more types.
前記粘着付与剤の軟化点(軟化温度)は特に限定されず、例えば、90℃以上程度であることが好ましく、100℃以上程度とすることができ、また、200℃以下程度であることが好ましく、180℃以下程度であることが好ましい。なお、ここでいう粘着付与樹脂の軟化点は、JIS K5902及びJIS K2207のいずれかに規定する軟化点試験方法(環球法)によって測定された値として定義される。 The softening point (softening temperature) of the tackifier is not particularly limited, and is preferably about 90° C. or higher, about 100° C. or higher, and preferably about 200° C. or lower. It is preferably about 180° C. or lower. The softening point of the tackifying resin here is defined as a value measured by the softening point test method (ring and ball method) defined in either JIS K5902 or JIS K2207.
前記粘着付与剤の重量平均分子量(Mw)は特に限定されず、例えば、5万以下とすることができ、3万以下であることが好ましく、1万以下であることがより好ましく、8000以下であることがさらに好ましく、5000以下であることが特に好ましい。また、粘着付与剤の重量平均分子量(Mw)は、例えば、500以上とすることができ、1000以上であることが好ましく、2000以上であることがさらに好ましい。 The weight average molecular weight (Mw) of the tackifier is not particularly limited and may be, for example, 50,000 or less, preferably 30,000 or less, more preferably 10,000 or less, and 8000 or less. It is more preferable to be present, and it is particularly preferable to be 5000 or less. The weight average molecular weight (Mw) of the tackifier can be, for example, 500 or more, preferably 1000 or more, and more preferably 2000 or more.
粘着剤組成物が前記粘着付与剤を含む場合、その含有量は特に限定されない。例えば、粘着剤組成物において、前記ポリオレフィン100質量部に対し、前記粘着付与剤の含有量の下限は1質量部とすることができ、10質量部であることが好ましく、20質量部であることがさらに好ましい。また、粘着剤組成物において、ポリオレフィン100質量部に対し、前記粘着付与剤の含有量の上限は80質量部とすることができ、70質量部であることが好ましく、60質量部であることがさらに好ましい。 When the pressure-sensitive adhesive composition contains the tackifier, the content thereof is not particularly limited. For example, in the pressure-sensitive adhesive composition, the lower limit of the content of the tackifier may be 1 part by mass, preferably 10 parts by mass, and preferably 20 parts by mass with respect to 100 parts by mass of the polyolefin. Is more preferable. In addition, in the pressure-sensitive adhesive composition, the upper limit of the content of the tackifier can be 80 parts by mass, preferably 70 parts by mass, and preferably 60 parts by mass with respect to 100 parts by mass of polyolefin. More preferable.
前記粘着剤組成物の調製方法は特に限定されず、所定の原料を所定の含有割合となるように混合することで調製することができる。混合方法も特に限定されず、例えば、市販の混合機を使用できる。 The method for preparing the pressure-sensitive adhesive composition is not particularly limited, and it can be prepared by mixing predetermined raw materials in a predetermined content ratio. The mixing method is not particularly limited, and for example, a commercially available mixer can be used.
粘着剤組成物は、本発明の効果が阻害されない限り、その他の成分、例えば、帯電防止剤、酸化防止剤、防腐剤等が含まれていてもよい。粘着剤組成物がその他の成分を含む場合、その含有量は、例えば、粘着剤組成物の全質量に対して10質量%以下、好ましくは5質量%以下、より好ましくは1質量%以下、特に好ましくは0.1質量%以下とすることができる。 The pressure-sensitive adhesive composition may contain other components, for example, an antistatic agent, an antioxidant, a preservative and the like, as long as the effects of the present invention are not impaired. When the pressure-sensitive adhesive composition contains other components, the content is, for example, 10% by mass or less, preferably 5% by mass or less, more preferably 1% by mass or less, particularly preferably 1% by mass or less, based on the total mass of the pressure-sensitive adhesive composition. It can be preferably 0.1% by mass or less.
(粘着剤層の形成方法)
粘着剤層を形成する方法は特に限定されず、例えば、公知の手法を広く適用することができる。具体的に粘着剤層の形成方法は、前記粘着剤組成物を基材上に塗布して粘着剤組成物の塗膜を形成する工程、及び、該塗膜を乾燥処理することで、粘着剤層を形成する工程を備えることができる。
(Method for forming adhesive layer)
The method for forming the pressure-sensitive adhesive layer is not particularly limited, and, for example, known methods can be widely applied. Specifically, the method for forming a pressure-sensitive adhesive layer includes a step of applying the pressure-sensitive adhesive composition on a substrate to form a coating film of the pressure-sensitive adhesive composition, and a drying treatment of the coating film to form a pressure-sensitive adhesive. A step of forming a layer can be provided.
粘着剤組成物を基材に塗布するにあたって、塗布性を向上させるべく、粘着剤組成物は溶剤を含むこともできる。溶剤としては特に限定されず、例えば、酢酸メチル、酢酸エチル等のエステル化合物;ジエチルエーテル等のエーテル化合物;アセトン、メチルエチルケトン等のケトン化合物;ヘキサン、ヘプタン等の脂肪族炭化水素;シクロヘキサン等の脂環式炭化水素;ベンゼン、トルエン及びキシレン等の芳香族炭化水素;クロロホルム、1,2−ジクロロエタン等の塩素系炭化水素;メタノール、エタノール、イソプロピルアルコール及びt−ブタノール等のアルコール等が挙げられる。溶剤は、単独又は2種以上の混合物として使用することができる。 When the pressure-sensitive adhesive composition is applied to the substrate, the pressure-sensitive adhesive composition may contain a solvent in order to improve the coatability. The solvent is not particularly limited, and examples thereof include ester compounds such as methyl acetate and ethyl acetate; ether compounds such as diethyl ether; ketone compounds such as acetone and methyl ethyl ketone; aliphatic hydrocarbons such as hexane and heptane; alicyclic rings such as cyclohexane. Formula hydrocarbons; aromatic hydrocarbons such as benzene, toluene and xylene; chlorinated hydrocarbons such as chloroform and 1,2-dichloroethane; alcohols such as methanol, ethanol, isopropyl alcohol and t-butanol. The solvent can be used alone or as a mixture of two or more kinds.
粘着剤組成物が溶剤を含む場合、塗布性を考慮して、該粘着剤組成物の固形分濃度が10〜60質量%の範囲となるように溶剤を使用することが好ましく、15〜50質量%の範囲となるように溶剤を使用することがさらに好ましい。なお、粘着剤層の製造過程において、粘着剤層に含まれていた溶剤はすべて又は大部分は揮発する。 When the pressure-sensitive adhesive composition contains a solvent, it is preferable to use the solvent in consideration of coatability so that the solid content concentration of the pressure-sensitive adhesive composition is in the range of 10 to 60% by mass. It is more preferable to use a solvent so that it is in the range of %. In the manufacturing process of the pressure-sensitive adhesive layer, all or most of the solvent contained in the pressure-sensitive adhesive layer is volatilized.
粘着剤組成物を基材上に塗布する方法は特に限定されず、例えば、公知の塗布方法を広く採用することができる。例えば、ブレードコーター、エアナイフコーター、ロールコーター、バーコーター、グラビアコーター、マイクログラビアコーター、ロッドブレードコーター、リップコーター、ダイコーター、カーテンコーター等の市販の塗布装置を用いて前記粘着剤組成物を塗布することができる。 The method of applying the pressure-sensitive adhesive composition onto the substrate is not particularly limited, and, for example, known coating methods can be widely adopted. For example, the adhesive composition is applied using a commercially available coating device such as a blade coater, an air knife coater, a roll coater, a bar coater, a gravure coater, a microgravure coater, a rod blade coater, a lip coater, a die coater, and a curtain coater. be able to.
粘着剤組成物の塗布量は特に限定されず、目的とする粘着剤層の厚みに応じて適宜設定することができる。例えば、粘着剤組成物の塗布量は、後記する乾燥処理後に形成される粘着剤層の厚みが5〜1000μmとなるように調節することができる。 The coating amount of the pressure-sensitive adhesive composition is not particularly limited and can be appropriately set according to the target thickness of the pressure-sensitive adhesive layer. For example, the coating amount of the pressure-sensitive adhesive composition can be adjusted so that the thickness of the pressure-sensitive adhesive layer formed after the drying treatment described below is 5 to 1000 μm.
粘着剤組成物を塗布するための基材の種類も特に限定的ではなく、粘着剤層の形成に用いられる基材を広く使用することができる。例えば、粘着剤組成物を塗布するための基材として、剥離シートを挙げることができる。 The type of base material for applying the pressure-sensitive adhesive composition is not particularly limited, and the base material used for forming the pressure-sensitive adhesive layer can be widely used. For example, a release sheet can be mentioned as a base material for applying the pressure-sensitive adhesive composition.
剥離シートとしては、例えば、粘着シートにおいて接着剤層を保護するために使用されている、いわゆるセパレータを挙げることができる。より具体的には、剥離シートとして、離型層を備える樹脂フィルム等を挙げることができる。 Examples of the release sheet include so-called separators used for protecting the adhesive layer in the pressure-sensitive adhesive sheet. More specifically, examples of the release sheet include a resin film having a release layer.
