JP3432774B2 - Toner production method - Google Patents

Toner production method

Info

Publication number
JP3432774B2
JP3432774B2 JP24624499A JP24624499A JP3432774B2 JP 3432774 B2 JP3432774 B2 JP 3432774B2 JP 24624499 A JP24624499 A JP 24624499A JP 24624499 A JP24624499 A JP 24624499A JP 3432774 B2 JP3432774 B2 JP 3432774B2
Authority
JP
Japan
Prior art keywords
toner
roll
charge control
control agent
weight
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
JP24624499A
Other languages
Japanese (ja)
Other versions
JP2001075307A (en
Inventor
泰久 大谷
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kao Corp
Original Assignee
Kao Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kao Corp filed Critical Kao Corp
Priority to JP24624499A priority Critical patent/JP3432774B2/en
Publication of JP2001075307A publication Critical patent/JP2001075307A/en
Application granted granted Critical
Publication of JP3432774B2 publication Critical patent/JP3432774B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【発明の属する技術分野】本発明は電子写真法、静電印
刷法及び磁気記録法等に用いられるトナーの製造方法に
関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a method for producing a toner used in electrophotography, electrostatic printing, magnetic recording and the like.

【0002】[0002]

【従来の技術】トナーの性能に関する要素として、帯電
量制御とワックスなどの添加剤の分散度制御がある。ト
ナー粒子内の各種原料の分散状態は、粉砕法によるトナ
ーの製造方法においては、原料を混合する工程と混練す
る工程とによって、実質的に決定される。しかし、例え
ば、特許第2677685号公報のような押出機を用い
た方法では、混練熱による組成物の温度上昇に伴い、ト
ナーとして要求される荷電制御剤、ワックス等の分散を
十分に行うことができないという問題を有する。
2. Description of the Related Art As factors relating to toner performance, there are charge amount control and dispersion degree control of additives such as wax. The dispersion state of various raw materials in the toner particles is substantially determined by the step of mixing the raw materials and the step of kneading the raw materials in the method for producing the toner by the pulverization method. However, for example, in the method using an extruder as disclosed in Japanese Patent No. 2677685, it is possible to sufficiently disperse the charge control agent, wax and the like required as a toner as the temperature of the composition rises due to the heat of kneading. I have a problem that I can't.

【0003】[0003]

【発明が解決しようとする課題】本発明は、着色剤の分
散に優れ、荷電制御剤、ワックスの分散度を制御したト
ナーを製造する方法を提供することを目的とする。
SUMMARY OF THE INVENTION It is an object of the present invention to provide a method for producing a toner which is excellent in the dispersion of a colorant and in which the dispersion degree of a charge control agent and a wax is controlled.

【0004】[0004]

【課題を解決するための手段】即ち、本発明の要旨は、
予め着色剤を結着樹脂に溶融混合した混練物と結着樹脂
と荷電制御剤とを含有する組成物を加熱及び冷却機能を
有するオープンロール型連続混練機を用いて溶融混練す
る工程を有するトナーの製造方法であって、前記溶融混
練に際して、該混練機のロールの軸方向に沿って複数の
位置に供給口を設け、前記混練物と結着樹脂と荷電制御
剤とを該混練機の入り口側のロール端部0L(但し、L
はロール長さを示す)〜0.9Lの位置から連続的に供
給して溶融混練を行う、トナーの製造方法に関する。
The summary of the present invention is as follows.
A toner having a step of melt-kneading a kneaded product obtained by previously melting and mixing a colorant with a binder resin and a composition containing a binder resin and a charge control agent using an open roll type continuous kneader having a heating and cooling function. In the melt kneading, the supply port is provided at a plurality of positions along the axial direction of the roll of the kneading machine, and the kneaded material, the binder resin, and the charge control agent are introduced into the kneading machine. Side roll end 0L (however, L
Is a roll length) to 0.9 L and is continuously supplied for melt kneading.