剥離シートにおいて、樹脂フィルムとしては、例えば、ポリエチレンテレフタレートフィルム等を挙げることができる。 In the release sheet, examples of the resin film include a polyethylene terephthalate film and the like.
離型層とは、前記樹脂フィルムの少なくとも片面に形成された層であって、粘着剤層の粘着力よりも小さい剥離力を有し、容易に剥離シートを剥離することができるように形成された層であることを意味する。このような離型層は、例えば、粘着シートにおいて離型層として使用される公知の成分を広く適用することができる。例えば、公知のシリコーン材料で離型層を形成することができる。 The release layer is a layer formed on at least one surface of the resin film, has a peeling force smaller than the adhesive force of the pressure-sensitive adhesive layer, and is formed so that the release sheet can be easily peeled off. It means that it is a layer. For such a release layer, for example, known components used as a release layer in an adhesive sheet can be widely applied. For example, the release layer can be formed of a known silicone material.
基材として前記剥離シートを使用する場合、粘着剤組成物は、当該剥離シートの離型層面に塗布して、粘着剤組成物の塗膜を形成することができる。 When the release sheet is used as the substrate, the pressure-sensitive adhesive composition can be applied to the release layer surface of the release sheet to form a coating film of the pressure-sensitive adhesive composition.
粘着剤組成物を、前記剥離シート等の基材上に塗布して塗膜を形成した後、乾燥処理をすることで、粘着剤層が基材上に形成される。 The pressure-sensitive adhesive layer is formed on the base material by applying the pressure-sensitive adhesive composition onto the base material such as the release sheet to form a coating film and then performing a drying treatment.
乾燥処理の条件は特に限定されず、例えば、従来から行われている粘着剤組成物の塗膜の乾燥方法を広く採用することができる。このような乾燥処理は、例えば、公知の加熱装置等を用いて行うことができる。加熱温度は、例えば、50〜200℃とすることができ、好ましくは60〜150℃とすることができる。加熱時間は溶剤が揮発し、粘着剤層の残留溶剤濃度が例えば1000ppm以下になるように設定すればよく、粘着剤組成物の濃度、所望する粘着剤層の厚み等に応じて上記温度範囲で1〜30分程度の時間内で適宜設定することが好ましい。 The conditions of the drying treatment are not particularly limited, and, for example, a conventionally used method for drying the coating film of the pressure-sensitive adhesive composition can be widely adopted. Such a drying process can be performed using, for example, a known heating device. The heating temperature can be, for example, 50 to 200°C, and preferably 60 to 150°C. The heating time may be set so that the solvent is volatilized and the residual solvent concentration of the pressure-sensitive adhesive layer is, for example, 1000 ppm or less. It is preferable to set appropriately within a time of about 1 to 30 minutes.
乾燥処理により形成された粘着剤層には、さらに接着剤層を保護するための保護層を貼り合せることができる。この場合、保護層は、粘着剤層の基材とは逆側の面に貼り合わされる。保護層としては、例えば、前述と同様、剥離シートを挙げることができる。この保護層としての剥離シートも前記基材の場合と同様、離型層を備える樹脂フィルム等を挙げることができる。樹脂フィルムとしては、例えば、前述と同様、ポリエチレンテレフタレートフィルム等を挙げることができ、また、離型層は、例えば、公知のシリコーン材料で形成することができる。 A protective layer for protecting the adhesive layer can be further attached to the pressure-sensitive adhesive layer formed by the drying treatment. In this case, the protective layer is attached to the surface of the adhesive layer opposite to the base material. As the protective layer, for example, a release sheet can be used as described above. As for the release sheet as the protective layer, as in the case of the base material, a resin film having a release layer and the like can be mentioned. As the resin film, for example, a polyethylene terephthalate film and the like can be mentioned as in the above, and the release layer can be formed of, for example, a known silicone material.
基材及び保護層がいずれも剥離シート(それぞれ第1の剥離シート、第2の剥離シート)である場合、基材としての剥離シート(第1の剥離シート)の離型層の剥離力と、保護層を形成するための剥離シート(第2の剥離シート)の離型層の粘着力とは異なることが好ましい。つまり、基材及び保護層がいずれも剥離シートである場合、それぞれの剥離シートの剥離力が異なることが好ましい。この場合、剥離シートを剥がすときに一方の剥離シートだけを選択的に剥がすことが容易になり、いわゆる泣き別れの現象を抑止しやすい。 When the base material and the protective layer are both release sheets (first release sheet and second release sheet, respectively), the release force of the release layer of the release sheet (first release sheet) as the base material, It is preferable that it is different from the adhesive force of the release layer of the release sheet (second release sheet) for forming the protective layer. That is, when the base material and the protective layer are both release sheets, it is preferable that the release sheets have different release forces. In this case, it becomes easy to selectively peel off only one of the release sheets when peeling off the release sheet, and it is easy to suppress the so-called tearing phenomenon.
粘着剤層を形成し、必要に応じて保護層を上記のように形成した後、適宜、エージング処理を行うこともできる。エージング処理の方法は特に限定されず、例えば、15〜50℃の雰囲気下に粘着剤層を静置させる方法を挙げることができる。エージング時間は、温度によって適宜設定することができ、例えば、1日〜10日とすることができる。 After forming the pressure-sensitive adhesive layer and, if necessary, the protective layer as described above, aging treatment can be appropriately performed. The method of aging treatment is not particularly limited, and examples thereof include a method of allowing the pressure-sensitive adhesive layer to stand in an atmosphere of 15 to 50°C. The aging time can be appropriately set depending on the temperature, and can be, for example, 1 day to 10 days.
粘着剤層の厚さは特に限定されず、使用する用途等に応じて適宜設定することができる。例えば、粘着剤層の厚さは、5〜200μmとすることができ、5〜100μmであることが好ましく、5〜50μmであることがより好ましく、5〜25μmであることが特に好ましい。 The thickness of the pressure-sensitive adhesive layer is not particularly limited, and can be set as appropriate according to the intended use and the like. For example, the pressure-sensitive adhesive layer may have a thickness of 5 to 200 μm, preferably 5 to 100 μm, more preferably 5 to 50 μm, and particularly preferably 5 to 25 μm.
(粘着剤層の物性)
前述のように、本発明の粘着剤層は、活性エネルギー線を積算光量が3000mJ/cm2となるように照射して粘着剤層を後硬化した場合に下記物性(1)及び(2)を満たす。
物性(1):引張速度10mm/minの引張試験測定において、破断伸度が1200%以上であり、かつ、ひずみ1000%での応力が0.40N/mm2以上である。
物性(2):100μmの厚みでの透湿度が50g/m2・24hr以下である。
粘着剤層が上記物性(1)及び(2)の条件を満たすことにより、硬化後(後効果後)の粘着剤層は、優れた低透湿性及び耐久性を有することができる。
(Physical properties of adhesive layer)
As described above, the pressure-sensitive adhesive layer of the present invention has the following physical properties (1) and (2) when the pressure-sensitive adhesive layer is post-cured by irradiation with active energy rays so that the integrated light amount becomes 3000 mJ/cm 2. Fulfill.
Physical Properties (1): In a tensile test measurement at a tensile speed of 10 mm/min, the breaking elongation is 1200% or more, and the stress at a strain of 1000% is 0.40 N/mm 2 or more.
Physical properties (2): Water vapor permeability at a thickness of 100 μm is 50 g/m 2 ·24 hr or less.
When the pressure-sensitive adhesive layer satisfies the above physical properties (1) and (2), the pressure-sensitive adhesive layer after curing (after post-effect) can have excellent low moisture permeability and durability.
上記物性を測定するにあたって、粘着剤層に照射する前記活性エネルギー線としては、紫外線、電子線、可視光線、X線、イオン線等が挙げられる。中でも、汎用性の点から、紫外線または電子線が好ましく、紫外線が特に好ましい。紫外線の光源としては、例えば、高圧水銀灯、低圧水銀灯、超高圧水銀灯、メタルハライドランプ、カーボンアーク、キセノンアーク、無電極紫外線ランプ等を使用できる。電子線としては、例えば、コックロフトワルト型、バンデクラフ型、共振変圧型、絶縁コア変圧器型、直線型、ダイナミトロン型、高周波型等の各種電子線加速器から放出される電子線を使用できる。 In measuring the above physical properties, examples of the active energy ray with which the pressure-sensitive adhesive layer is irradiated include ultraviolet rays, electron rays, visible rays, X rays, and ion rays. Among them, ultraviolet rays or electron beams are preferable, and ultraviolet rays are particularly preferable, from the viewpoint of versatility. As the ultraviolet light source, for example, a high pressure mercury lamp, a low pressure mercury lamp, an ultrahigh pressure mercury lamp, a metal halide lamp, a carbon arc, a xenon arc, an electrodeless ultraviolet lamp, or the like can be used. As the electron beam, for example, an electron beam emitted from various electron beam accelerators such as Cockloft-Walt type, Bande-Clough type, resonance transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type can be used.