【0005】[0005]

【発明の実施の形態】また、本発明のトナーの製造方法
においては、溶融混練する際に加熱及び冷却機能を有す
るオープンロール型連続混練機を用い、かつ複数の供給
口から原料を供給する点に一つの大きな特徴がある。こ
れにより、荷電制御剤等の分散度を容易に制御でき、安
定した荷電特性を有するトナーを容易に製造することが
できるという優れた効果を発現する。
BEST MODE FOR CARRYING OUT THE INVENTION In the method for producing a toner according to the present invention, an open roll type continuous kneader having a heating and cooling function at the time of melt kneading is used, and raw materials are fed from a plurality of feeding ports. There is one big feature in. Thereby, the excellent effect that the degree of dispersion of the charge control agent and the like can be easily controlled and the toner having stable charging characteristics can be easily manufactured is exhibited.

【0006】本発明に用いられるオープンロール型連続
混練機は、2本のロールが並行に近接して配設されたオ
ープンロール型連続混練機に、ロールの軸方向に沿って
複数の位置に原料の供給口を設けたものが使用される。
各ロールは、熱媒体を通すことにより加熱又は冷却を行
うことができる。即ち、一方を加熱ロールとし、結着樹
脂の溶融温度付近の温度に調節し、もう一方のロールを
冷却ロールとし、結着樹脂の溶融温度以下の温度に調節
する。なお、溶融温度(Tm)は、高化式フローテスタ
ー(CFT−500、島津製作所(株)製)を用い、ダ
イスの細孔の径1mm、長さ1mm、荷重20kg/c
2 (196N/cm2 )、昇温速度6℃/minの条
件下で1cm3 の試料を溶融流出させたときの流出開始
点から流出終了点の高さの1/2に相当する温度とす
る。
The open roll type continuous kneader used in the present invention is an open roll type continuous kneader in which two rolls are arranged in parallel and close to each other, and raw materials are provided at a plurality of positions along the axial direction of the roll. The one provided with the supply port of is used.
Each roll can be heated or cooled by passing a heat medium. That is, one of the rolls is used as a heating roll, and the temperature is adjusted to a temperature near the melting temperature of the binder resin, and the other roll is used as a cooling roll and adjusted to a temperature equal to or lower than the melting temperature of the binder resin. The melting temperature (Tm) used was a Koka type flow tester (CFT-500, manufactured by Shimadzu Corporation), and the diameter of the pores of the die was 1 mm, the length was 1 mm, and the load was 20 kg / c.
m 2 (196 N / cm 2 ) and a temperature corresponding to ½ of the height from the outflow start point to the outflow end point when a 1 cm 3 sample is melted and flown out under the condition of a temperature rising rate of 6 ° C./min. To do.

【0007】2本のロールの間隙は、好ましくは0.1
〜10mm、更に好ましくは0.1〜3mmである。ま
た、各ロールの構造、大きさ、材料等について特に限定
はなく、ロール表面は、平滑であってもよく、波型、凸
凹型等であってもよい。
The gap between the two rolls is preferably 0.1.
10 mm, more preferably 0.1 to 3 mm. Further, the structure, size, material, etc. of each roll are not particularly limited, and the roll surface may be smooth, corrugated, or uneven.

【0008】2本のロールを内方向、逆の方向に回転さ
せながら、ロールの軸方向に沿って複数の位置に設けら
れた供給口からロール上面又は2本のロールの間に原料
を供給することで、混練を行うことが好ましい。
While rotating the two rolls in the opposite direction, the raw material is supplied from the supply ports provided at a plurality of positions along the axial direction of the roll to the upper surface of the roll or between the two rolls. Therefore, it is preferable to carry out kneading.

【0009】その際のロールの回転数は、周速度2〜1
00m/minであることが好ましく、2本のロールの
回転数比(冷却ロールの回転数/加熱ロールの回転数)
は、1/10〜9/10であることが好ましい。
The number of rotations of the roll at that time is such that the peripheral speed is 2-1
The rotation speed ratio of the two rolls is preferably 00 m / min (cooling roll rotation speed / heating roll rotation speed)
Is preferably 1/10 to 9/10.

【0010】また、混練温度と、ロール回転数とを適宜
調節することにより所望の混練力を得ることができる。
A desired kneading force can be obtained by appropriately adjusting the kneading temperature and the number of roll rotations.

【0011】なお、オープンロール型連続混練機へ原料
を供給するには、例えば、テーブルフィーダー等を用い
て行う。
The raw material is supplied to the open roll type continuous kneader by using, for example, a table feeder.

【0012】また、原料を供給する前に、各原料を混合
装置を用いて予備混合してもよい。混合装置としては、
特に限定するものではなく、ヘンシェルミキサー(三井
鉱山製)、スーパーミキサー(カワタ製)、ハイスピー
ドミキサー(深江工業製)等の高速攪拌型混合装置が挙
げられる。
Before the raw materials are supplied, the raw materials may be premixed by using a mixing device. As a mixing device,
It is not particularly limited, and examples thereof include a high-speed stirring type mixing device such as a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.), a super mixer (manufactured by Kawata), and a high speed mixer (manufactured by Fukae Kogyo).

【0013】また、本発明のトナーの製造方法において
は、前記オープンロール型連続混練機を用いて溶融混練
するに際して、マスターバッチのように予め、着色剤を
結着樹脂に溶融混合した混練物を用いる点にも一つの大
きな特徴がある。かかる混練物を用いることにより、結
着樹脂中に着色剤等を十分に分散させることができると
いう優れた効果を発現する。
Further, in the method for producing a toner of the present invention, when melt-kneading using the open roll type continuous kneader, a kneaded product obtained by previously melt-mixing a colorant with a binder resin like a master batch is used. There is one major feature in the point of use. By using such a kneaded product, the excellent effect that the colorant and the like can be sufficiently dispersed in the binder resin is exhibited.

【0014】本発明に用いられる結着樹脂としては、特
に限定されるものではなく、黒トナー又はカラートナー
用の公知の結着樹脂を使用することができ、例えば、特
開平7−98518号公報第3頁第4欄第37行〜第6
頁第10欄第10行に記載のポリエステル樹脂、ビニル
樹脂等の結着樹脂や、原料モノマー混合物に離型剤を混
合し、重合反応で得られた結着樹脂を用いても良い。
The binder resin used in the present invention is not particularly limited, and known binder resins for black toner or color toner can be used. For example, JP-A-7-98518. Page 3, Column 4, Lines 37-6
Binder resins such as polyester resin and vinyl resin described in page 10, column 10 line, or binder resins obtained by polymerization reaction by mixing a release agent with a raw material monomer mixture may be used.

【0015】前記混練物中の結着樹脂の含有量は、50
〜90重量%が好ましく、60〜80重量%がより好ま
しい。
The content of the binder resin in the kneaded product is 50.
Is preferably 90 to 90% by weight, more preferably 60 to 80% by weight.

【0016】また、荷電制御剤やワックス等を含有する
最終組成物中における50〜95重量%、より好ましく
は80〜95重量%である。なお、本発明において、結
着樹脂は、前記混練物中に含有させて用いると共に、前
記オープンロール型連続混練機に別途添加して使用され
る。
Further, it is 50 to 95% by weight, more preferably 80 to 95% by weight in the final composition containing the charge control agent, wax and the like. In the present invention, the binder resin is used by being contained in the kneaded product, and is also separately added to the open roll type continuous kneader.

【0017】着色剤としては、特に限定されるものでは
なく、黒トナー又はカラートナー用の公知の着色剤を使
用することができる。着色剤は、黒色着色剤、黄色顔
料、赤色若しくは紅色顔料、青色系顔料、緑色顔料等が
あり、これらの着色剤は単独で用いても2種以上混合し
て用いても良い。
The colorant is not particularly limited, and a known colorant for black toner or color toner can be used. Colorants include black colorants, yellow pigments, red or red pigments, blue pigments, green pigments, etc. These colorants may be used alone or in combination of two or more.

【0018】前記混練物中の着色剤の含有量は、10〜
50重量%が好ましく、20〜40重量%がより好まし
い。
The content of the colorant in the kneaded product is 10 to 10.
50 wt% is preferable, and 20-40 wt% is more preferable.

【0019】また、最終組成物中における着色剤の含有
量は、着色剤の含有量は、2〜15重量%が好ましく、
3〜10重量%がより好ましい。
The content of the colorant in the final composition is preferably 2 to 15% by weight,
3 to 10% by weight is more preferable.