<物性(1)>
物性(1)において、引張試験の測定条件はJIS K 7161−1に準拠する。これにより、破断伸度及びひずみ1000%での応力を測定できる。具体的にこの引張試験は、引張速度は10mm/minとし、23℃、相対湿度50%の環境下で測定する。また、測定サンプルは、厚さ20μm、幅60mm、長さ250mmの後硬化の粘着剤層を、長さ方向に丸めて断面積5mm2、高さ60mmの円柱形状に加工して用いる。チャック間距離が30mmとなるようサンプルをセットして引っ張り、測定サンプルのひずみが1000%となったときの応力値及び測定サンプルが破断した時の伸度(破断伸度)を計測する。引張試験には、島津製作所製のオートグラフAGS−Xを用いる。
<Physical properties (1)>
In the physical properties (1), the measurement conditions of the tensile test are based on JIS K7161-1. This makes it possible to measure the elongation at break and the stress at a strain of 1000%. Specifically, this tensile test is performed under the environment of 23° C. and relative humidity of 50% at a tensile speed of 10 mm/min. Further, the measurement sample is used by processing a post-cured pressure-sensitive adhesive layer having a thickness of 20 μm, a width of 60 mm, and a length of 250 mm into a columnar shape having a cross-sectional area of 5 mm 2 and a height of 60 mm by rolling in the length direction. The sample is set and pulled so that the distance between chucks is 30 mm, and the stress value when the strain of the measurement sample becomes 1000% and the elongation at break of the measurement sample (breaking elongation) are measured. Shimadzu Corporation Autograph AGS-X is used for the tensile test.
物性(1)において、活性エネルギー線照射後の粘着剤層の破断伸度が1200%以上であり、かつ、活性エネルギー線照射後の粘着剤層のひずみ1000%での応力が0.40N/mm2以上であることで、粘着剤層は優れた耐久性をもたらすことができる。 In the physical properties (1), the breaking elongation of the pressure-sensitive adhesive layer after irradiation with active energy rays is 1200% or more, and the stress at strain 1000% of the pressure-sensitive adhesive layer after irradiation with active energy rays is 0.40 N/mm. When it is 2 or more, the pressure-sensitive adhesive layer can provide excellent durability.
物性(1)において、破断伸度は1250%以上であることが好ましく、1300%以上であることがより好ましい。また、物性(1)において、破断伸度の上限は特に限定はないが、通常、破断伸度は2000%以下である。 In the physical property (1), the breaking elongation is preferably 1250% or more, more preferably 1300% or more. In the physical property (1), the upper limit of the breaking elongation is not particularly limited, but the breaking elongation is usually 2000% or less.
物性(1)において、破断伸度が1200%以上であり、かつ、ひずみ1000%での応力が0.40N/mm2以上であることで、粘着剤層は優れた耐久性をもたらすことができる。 In the physical property (1), the elongation at break is 1200% or more, and the stress at a strain of 1000% is 0.40 N/mm 2 or more, whereby the pressure-sensitive adhesive layer can bring excellent durability. ..
物性(1)において、ひずみ1000%での応力が0.45N/mm2以上であることが好ましく、0.5N/mm2以上であることがより好ましい。また、物性(1)において、ひずみ1000%での応力の上限は特に限定はないが、通常、ひずみ1000%での応力は3.0N/mm2以下である。 In Physical Properties (1), it is preferable that the stress at 1000% strain is 0.45N / mm 2 or more, more preferably 0.5 N / mm 2 or more. In the physical property (1), the upper limit of the stress at 1000% strain is not particularly limited, but the stress at 1000% strain is usually 3.0 N/mm 2 or less.
粘着剤層は、活性エネルギー線照射前のひずみ1000%での応力は、例えば、0.01〜0.30N/mm2である。 In the pressure-sensitive adhesive layer, the stress at a strain of 1000% before irradiation with active energy rays is, for example, 0.01 to 0.30 N/mm 2 .
本発明の粘着剤層は、ポリオレフィンと、(メタ)アクリル系モノマーと、水素引抜型開始剤とを含有する粘着剤組成物を用いて形成されることから、物性(1)を満たすことができる。粘着剤組成物中のポリオレフィン及び(メタ)アクリル系モノマーと、水素引抜型開始剤の種類及び量を調節することで、物性(1)における、破断伸度及びひずみ1000%での応力を適切に制御することができる。 Since the pressure-sensitive adhesive layer of the present invention is formed using a pressure-sensitive adhesive composition containing a polyolefin, a (meth)acrylic monomer, and a hydrogen abstraction type initiator, it can satisfy the physical properties (1). .. By adjusting the types and amounts of the polyolefin and (meth)acrylic monomers and the hydrogen abstraction type initiator in the pressure-sensitive adhesive composition, the elongation at break and the stress at a strain of 1000% in the physical properties (1) are appropriately adjusted. Can be controlled.
<物性(2)>
物性(2)において、透湿度(g/m2・24hr)は、日本国特許第5089809に記載の方法を参照する。具体的には以下の方法で透湿度を測定する。
100μm厚みの後硬化後の粘着剤層を裏材(旭化成社製「BEMCOT M−1」)に積層して透湿度を測定するためのサンプルを得る。このサンプルを、小数点以下3桁までの重さを正確に秤量した50gの蒸留水が入った直径2.54cmの開口部付きガラスジャー又はガラス瓶(以下、「ガラス容器」と表記する)の最上部に、前記粘着剤層がガラス容器の底側に対向するように設置する。前記粘着剤層を、オープンリングカバーで定位置に保持しつつ、隙間から水蒸気等が外部へ漏れないように粘着剤層によりガラス容器の内部を密封した後、このガラス容器(粘着剤層を備えたガラス容器)を、相対湿度20%で40℃に設定したオーブンに約24時間、当該ガラス容器を直立(このとき、水がサンプルに触れない)にして設置する。その後、粘着剤層を備えたガラス容器の重量喪失を計測し、この重量喪失から透湿度(g/m2・24hr)を算出する。なお、粘着剤層の厚み(100μm)は、粘着剤組成物の塗布量から見積もったものである。
<Physical properties (2)>
In the physical properties (2), for the water vapor permeability (g/m 2 ·24 hr), refer to the method described in Japanese Patent No. 5089809. Specifically, the moisture permeability is measured by the following method.
A pressure-sensitive adhesive layer after post-curing having a thickness of 100 μm is laminated on a backing material (“BEMCOT M-1” manufactured by Asahi Kasei Corp.) to obtain a sample for measuring water vapor transmission rate. The top of a glass jar or glass bottle with an opening having a diameter of 2.54 cm (hereinafter, referred to as a “glass container”) containing 50 g of distilled water in which a weight of up to three decimal places is accurately weighed Then, the adhesive layer is installed so as to face the bottom side of the glass container. While holding the pressure-sensitive adhesive layer in place with an open ring cover, after sealing the inside of the glass container with the pressure-sensitive adhesive layer so as to prevent water vapor and the like from leaking to the outside from the gap, the glass container (comprising the pressure-sensitive adhesive layer The glass container) is placed in an oven set at 40° C. with a relative humidity of 20% for about 24 hours with the glass container standing upright (where water does not touch the sample). Then, the weight loss of the glass container provided with the adhesive layer is measured, and the moisture vapor transmission rate (g/m 2 ·24 hr) is calculated from the weight loss. The thickness (100 μm) of the pressure-sensitive adhesive layer is estimated from the coating amount of the pressure-sensitive adhesive composition.
物性(2)において、活性エネルギー線照射後の100μm厚みの粘着剤層の透湿度が50g/m2・24hr以下であることで、粘着剤層は低い透湿性をもたらすことができる。これにより、低透湿性が要求される用途に粘着剤層を適用することが可能となる。 In the physical property (2), the moisture permeability of the pressure-sensitive adhesive layer having a thickness of 100 μm after irradiation with active energy rays is 50 g/m 2 ·24 hr or less, so that the pressure-sensitive adhesive layer can provide low moisture permeability. This makes it possible to apply the pressure-sensitive adhesive layer to applications where low moisture permeability is required.
物性(2)において、透湿度は45g/m2・24hr以下であることが好ましく、30g/m2・24hr以下であることがより好ましい。また、物性(2)において、透湿度の下限は特に限定はないが、通常、透湿度は1g/m2・24hr以上である。 In the physical property (2), the water vapor permeability is preferably 45 g/m 2 ·24 hr or less, and more preferably 30 g/m 2 ·24 hr or less. In the physical property (2), the lower limit of the water vapor transmission rate is not particularly limited, but the water vapor transmission rate is usually 1 g/m 2 ·24 hr or more.
本発明の粘着剤層は、ポリオレフィンと、(メタ)アクリル系モノマーと、水素引抜型開始剤とを含有する粘着剤組成物を用いて形成されることから、物性(2)を満たすことができる。また、粘着剤組成物中のポリオレフィンの含有割合を調節することで、物性(2)における、透湿度の値を適切に制御することができる。 Since the pressure-sensitive adhesive layer of the present invention is formed using a pressure-sensitive adhesive composition containing a polyolefin, a (meth)acrylic monomer, and a hydrogen abstraction type initiator, it can satisfy the physical properties (2). .. In addition, by adjusting the content ratio of the polyolefin in the pressure-sensitive adhesive composition, it is possible to appropriately control the value of the water vapor transmission rate in the physical property (2).
(その他物性)
本発明の粘着剤層は、活性エネルギー線を積算光量が3000mJ/cm2となるように照射して粘着剤層を後硬化した場合の比誘電率が3.0以下であることが好ましい。この場合、粘着剤層は、各種の画像表示装置等の接着用途に好適に使用することができる。粘着剤層を後硬化した場合の比誘電率は、例えば、ポリオレフィンを含む粘着剤組成物を使用することで、適切な範囲内に調節することができる。
(Other physical properties)
The pressure-sensitive adhesive layer of the present invention preferably has a relative dielectric constant of 3.0 or less when the pressure-sensitive adhesive layer is post-cured by irradiation with active energy rays so that the integrated light amount becomes 3000 mJ/cm 2 . In this case, the pressure-sensitive adhesive layer can be suitably used for bonding applications such as various image display devices. The relative dielectric constant when the pressure-sensitive adhesive layer is post-cured can be adjusted within an appropriate range by using, for example, a pressure-sensitive adhesive composition containing polyolefin.
粘着剤層の比誘電率の測定は以下の手順で実施できる。粘着剤層(粘着シートから第1の剥離シート及び第2の剥離シートを剥離したもの)を2枚の銅箔の間に挟み、オートクレーブ処理(40℃、0.5MPa、30分間)を実施する。その後、誘電体測定システム((株)東陽テクニカ製、1260型)によりJIS C 2138に基づいて比誘電率を測定する。比誘電率の測定において、周波数は1MHz、測定環境は23℃、相対湿度50%とする。 The relative dielectric constant of the pressure-sensitive adhesive layer can be measured by the following procedure. The pressure-sensitive adhesive layer (those obtained by peeling the first release sheet and the second release sheet from the pressure-sensitive adhesive sheet) is sandwiched between two copper foils, and an autoclave treatment (40° C., 0.5 MPa, 30 minutes) is performed. .. After that, the relative permittivity is measured based on JIS C 2138 with a dielectric measuring system (1260 type, manufactured by Toyo Technica Co., Ltd.). In the measurement of the relative permittivity, the frequency is 1 MHz, the measurement environment is 23° C., and the relative humidity is 50%.
粘着剤層のゲル分率は10〜70%であり、前記後硬化後の粘着剤層のゲル分率が60〜100%であり、かつ、前記後硬化後の粘着剤層のゲル分率が後硬化前のゲル分率よりも10%以上高いことが好ましい。この場合、硬化後の粘着剤層は、基材密着性に優れ、また、優れた耐久性を有することができる。 The pressure-sensitive adhesive layer has a gel fraction of 10 to 70%, the post-curing pressure-sensitive adhesive layer has a gel fraction of 60 to 100%, and the post-curing pressure-sensitive adhesive layer has a gel fraction of 60 to 100%. It is preferably 10% or more higher than the gel fraction before post-curing. In this case, the pressure-sensitive adhesive layer after curing can have excellent base material adhesion and excellent durability.
粘着剤層の23℃における剪断貯蔵弾性率G’は、例えば、粘着剤層の耐久性が向上しやすく、剥がれ及び気泡発生も生じにくいという観点から、1.0×105〜8.0×106の範囲とすることができる。また、粘着剤層の85℃における剪断貯蔵弾性率G’は、例えば、1.0×104〜8.0×104の範囲とすることができる。 The shear storage elastic modulus G′ at 23° C. of the pressure-sensitive adhesive layer is, for example, 1.0×10 5 to 8.0× from the viewpoint that the durability of the pressure-sensitive adhesive layer is easily improved and peeling and bubble generation are less likely to occur. It can be in the range of 10 6 . Further, the shear storage elastic modulus G′ at 85° C. of the pressure-sensitive adhesive layer can be set, for example, in the range of 1.0×10 4 to 8.0×10 4 .
2.粘着シート
本発明の粘着シートは、粘着剤層のみで形成されていてもよいし、必要に応じて他の層を有していてもよい。他の層は、粘着剤層の片面又は両面に形成することができる。他の層としては、前述の剥離シートを挙げることができる。粘着剤層の両面に剥離シートが形成される場合は、前述のように、両剥離シート(第1の剥離シート及び第2の剥離シート)の剥離力が異なるようにすることができる。
2. Adhesive Sheet The adhesive sheet of the present invention may be formed of only an adhesive layer, or may have other layers as necessary. The other layer can be formed on one side or both sides of the pressure-sensitive adhesive layer. Examples of the other layer include the release sheet described above. When the release sheets are formed on both surfaces of the pressure-sensitive adhesive layer, both release sheets (the first release sheet and the second release sheet) can have different release forces as described above.
例えば、前述の粘着剤層の形成方法において、基材として剥離シートを使用し、また、保護層としても剥離シートを使用する場合は、粘着剤層の両面に剥離シートを有する粘着シート(剥離層付き粘着シート)を直接得ることができる。なお、粘着剤層を形成した後、別途、その両面に剥離シートを設けて、剥離層付き粘着シートを得ることもできる。 For example, in the method for forming the pressure-sensitive adhesive layer described above, when the release sheet is used as the base material and the release sheet is also used as the protective layer, the pressure-sensitive adhesive sheet having the release sheet on both sides of the pressure-sensitive adhesive layer (release layer Directly attached adhesive sheet). After forming the pressure-sensitive adhesive layer, a release sheet may be separately provided on both surfaces of the pressure-sensitive adhesive layer to obtain a pressure-sensitive adhesive sheet with a release layer.
粘着シートが剥離シートを有する場合、これらの剥離シートは粘着シートにおける、いわゆるセパレータとしての機能を有することができる。 When the pressure-sensitive adhesive sheet has a release sheet, these release sheets can have a function as a so-called separator in the pressure-sensitive adhesive sheet.
粘着シートが剥離シートを備える場合、剥離シートの厚みは特に限定されない。例えば、剥離シートの厚みは5〜300μmとすることができ、好ましくは10〜150μmとすることができる。粘着剤層の両面の剥離シートは互いに厚みが異なっていてもよい。 When the pressure-sensitive adhesive sheet includes a release sheet, the thickness of the release sheet is not particularly limited. For example, the thickness of the release sheet can be 5 to 300 μm, and preferably 10 to 150 μm. The release sheets on both sides of the adhesive layer may have different thicknesses.
図1は、粘着シートの実施形態の一例であって、断面の概略図である。図1に示されるように、粘着シートは、粘着剤層11の片面に透明基材12aを備えることができる。この場合、粘着剤層11のもう一方の面は剥離シート12bによって覆われていることが好ましい。粘着シートを使用する場合はこの剥離シート12bを剥がして所望の被着体に粘着剤層11が密着するように貼合し、その後、後記するように活性エネルギー線を照射するなどして後硬化をすることが好ましい。透明基材としてはポリエチレンテレフタレートフィルムやアクリルフィルム、ポリカーボネートフィルム、トリアセチルセルロースフィルム、シクロオレフィンポリマーフィルムなど光学分野に用いられる一般的なフィルムを用いることができる。またこれらの透明基材の粘着剤層側には易接着層を設けていてもよい。さらに、透明基材の粘着剤層とは逆面にはハードコート層や反射防止層、防汚層、紫外線吸収層などの機能層が備えられていてもよい。 FIG. 1 is an example of an embodiment of a pressure-sensitive adhesive sheet, and is a schematic cross-sectional view. As shown in FIG. 1, the pressure-sensitive adhesive sheet can include a transparent substrate 12 a on one surface of the pressure-sensitive adhesive layer 11. In this case, the other surface of the adhesive layer 11 is preferably covered with the release sheet 12b. When using a pressure-sensitive adhesive sheet, the release sheet 12b is peeled off and the pressure-sensitive adhesive layer 11 is adhered to a desired adherend so that the pressure-sensitive adhesive layer 11 is adhered to the adherend, and then post-curing is performed by irradiating with active energy rays as described later. Is preferred. As the transparent substrate, a general film used in the optical field such as a polyethylene terephthalate film, an acrylic film, a polycarbonate film, a triacetyl cellulose film, a cycloolefin polymer film can be used. Further, an easy adhesion layer may be provided on the adhesive layer side of these transparent substrates. Further, a functional layer such as a hard coat layer, an antireflection layer, an antifouling layer, and an ultraviolet absorbing layer may be provided on the surface of the transparent substrate opposite to the adhesive layer.
粘着シートは、その両表面に剥離シートを備えることもできる。粘着シートの両表面に剥離シートが備えられている場合、図1に示されるように粘着剤層11の両表面に剥離シート12a及び12bを有することが好ましい。 The pressure-sensitive adhesive sheet can be provided with release sheets on both surfaces thereof. When the release sheet is provided on both surfaces of the pressure-sensitive adhesive sheet, it is preferable to have release sheets 12a and 12b on both surfaces of the pressure-sensitive adhesive layer 11 as shown in FIG.