【0020】前記混練物の製造方法としては、特に限定
はなく、例えば、加熱ロールミル、回分式ニーダー、2
軸押し出し機、オープンロール型連続混練機等の公知の
製造装置を用いて、結着樹脂の溶融温度(Tm)に対し
て、Tm−20℃〜Tm+50℃でマスターバッチを行
えばよい。
The method for producing the kneaded product is not particularly limited, and examples thereof include a heating roll mill, a batch kneader, and
A masterbatch may be performed at a temperature of Tm-20 ° C to Tm + 50 ° C with respect to the melting temperature (Tm) of the binder resin using a known manufacturing apparatus such as an axial extruder or an open roll type continuous kneader.

【0021】前記混練物及び結着樹脂のオープンロール
型連続混練機への供給は、着色剤の分散度をより向上さ
せる観点から、0L〜0.9Lの位置、好ましくは0L
〜0.5Lの位置、より好ましくは0L〜0.3Lの位
置の1箇所以上の供給口から行うことができる。
The kneaded product and the binder resin are supplied to the open roll type continuous kneader at a position of 0 L to 0.9 L, preferably 0 L, from the viewpoint of further improving the dispersity of the colorant.
It can be performed from one or more supply ports at a position of 0.5L, more preferably at a position of 0L to 0.3L.

【0022】荷電制御剤としては、特に限定されるもの
ではなく、黒トナー又はカラートナー用の公知の荷電制
御剤を使用することができる。負帯電トナー用の荷電制
御剤としては、クロム・アゾ錯体染料;鉄アゾ錯体染
料;コバルト・アゾ錯体染料;サリチル酸もしくはその
誘導体のクロム・亜鉛・アルミニウム・ホウ素錯体もし
くは塩化合物;ナフトール酸もしくはその誘導体のクロ
ム・亜鉛・アルミニウム・ホウ素錯体もしくは塩化合
物;ベンジル酸もしくはその誘導体のクロム・亜鉛・ア
ルミニウム・ホウ素錯体もしくは塩化合物;長鎖アルキ
ル・カルボン酸塩、長鎖アルキル・スルフォン酸塩など
の界面活性剤類等が挙げられる。また、正帯電トナー用
の荷電制御剤としては、ニグロシン染料及びその誘導
体、トリフェニルメタン誘導体、四級アンモニウム塩、
四級ホスフォニウム塩、四級ビリジニウム塩、グアニジ
ン塩、アミジン塩等の誘導体等が挙げられる。
The charge control agent is not particularly limited, and a known charge control agent for black toner or color toner can be used. As charge control agents for negatively charged toner, chromium / azo complex dyes; iron azo complex dyes; cobalt / azo complex dyes; chromium / zinc / aluminum / boron complexes or salicylic acid or its derivative compounds; naphtholic acid or its derivative compounds Chromium ・ Zinc ・ Aluminum ・ Boron Complex or Salt Compound; Chromium ・ Zinc ・ Aluminum ・ Boron Complex or Salt Compound of Benzyl Acid or its Derivatives; Long Chain Alkyl Carboxylate, Long Chain Alkyl Sulfonate, etc. Examples include agents. Further, as a charge control agent for positively charged toner, a nigrosine dye and its derivative, a triphenylmethane derivative, a quaternary ammonium salt,
Examples thereof include derivatives such as quaternary phosphonium salt, quaternary viridinium salt, guanidine salt and amidine salt.