<粘着シートの使用方法(後硬化方法)>
粘着シートは、基板、フィルム等の部材(被着体)どうしを貼り合せて接着させる用途に広く使用することができる。
<How to use the adhesive sheet (post-curing method)>
The pressure-sensitive adhesive sheet can be widely used for applications in which members (adherends) such as substrates and films are adhered to each other.
例えば、一対の被着体の間に粘着シートを介在させ、被着体どうしを粘着シートで貼り合せ積層体を形成し、「後硬化」をすることで、被着体どうしを粘着シートで貼り合せることができる。なお、粘着シートが剥離シートを備える場合は、当該剥離シートを剥がした状態で、一対の被着体の間に粘着シートを介在させる。 For example, by interposing an adhesive sheet between a pair of adherends, adhering the adherends to each other with the adhesive sheet to form a laminated body, and “post-curing” the adherends to each other with the adhesive sheet. Can be combined. When the pressure-sensitive adhesive sheet includes a release sheet, the pressure-sensitive adhesive sheet is interposed between the pair of adherends with the release sheet peeled off.
粘着シートにおける粘着剤層は、活性エネルギー線を照射して後硬化することで、水素引抜型開始剤が(メタ)アクリル系モノマーの水素を引き抜くことで、架橋反応が進行し得る。これにより、粘着剤層の硬化がさらに進行し、この粘着剤層の硬化によって、被着体どうしがより強固に接着される。 The pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet is irradiated with active energy rays and post-cured, so that the hydrogen abstraction-type initiator abstracts hydrogen of the (meth)acrylic monomer, whereby the crosslinking reaction can proceed. Thereby, the curing of the pressure-sensitive adhesive layer further progresses, and the adherends are more firmly adhered to each other by the curing of the pressure-sensitive adhesive layer.
ここで、粘着剤層を後硬化する方法は特に限定されず、例えば、公知の硬化方法を広く採用することができる。具体的には、活性エネルギー線を粘着剤層に照射することで、粘着剤層を後硬化することができる。なお、念のための注記に過ぎないが、粘着シートを各種用途で使用するための後硬化の条件は、前述の物性(1)及び(2)を測定するために行う後硬化の条件に限定されるものではない。 Here, the method of post-curing the pressure-sensitive adhesive layer is not particularly limited, and, for example, known curing methods can be widely adopted. Specifically, the adhesive layer can be post-cured by irradiating the adhesive layer with active energy rays. It should be noted that the post-curing conditions for using the pressure-sensitive adhesive sheet in various applications are limited to the post-curing conditions for measuring the above-mentioned physical properties (1) and (2), just as a precautionary note. It is not something that will be done.
前記活性エネルギー線としては、紫外線、電子線、可視光線、X線、イオン線等が挙げられる。中でも、汎用性の点から、紫外線または電子線が好ましく、紫外線が特に好ましい。紫外線の光源としては、例えば、高圧水銀灯、低圧水銀灯、超高圧水銀灯、メタルハライドランプ、カーボンアーク、キセノンアーク、無電極紫外線ランプ等を使用できる。電子線としては、例えば、コックロフトワルト型、バンデクラフ型、共振変圧型、絶縁コア変圧器型、直線型、ダイナミトロン型、高周波型等の各種電子線加速器から放出される電子線を使用できる。 Examples of the active energy rays include ultraviolet rays, electron rays, visible rays, X rays, and ion rays. Among them, ultraviolet rays or electron beams are preferable, and ultraviolet rays are particularly preferable, from the viewpoint of versatility. As the ultraviolet light source, for example, a high pressure mercury lamp, a low pressure mercury lamp, an ultrahigh pressure mercury lamp, a metal halide lamp, a carbon arc, a xenon arc, an electrodeless ultraviolet lamp, or the like can be used. As the electron beam, for example, an electron beam emitted from various electron beam accelerators such as Cockloft-Walt type, Bande-Clough type, resonance transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type can be used.
活性エネルギー線照射の積算光量は、例えば500〜10000mJ/cm2、好ましくは1000〜8000mJ/cm2、より好ましくは1500〜6000mJ/cm2である。 Integrated light quantity of the active energy ray irradiation, for example 500~10000mJ / cm 2, preferably 1000~8000mJ / cm 2, more preferably 1500~6000mJ / cm 2.
活性エネルギー線の照射方法も特に限定されず、例えば、被着体どうしを粘着シートで貼り合せて形成させた積層体の全面に対して活性エネルギー線を照射することができる。この観点から、被着体の少なくとも一方は、透明であることが好ましい。活性エネルギー線の照射にあたっては、例えば、公知の活性エネルギー線照射装置を使用することができる。 The method of irradiating the active energy ray is not particularly limited, and for example, the entire surface of the laminate formed by adhering adherends with an adhesive sheet can be irradiated with the active energy ray. From this viewpoint, at least one of the adherends is preferably transparent. For irradiation with the active energy ray, for example, a known active energy ray irradiation device can be used.
<粘着シートの用途>
本発明の粘着シートは、耐久性を必要とする光学部材であって、形状が複雑で積層体になってからの打抜き加工が必要な光学部材の貼合用に好ましく用いられる。
<Use of adhesive sheet>
The pressure-sensitive adhesive sheet of the present invention is an optical member that requires durability, and is preferably used for bonding an optical member that has a complicated shape and that requires punching after forming a laminated body.
本発明の粘着シートは、基材等の被着体に貼合し、後硬化させた後、高温高湿環境下に曝した場合であっても、耐久性に優れているため、浮きや剥がれの発生を抑制できる。本発明の粘着シートは、例えば、ポリカーボネートフィルムに貼合し、後硬化させた後、高温高湿環境下に曝した場合であっても、ポリカーボネートフィルムから浮いたり、剥がれたりすることを抑制することができる。 The pressure-sensitive adhesive sheet of the present invention is excellent in durability even when exposed to a high-temperature and high-humidity environment after being attached to an adherend such as a base material and post-cured, and therefore, it does not float or peel off. Can be suppressed. The pressure-sensitive adhesive sheet of the present invention is, for example, attached to a polycarbonate film, and after being post-cured, even when exposed to a high temperature and high humidity environment, it is prevented from floating or peeling from the polycarbonate film. You can
本発明の粘着シートは、偏光板などの光学部材に貼合されるものであってもよい。ここで、偏光板とは、偏光子と偏光子保護フィルムを含むものであり、本発明の粘着シートは偏光子保護フィルムに貼合されることが好ましい。偏光子保護フィルムとしては、シクロオレフィン系樹脂フィルム、トリアセチルセルロース、ジアセチルセルロースなどの酢酸セルロース系樹脂フィルム、ポリエチレンテレフタレート、ポリエチレンナフタレート、ポリブチレンテレフタレートなどのポリエステル系樹脂フィルム、ポリカーボネート系樹脂フィルム、アクリル系樹脂フィルム、ポリプロピレン系樹脂フィルムなどが挙げられる。 The pressure-sensitive adhesive sheet of the present invention may be attached to an optical member such as a polarizing plate. Here, the polarizing plate includes a polarizer and a polarizer protective film, and the pressure-sensitive adhesive sheet of the present invention is preferably attached to the polarizer protective film. As the polarizer protective film, cycloolefin resin film, cellulose acetate resin film such as triacetyl cellulose and diacetyl cellulose, polyester resin film such as polyethylene terephthalate, polyethylene naphthalate and polybutylene terephthalate, polycarbonate resin film, acrylic Examples thereof include a resin resin film and a polypropylene resin film.
本発明の粘着シートが両面粘着シートである場合は、2つの被着体の貼合に用いることができる。この場合、本発明の粘着シートは、タッチパネルの内部における透明光学用フィルム同士の貼合、透明光学用フィルムとガラスとの貼合、タッチパネルの透明光学用フィルムと液晶パネルとの貼合、カバーガラスと透明光学用フィルムとの貼合、カバーガラスと透明光学用フィルムとの貼合などに用いられ、いずれかの部材がポリカーボネート基材である場合に有用である。透明光学用フィルムは、ポリエチレンテレフタレートフィルムやアクリルフィルム、ポリカーボネートフィルム、トリアセチルセルロースフィルム、シクロオレフィンポリマーフィルムなど光学分野に用いられる一般的なフィルムを用いることが出来る。また、透明光学用フィルムやポリカーボネート基材にはハードコート層が設けられていてもよい。 When the pressure-sensitive adhesive sheet of the present invention is a double-sided pressure-sensitive adhesive sheet, it can be used for bonding two adherends. In this case, the pressure-sensitive adhesive sheet of the present invention includes bonding of transparent optical films to each other inside a touch panel, bonding of transparent optical film and glass, bonding of transparent optical film of touch panel and liquid crystal panel, cover glass. And a transparent optical film, or a cover glass and a transparent optical film, and is useful when either member is a polycarbonate substrate. As the transparent optical film, a general film used in the optical field such as a polyethylene terephthalate film, an acrylic film, a polycarbonate film, a triacetyl cellulose film, or a cycloolefin polymer film can be used. A hard coat layer may be provided on the transparent optical film or the polycarbonate substrate.
本発明の粘着シートは、低い透湿性を有し、しかも、耐久性にも優れることから、各種画像表示装置等に広く適用することができ、特に低透湿性に優れることから、有機EL(OLED)等に好適に使用することができる。 INDUSTRIAL APPLICABILITY The pressure-sensitive adhesive sheet of the present invention has low moisture permeability and excellent durability, and thus can be widely applied to various image display devices and the like. ) Etc. can be used suitably.
2.積層体
積層体は、前述した粘着シート又はその硬化物を備える。なお、粘着シートが剥離シートを備える場合は、当該剥離シートが剥離された状態で積層体に存在する。つまり、積層体は前記粘着剤層を備えているということができる。
2. Laminated body The laminated body includes the above-mentioned pressure-sensitive adhesive sheet or a cured product thereof. When the pressure-sensitive adhesive sheet includes a release sheet, the release sheet is present in the laminated body in a peeled state. That is, it can be said that the laminate has the pressure-sensitive adhesive layer.
積層体は、粘着シートの両面に被着体を備えることができる。粘着シートが両面粘着シートである場合、2つの被着体を後硬化前の粘着シートで貼合した状態で活性エネルギー線を照射して、粘着剤層を後硬化することで積層体を形成することが好ましい。ここで、被着体は、基材及び光学部材であることがより好ましく、ポリカーボネートフィルム、偏光板、透明フィルム、透明樹脂またはガラスであることが特に好ましい。 The laminate can be provided with adherends on both sides of the adhesive sheet. When the pressure-sensitive adhesive sheet is a double-sided pressure-sensitive adhesive sheet, two adherends are pasted with the pressure-sensitive adhesive sheet before post-curing to irradiate active energy rays, and the pressure-sensitive adhesive layer is post-cured to form a laminate. It is preferable. Here, the adherend is more preferably a substrate and an optical member, and particularly preferably a polycarbonate film, a polarizing plate, a transparent film, a transparent resin or glass.
図2は、積層体の一例の断面を表す概略図である。図2は、本発明の粘着シート21を基材22と光学部材24に貼合した積層体20の構成の一例を表す断面図である。図2に示されているように、本発明の粘着シート21は、基材22に貼合するために用いられることが好ましく、基材22と他の光学部材24の貼合に用いられることが好ましい。なお、本発明の粘着シート21は、偏光板との貼合に用いられてもよい。 FIG. 2 is a schematic view showing a cross section of an example of the laminated body. FIG. 2 is a cross-sectional view showing an example of the configuration of the laminate 20 in which the pressure-sensitive adhesive sheet 21 of the present invention is attached to the base material 22 and the optical member 24. As shown in FIG. 2, the pressure-sensitive adhesive sheet 21 of the present invention is preferably used for bonding to the base material 22, and is used for bonding the base material 22 and the other optical member 24. preferable. The pressure-sensitive adhesive sheet 21 of the present invention may be used for bonding with a polarizing plate.
積層体に含まれる光学部材としては、タッチパネルや画像表示装置等の光学製品における各構成部材や最表層のカバーレンズに貼合される飛散防止フィルム等を挙げることができる。タッチパネルの構成部材としては、例えば透明樹脂フィルムにITO膜が設けられたITOフィルム、ガラス板の表面にITO膜が設けられたITOガラス、透明樹脂フィルムに導電性ポリマーをコーティングした透明導電性フィルム、ハードコートフィルム、耐指紋性フィルムなどが挙げられる。画像表示装置の構成部材としては、例えば液晶表示装置に用いられる反射防止フィルム、配向フィルム、偏光フィルム、位相差フィルム、輝度向上フィルムなどが挙げられる。 Examples of the optical member included in the laminated body include various constituent members in optical products such as a touch panel and an image display device, and an anti-scattering film attached to the cover lens of the outermost layer. As a component of the touch panel, for example, an ITO film provided with an ITO film on a transparent resin film, an ITO glass provided with an ITO film on the surface of a glass plate, a transparent conductive film obtained by coating a conductive polymer on a transparent resin film, A hard coat film, a fingerprint resistant film and the like can be mentioned. Examples of constituent members of the image display device include an antireflection film, an alignment film, a polarizing film, a retardation film, and a brightness enhancement film used in a liquid crystal display device.
これらの部材に用いられる材料としては、ガラス、ポリカーボネート、ポリエチレンテレフタレート、ポリメチルメタクリレート、ポリエチレンナフタレート、シクロオレフィンポリマー、トリアセチルセルロース,ポリイミド、セルロースアシレートなどが挙げられる。 Examples of materials used for these members include glass, polycarbonate, polyethylene terephthalate, polymethyl methacrylate, polyethylene naphthalate, cycloolefin polymer, triacetyl cellulose, polyimide, and cellulose acylate.
積層体は、前述のように、粘着シートの少なくとも一方の面側に被着体を積層する工程、及び前記粘着シートの粘着剤層に活性エネルギー線を照射することにより前記粘着剤層を後硬化させる工程を備える製造方法により得ることができる。 As described above, the laminate is a step of laminating the adherend on at least one surface side of the pressure-sensitive adhesive sheet, and post-curing the pressure-sensitive adhesive layer by irradiating the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet with active energy rays. It can be obtained by a manufacturing method including a step of
以下、実施例により本発明をより具体的に説明するが、本発明はこれら実施例の態様に限定されるものではない。 Hereinafter, the present invention will be described more specifically by way of examples, but the present invention is not limited to the modes of these examples.
粘着剤組成物の調製例
(調製例1)
ポリオレフィンとして、エチレン・プロピレンゴム(JSR社製「T7241」)を100質量部、粘着付与剤として、三井化学社製「FTR8120」を50質量部、アクリル系多官能モノマーとして、共栄社化学社製「ライトアクリレートDCP−A」(ジメチロールトリシクロデカンジアクリレート)を3質量部、アクリル系単官能モノマーとして、大阪有機化学工業社製「IBXA」(イソボルニルアクリレート)を3質量部、及び、水素引抜型開始剤として、LAMBSON社製「4MBP」(4−メチルベンゾフェノン)を1質量部、それぞれ混合することで粘着剤組成物を得た。
Preparation Example of Adhesive Composition (Preparation Example 1)
100 parts by mass of ethylene/propylene rubber (“T7241” manufactured by JSR) as a polyolefin, 50 parts by mass of “FTR8120” manufactured by Mitsui Chemicals, Inc. as a tackifier, and “light” manufactured by Kyoeisha Chemical Co., Ltd. as an acrylic polyfunctional monomer. 3 parts by mass of acrylate DCP-A" (dimethyloltricyclodecane diacrylate), 3 parts by mass of "IBXA" (isobornyl acrylate) manufactured by Osaka Organic Chemical Industry as an acrylic monofunctional monomer, and hydrogen abstraction An adhesive composition was obtained by mixing 1 part by mass of "4MBP" (4-methylbenzophenone) manufactured by LAMBSON Co., Ltd. as a mold initiator.
(調製例2)
アクリル系多官能モノマーをビスフェノールA エチレンオキサイド変性ジアクリレート(東亞合成(株)製、アロニックスM−211B)に変更したこと以外は調製例1と同様の方法で粘着剤組成物を得た。
(Preparation example 2)
A pressure-sensitive adhesive composition was obtained in the same manner as in Preparation Example 1 except that the acrylic polyfunctional monomer was changed to bisphenol A ethylene oxide-modified diacrylate (Aronix M-211B manufactured by Toagosei Co., Ltd.).
(調製例3)
アクリル系多官能モノマーとアクリル系単官能モノマーの添加量をいずれも5質量部に変更した以外は調製例1と同様の方法で粘着剤組成物を得た。
(Preparation example 3)
An adhesive composition was obtained in the same manner as in Preparation Example 1 except that the amounts of the acrylic polyfunctional monomer and the acrylic monofunctional monomer were both changed to 5 parts by mass.
(調製例4)
アクリル系多官能モノマーとアクリル系単官能モノマーの添加量をいずれも5質量部に変更した以外は調製例3と同様の方法で粘着剤組成物を得た。
(Preparation example 4)
A pressure-sensitive adhesive composition was obtained in the same manner as in Preparation Example 3, except that the addition amounts of both the acrylic polyfunctional monomer and the acrylic monofunctional monomer were changed to 5 parts by mass.
(調製例5)
アクリル系多官能モノマーとアクリル系単官能モノマーの添加量をいずれも15質量部に変更した以外は調製例1と同様の方法で粘着剤組成物を得た。
(Preparation example 5)
An adhesive composition was obtained in the same manner as in Preparation Example 1 except that the addition amounts of both the acrylic polyfunctional monomer and the acrylic monofunctional monomer were changed to 15 parts by mass.