【0023】荷電制御剤は、所望の分散度に合わせて、
0L〜0.9Lの位置、重複せず好ましくは0L〜0.
8Lの位置、より好ましくは0.2L〜0.7Lの位置
の1個所以上の供給口から供給する。また、荷電制御剤
を複数用いるとき、それぞれの目的の分散度に合わせ
て、その供給位置を変えることができる。なお、荷電制
御剤は、分散度を上げていくとその効果は上昇するもの
の、更にその分散度を上げすぎるとその効果は下降して
いく。従って、用いる荷電制御剤の最適な分散度となる
ように、平均粒径(荷電制御剤の分散粒径)を制御する
のが好ましく、荷電制御剤の混練物中における最適な平
均粒径は、0.1〜3μm、好ましくは0.1〜2μm
であることが望ましい。荷電制御剤を高分散させるため
には、オープンロール型連続混練機を用いる際に、混練
時の混合熱を除去し、混練物の粘度を上昇させて、より
強い分散力を生じさせるのが好ましい。該平均粒径は、
式(I):
The charge control agent is adjusted to a desired degree of dispersion,
Positions of 0L to 0.9L, preferably 0L to 0.
It is supplied from one or more supply ports at a position of 8L, more preferably at a position of 0.2L to 0.7L. When a plurality of charge control agents are used, the supply position can be changed according to the degree of dispersion for each purpose. The effect of the charge control agent increases as the degree of dispersion is increased, but the effect decreases as the degree of dispersion is further increased. Therefore, it is preferable to control the average particle size (dispersed particle size of the charge control agent) so that the charge control agent to be used has an optimum degree of dispersion, and the optimum average particle size in the kneaded material of the charge control agent is 0.1-3 μm, preferably 0.1-2 μm
Is desirable. In order to highly disperse the charge control agent, when using an open roll type continuous kneader, it is preferable to remove the heat of mixing during kneading and increase the viscosity of the kneaded product to generate a stronger dispersing force. . The average particle size is
Formula (I):

【0024】[0024]

【数1】 [Equation 1]

【0025】(a:粒子の長径〔μm〕、b:粒子の短
径〔μm〕、n:粒子の測定個数、なお、長径及び短径
は透過型電子顕微鏡で観察して得た。)で求めることが
できる。
(A: major axis of particle [μm], b: minor axis of particle [μm], n: number of measured particles, major axis and minor axis were obtained by observing with a transmission electron microscope). You can ask.

【0026】また、荷電制御剤の最終組成物中における
含有量は、電荷を付与することの観点から、0.1重量
%以上、好ましくは0.5重量%以上であることが望ま
しく、荷電制御及びトナーとしての透明性の観点から、
15重量%以下、好ましくは10重量%以下であること
が望ましい。
The content of the charge control agent in the final composition is preferably 0.1% by weight or more, and more preferably 0.5% by weight or more, from the viewpoint of imparting an electric charge. And from the viewpoint of transparency as a toner,
It is desirable that the content is 15% by weight or less, preferably 10% by weight or less.

【0027】また、本発明に用いられる組成物は、さら
にワックス等を含有してもよい。ワックスとしては、天
然ワックス及び合成ワックス類、シリコーン系、高級脂
肪酸、ポリオレフィン系、低分子重合体等が挙げられ
る。これらの中でも、天然ワックスが好適に用いられ、
具体的には、カルナバワックス、ライスワックス、キャ
ンデリラワックス、蜜ロウ等が挙げられる。
The composition used in the present invention may further contain wax and the like. Examples of waxes include natural waxes and synthetic waxes, silicone-based waxes, higher fatty acids, polyolefin-based waxes, and low molecular weight polymers. Among these, natural wax is preferably used,
Specific examples include carnauba wax, rice wax, candelilla wax, and beeswax.

【0028】ワックスは、所望の分散度に合わせて、0
L〜0.9Lの位置、好ましくは0L〜0.8Lの位
置、より好ましくは0L〜0.6Lの位置の1個所以上
の供給口から供給することが好ましい。また、ワックス
を複数用いるとき、それぞれの目的の分散度に合わせ
て、その供給位置を変えることができる。トナー中にお
けるワックスは、結着樹脂とは相溶せず分離した状態で
存在するため、ワックスの平均粒径(ワックスの分散粒
径)が大きすぎると、ワックスがトナー表面に現れ、現
像機内の感光体に付着したり、時間の経過と共に、帯電
量が低下し安定した現像が行えなくなる。一方、ワック
スの平均粒径が小さすぎると、定着時に、ワックスがブ
リードアウトする速度が遅くなり、オフセット防止剤と
して働かなくなる。そのため、前記式(1)で求められ
るワックスの平均粒径は、トナーの重量平均粒径(D)
に対して、0.1〜0.3Dμmであることが好まし
く、具体的には、0.5〜3μmであることが望まし
い。なお、トナーの重量平均粒径(D)は、コールター
カウンター(ベックマン・コールター社、アパチャー1
00μm)にて測定した。
The wax is 0 depending on the desired degree of dispersion.
It is preferable to supply from one or more supply ports at a position of L to 0.9L, preferably a position of 0L to 0.8L, and more preferably a position of 0L to 0.6L. When a plurality of waxes are used, the supply position can be changed according to the degree of dispersion for each purpose. The wax in the toner is incompatible with the binder resin and exists in a separated state. Therefore, if the average particle size of the wax (dispersed particle size of the wax) is too large, the wax appears on the toner surface, and If the toner adheres to the photoconductor or the time elapses, the charge amount decreases and stable development cannot be performed. On the other hand, if the average particle size of the wax is too small, the speed of bleeding out of the wax at the time of fixing becomes slow and the wax does not function as an offset preventing agent. Therefore, the average particle diameter of the wax obtained by the above formula (1) is the weight average particle diameter (D) of the toner.
On the other hand, it is preferably 0.1 to 0.3 Dm, and specifically, 0.5 to 3 m is desirable. The weight average particle diameter (D) of the toner is the Coulter counter (Beckman Coulter, Inc., Aperture 1).
00 μm).