(調製例6)
アクリル系多官能モノマー及びアクリル系単官能モノマー並びに水素引抜開始剤を使用しなかったこと以外は調製例1と同様の方法で粘着剤組成物を得た。
(Preparation example 6)
An adhesive composition was obtained in the same manner as in Preparation Example 1 except that the acrylic polyfunctional monomer, the acrylic monofunctional monomer and the hydrogen abstraction initiator were not used.
(調製例7)
アクリル系重合体として、綜研化学社製「SK2094」100質量部と、粘着付与剤として、三井化学社製「FTR8120」50質量部と、水素引抜型開始剤として、LAMBSON社製「4MBP」1質量部とをそれぞれ混合することで、粘着剤組成物を得た。
(Preparation example 7)
100 parts by mass of "SK2094" manufactured by Soken Chemical Industry Co., Ltd. as an acrylic polymer, 50 parts by mass of "FTR8120" manufactured by Mitsui Chemicals Co., Ltd. as a tackifier, and 1 mass of "4MBP" manufactured by LAMBSON as a hydrogen abstraction initiator. A pressure-sensitive adhesive composition was obtained by mixing each of these parts with each other.
粘着剤層の形成(粘着シートの作製)
(実施例1)
調製例1で得た粘着剤組成物を用いて粘着剤層を形成した。第1の剥離シートとして、シリコーン系剥離剤で処理された易接着剤層を備えた厚さ100μmのポリエチレンテレフタレートフィルム(重セパレータフィルム、帝人デュポンフィルム(株)製、離型処理されたポリエチレンテレフタレートフィルム)を準備した。この第1の剥離シートの易接着剤層側の面に、乾燥後の塗工厚みが所望の値(20μm又は100μm)となるように、調製例1で得た粘着剤組成物を、ヨシミツ精機株式会社製「ドクターブレードYD型」にて均一に塗工し、粘着剤組成物の塗膜を作製した後、100℃の空気循環式恒温オーブンで3分間乾燥処理することで、第1の剥離シートの表面に粘着剤層を形成した。
Formation of adhesive layer (preparation of adhesive sheet)
(Example 1)
A pressure-sensitive adhesive layer was formed using the pressure-sensitive adhesive composition obtained in Preparation Example 1. As the first release sheet, a polyethylene terephthalate film having a thickness of 100 μm and provided with an easily adhesive layer treated with a silicone release agent (heavy separator film, manufactured by Teijin DuPont Films Ltd., release-treated polyethylene terephthalate film) ) Prepared. The pressure-sensitive adhesive composition obtained in Preparation Example 1 was applied to the surface of the first release sheet on the easy-adhesive layer side so that the coating thickness after drying would be a desired value (20 μm or 100 μm). Coated evenly with "Dr. Blade YD type" manufactured by Co., Ltd. to prepare a coating film of the pressure-sensitive adhesive composition, and then dried for 3 minutes in an air-circulating constant temperature oven at 100° C. for the first peeling. An adhesive layer was formed on the surface of the sheet.
次いで、第1の剥離シートより剥離性の高い離型処理が施された厚さ75μmの第2の剥離シート(軽セパレータフィルム、帝人デュポンフィルム(株)製、離型処理されたポリエチレンテレフタレートフィルム)を準備した。この第2の剥離シートを、第1の剥離シートの表面に形成されている粘着剤層の上に貼り合わせた。これにより、粘着剤層が剥離力差のある1対の剥離シートに挟まれた第1の剥離シート/粘着剤層(A−1)/第2の剥離シートの構成の剥離シート付き粘着シートが得られた。 Then, a second release sheet having a thickness of 75 μm and subjected to a release treatment having higher release property than the first release sheet (light separator film, manufactured by Teijin DuPont Films Ltd., release-treated polyethylene terephthalate film) Prepared. This second release sheet was laminated on the pressure-sensitive adhesive layer formed on the surface of the first release sheet. Thereby, the pressure-sensitive adhesive sheet with the release sheet having the structure of the first release sheet/the pressure-sensitive adhesive layer (A-1)/the second release sheet in which the pressure-sensitive adhesive layer is sandwiched between the pair of release sheets having different release forces is obtained. Was obtained.
(実施例2)
調製例1で得た粘着剤組成物を調製例2で得た粘着剤組成物に変更したこと以外は実施例1と同様の方法で剥離シート付き粘着シートを得た。
(Example 2)
A pressure-sensitive adhesive sheet with a release sheet was obtained in the same manner as in Example 1 except that the pressure-sensitive adhesive composition obtained in Preparation Example 1 was changed to the pressure-sensitive adhesive composition obtained in Preparation Example 2.
(実施例3)
調製例1で得た粘着剤組成物を調製例3で得た粘着剤組成物に変更したこと以外は実施例1と同様の方法で剥離シート付き粘着シートを得た。
(Example 3)
A pressure-sensitive adhesive sheet with a release sheet was obtained in the same manner as in Example 1 except that the pressure-sensitive adhesive composition obtained in Preparation Example 1 was changed to the pressure-sensitive adhesive composition obtained in Preparation Example 3.
(実施例4)
調製例1で得た粘着剤組成物を調製例4で得た粘着剤組成物に変更したこと以外は実施例1と同様の方法で剥離シート付き粘着シートを得た。
(Example 4)
A pressure-sensitive adhesive sheet with a release sheet was obtained in the same manner as in Example 1 except that the pressure-sensitive adhesive composition obtained in Preparation Example 1 was changed to the pressure-sensitive adhesive composition obtained in Preparation Example 4.
(比較例1)
調製例1で得た粘着剤組成物を調製例5で得た粘着剤組成物に変更したこと以外は実施例1と同様の方法で剥離シート付き粘着シートを得た。
(Comparative Example 1)
A pressure-sensitive adhesive sheet with a release sheet was obtained in the same manner as in Example 1 except that the pressure-sensitive adhesive composition obtained in Preparation Example 1 was changed to the pressure-sensitive adhesive composition obtained in Preparation Example 5.
(比較例2)
調製例1で得た粘着剤組成物を調製例6で得た粘着剤組成物に変更したこと以外は実施例1と同様の方法で剥離シート付き粘着シートを得た。
(Comparative example 2)
A pressure-sensitive adhesive sheet with a release sheet was obtained in the same manner as in Example 1 except that the pressure-sensitive adhesive composition obtained in Preparation Example 1 was changed to the pressure-sensitive adhesive composition obtained in Preparation Example 6.
(比較例3)
調製例1で得た粘着剤組成物を調製例7で得た粘着剤組成物に変更したこと、および剥離シート付き粘着シートを23℃、相対湿度50%の条件で7日間静置して、エージング処理を行った以外は実施例1と同様の方法で剥離シート付き粘着シートを得た。
(Comparative example 3)
The pressure-sensitive adhesive composition obtained in Preparation Example 1 was changed to the pressure-sensitive adhesive composition obtained in Preparation Example 7, and the pressure-sensitive adhesive sheet with a release sheet was allowed to stand for 7 days at 23° C. and 50% relative humidity, A pressure-sensitive adhesive sheet with a release sheet was obtained in the same manner as in Example 1 except that the aging treatment was performed.
(評価方法)
<引張試験測定>
引張試験はJIS K 7161−1に準拠して、粘着剤層の破断伸度及びひずみ1000%での応力を測定した。具体的に引張試験は、引張速度は10mm/minとし、23℃、相対湿度50%の環境下で測定した。また、測定サンプルは、厚さ20μm、幅60mm、長さ250mmの後硬化の粘着剤層を、長さ方向に丸めて断面積5mm2、高さ60mmの円柱形状に加工して用いた。チャック間距離が30mmとなるようサンプルをセットして引っ張り、測定サンプルのひずみが1000%となったときの応力値及び測定サンプルが破断した時の伸度(破断伸度)を計測した。引張試験には、島津製作所製のオートグラフAGS−Xを用いた。
(Evaluation method)
<Tensile test measurement>
In the tensile test, the breaking elongation of the pressure-sensitive adhesive layer and the stress at a strain of 1000% were measured according to JIS K7161-1. Specifically, in the tensile test, the tensile speed was set to 10 mm/min, and measurement was performed in an environment of 23° C. and relative humidity of 50%. The measurement sample was used by processing a post-cured pressure-sensitive adhesive layer having a thickness of 20 μm, a width of 60 mm, and a length of 250 mm into a columnar shape having a cross-sectional area of 5 mm 2 and a height of 60 mm by rolling in the length direction. The sample was set and pulled so that the distance between chucks was 30 mm, and the stress value when the strain of the measurement sample was 1000% and the elongation at break of the measurement sample (breaking elongation) were measured. Shimadzu autograph AGS-X was used for the tensile test.
<透湿度測定>
透湿度(g/m2・24hr)は、日本国特許第5089809に記載の方法を参照する。具体的には以下の方法で透湿度を測定した。
100μm厚みの後硬化後の粘着剤層を裏材(旭化成社製「BEMCOT M−1」)に積層して透湿度を測定するためのサンプルを得た。このサンプルを、小数点以下3桁までの重さを正確に秤量した50gの蒸留水が入った直径2.54cmの開口部付きガラス瓶の最上部に、前記粘着剤層がガラス瓶の底側に対向するように設置した。前記粘着剤層を、オープンリングカバーで定位置に保持しつつ、隙間から水蒸気等が外部へ漏れないように粘着剤層によりガラス容器の内部を密封した後、このガラス瓶(粘着剤層を備えたガラス瓶)を、相対湿度20%で40℃に設定したオーブンに約24時間、当該ガラス瓶を直立(このとき、水がサンプルに触れない)にして設置した。その後、粘着剤層を備えたガラス瓶の重量喪失を計測し、この重量喪失から透湿度(g/m2・24hr)を算出した。なお、粘着剤層の厚み(100μm)は、粘着剤組成物の塗布量から見積もった。
<Measurement of moisture permeability>
For the moisture vapor transmission rate (g/m 2 ·24 hr), refer to the method described in Japanese Patent No. 5089809. Specifically, the water vapor permeability was measured by the following method.
A pressure-sensitive adhesive layer after post-curing having a thickness of 100 μm was laminated on a backing material (“BEMCOT M-1” manufactured by Asahi Kasei Corp.) to obtain a sample for measuring moisture permeability. This sample is placed on the top of a glass bottle with an opening having a diameter of 2.54 cm and containing 50 g of distilled water in which the weight up to three decimal places is accurately weighed, and the adhesive layer faces the bottom side of the glass bottle. Was installed. While holding the pressure-sensitive adhesive layer in place with an open ring cover, the inside of the glass container was sealed with the pressure-sensitive adhesive layer so that water vapor and the like would not leak to the outside from the gap, and then this glass bottle (including the pressure-sensitive adhesive layer The glass bottle) was placed in an oven set at 40° C. with a relative humidity of 20% for about 24 hours with the glass bottle standing upright (where water does not touch the sample). Then, the weight loss of the glass bottle provided with the adhesive layer was measured, and the moisture vapor transmission rate (g/m 2 ·24 hr) was calculated from the weight loss. The thickness (100 μm) of the pressure-sensitive adhesive layer was estimated from the coating amount of the pressure-sensitive adhesive composition.
<耐久性>
粘着剤層の軽セパレータフィルムである第2の剥離シートを剥がし、偏光板(ポラテクノ(株)製、SKN−18243T)に貼合した。次に重セパレータフィルムである第1の剥離シートを剥がし、PCフィルム(帝人社製、ピュアエースGS)に貼着した。偏光板/粘着剤層/PCフィルムの構成のサンプルをオートクレーブ処理(40℃、0.5MPa、30min)し、次いで、PCフィルム側より紫外線を積算光量が3000mJ/cm2となるように照射し、100mm×200mmの大きさの試験サンプルを得た。その後、試験サンプルを60℃,相対湿度95%の環境下に240時間静置した。その後、試験サンプルを観察し、浮き及び剥がれの発生の有無を観察し、それぞれ下記の判定基準で評価した。
≪気泡≫
○:最大長さが0.2mm以上である気泡の発生は見られなかった。
×:最大長さが0.2mm以上の気泡の発生が見られた。
≪剥がれ≫
○:1.0mm以上の剥がれが観察されなかった。
×:1.0mm以上の剥がれが観察された。
<Durability>
The second release sheet, which is a light separator film for the pressure-sensitive adhesive layer, was peeled off and attached to a polarizing plate (SKN-18243T manufactured by Polatechno Co., Ltd.). Next, the first release sheet, which is a heavy separator film, was peeled off and attached to a PC film (Pure Ace GS manufactured by Teijin Ltd.). The sample having the configuration of polarizing plate/adhesive layer/PC film was autoclaved (40° C., 0.5 MPa, 30 min), and then irradiated with ultraviolet rays from the PC film side so that the integrated light amount was 3000 mJ/cm 2 . A test sample with a size of 100 mm×200 mm was obtained. Then, the test sample was left to stand in an environment of 60° C. and 95% relative humidity for 240 hours. Then, the test sample was observed, and the presence or absence of floating and peeling was observed, and each was evaluated according to the following criteria.
<<Bubbles>>
◯: No generation of bubbles having a maximum length of 0.2 mm or more was observed.
X: Generation of bubbles having a maximum length of 0.2 mm or more was observed.
≪Peeling off≫
◯: No peeling of 1.0 mm or more was observed.
X: Peeling of 1.0 mm or more was observed.
<剪断貯蔵弾性率G’の測定>
剪断貯蔵弾性率G’は、動的粘弾性装置Rheogel―E4000(株式会社ユービーエム製)を用いて測定した。固体剪断モード、周波数1Hz、歪み1.0%の条件で、20℃〜120℃までの温度領域における粘着剤層の剪断貯蔵弾性率G’を測定し、23℃及び85℃における剪断貯蔵弾性率G’の値を算出した。測定は、実施例及び比較例で得た粘着シートの粘着剤層に、セパレータが付いた状態で紫外線を積算光量が3000mJ/cm2となるように照射して後硬化させてから行った。
<Measurement of shear storage elastic modulus G'>
The shear storage elastic modulus G′ was measured using a dynamic viscoelastic device Rheogel-E4000 (manufactured by UBM Co., Ltd.). The shear storage elastic modulus G′ of the pressure-sensitive adhesive layer in the temperature range from 20° C. to 120° C. was measured under the conditions of solid shear mode, frequency 1 Hz, and strain 1.0%, and the shear storage elastic modulus at 23° C. and 85° C. The value of G'was calculated. The measurement was performed after irradiating the pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets obtained in Examples and Comparative Examples with ultraviolet rays so that the integrated light amount was 3000 mJ/cm 2 with the separator attached, and post-curing.
(評価結果)
表1は、各実施例及び比較例で使用した粘着剤組成物の成分及び含有割合を示している。あわせて表1には、各実施例及び比較例で得られた粘着剤層の剪断貯蔵弾性率G’、透湿度、引張試験結果及び耐久性評価の結果を示している。
(Evaluation results)
Table 1 shows the components and the content ratios of the pressure-sensitive adhesive compositions used in each example and comparative example. In addition, Table 1 shows the shear storage elastic modulus G′, the moisture permeability, the tensile test result, and the durability evaluation result of the pressure-sensitive adhesive layers obtained in each Example and Comparative Example.
各実施例で得られた粘着シートは低い透湿性を有し、かつ、気泡及び剥がれも発生しにくかったことから、優れた耐久性を有していた。一方、比較例1の粘着シートは、粘着剤層に含まれる(メタ)アクリル系モノマーが多すぎることから、低い透湿性を得ることができず、また、剥がれが発生しやすかった。比較例2の粘着シートは、(メタ)アクリル系モノマーを含まないため、伸度1000%での応力が小さく、気泡が発生しやすかった。比較例3の粘着シートは、粘着剤層がポリオレフィンを含まないので、物性(1)及び(2)を満たすことができず、耐久性が悪いものであった。 The pressure-sensitive adhesive sheets obtained in the respective examples had low moisture permeability and were resistant to bubbles and peeling, and thus had excellent durability. On the other hand, in the pressure-sensitive adhesive sheet of Comparative Example 1, since the (meth)acrylic monomer contained in the pressure-sensitive adhesive layer was too much, low moisture permeability could not be obtained, and peeling easily occurred. Since the pressure-sensitive adhesive sheet of Comparative Example 2 did not contain a (meth)acrylic monomer, the stress at an elongation of 1000% was small and air bubbles were easily generated. In the pressure-sensitive adhesive sheet of Comparative Example 3, since the pressure-sensitive adhesive layer did not contain polyolefin, the physical properties (1) and (2) could not be satisfied, and the durability was poor.
Claims (8)
前記(メタ)アクリル系モノマーが、分子内に重合性官能基を2つ以上有する多官能モノマーと、分子内に重合性官能基を1つのみ有する単官能モノマーとの混合物であり、
活性エネルギー線を積算光量が3000mJ/cm2となるように照射して後硬化した場合に下記物性(1)及び(2)
物性(1):引張速度10mm/minの引張試験測定において、破断伸度が1200%以上であり、かつ、ひずみ1000%での応力が0.40N/mm2以上である、
物性(2):100μmの厚みでの透湿度が50g/m2・24hr以下である、
を満たす、粘着剤層。 A pressure-sensitive adhesive composition containing a polyolefin, a (meth)acrylic monomer, and a hydrogen abstraction-type initiator,
The (meth)acrylic monomer is a mixture of a polyfunctional monomer having two or more polymerizable functional groups in the molecule and a monofunctional monomer having only one polymerizable functional group in the molecule,
The following physical properties (1) and (2) are obtained when the active energy ray is irradiated so that the integrated light amount becomes 3000 mJ/cm 2 and post-cured.
Physical properties (1): In a tensile test measurement at a tensile speed of 10 mm/min, the breaking elongation is 1200% or more, and the stress at a strain of 1000% is 0.40 N/mm 2 or more,
Physical properties (2): Water vapor permeability at a thickness of 100 μm is 50 g/m 2 ·24 hr or less,
Adhesive layer that fills.