【0029】また、ワックスの最終組成物中における含
有量は、良好なオフセット防止効果を発揮させる観点か
ら、1重量%以上、好ましくは3重量%以上であること
が望ましく、感光体へのフィルミング抑制の観点から、
20重量%以下、好ましくは15重量%以下であること
が望ましい。
The content of the wax in the final composition is preferably 1% by weight or more, and more preferably 3% by weight or more, from the viewpoint of exerting a good offset preventing effect. From the perspective of suppression
It is desired to be 20% by weight or less, preferably 15% by weight or less.

【0030】以上のような溶融混練の工程により得られ
た最終混練物は、オープンロール型連続混練機から連続
的に取り出すことができる。得られた最終混練物は、冷
却した後、固化し、粉砕し、分級するなど公知の工程で
さらに処理することにより、トナーを製造することがで
きる。
The final kneaded product obtained by the above melt kneading step can be continuously taken out from the open roll type continuous kneader. The final kneaded product thus obtained is cooled, then solidified, pulverized, and then further processed in a known step such as classification, whereby a toner can be produced.

【0031】冷却に用いられる冷却装置としては、例え
ば、冷却ベルト等が挙げられる。
Examples of the cooling device used for cooling include a cooling belt.

【0032】粉砕に用いられる粉砕装置としては、例え
ば、ジェットミル、衝突板式ミル、回転型機械ミル等が
挙げられる。
Examples of the crushing device used for crushing include a jet mill, a collision plate type mill, and a rotary mechanical mill.

【0033】分級に用いられる分級装置としては、例え
ば、風力分級機、慣性式分級機、篩式分級機等が挙げら
れる。
Examples of the classifying device used for classification include an air classifier, an inertial classifier and a sieve classifier.

【0034】かくして得られたトナーは、着色剤の分散
性、さらには電荷制御剤、ワックス等の分散性に優れた
ものである。
The toner thus obtained is excellent in dispersibility of the colorant, and further dispersibility of the charge control agent, wax and the like.

【0035】かかるトナーを電子写真法、静電印刷法及
び磁気記録法等の印刷方法に使用すると、トナーに印刷
機内の感光体へのフィルミングもなく、印刷後も画像が
安定しているという優れた効果が発現される。
When such a toner is used in a printing method such as an electrophotographic method, an electrostatic printing method and a magnetic recording method, the toner is not filmed on the photosensitive member in the printing machine and the image is stable after printing. An excellent effect is exhibited.

【0036】[0036]

【実施例】 混練物の調製 ・ポリエステル樹脂〔ガラス転移点(Tg)=60℃、溶融温度Tm=110 ℃(酸成分:テレフタル酸40重量部、フマール酸60重量部;アルコール成分 :ポリオキシエチレン(2.0)−2,2−ビス(4−ヒドロキシフェニル)プ ロパン100重量部)〕 70重量部 ・銅フタロシアニン顔料(C.I.ピグメント・ブルー (C. I. Pigment Blue ) 15:3) 30重量部 前記組成の原料を加熱ロールミルを用いて100℃で溶
融混合して混練物を調製した。なお、ガラス転移点と
は、示差走査熱量計(セイコー電子工業(株)製、商品
名:DSC210)を用い、200℃まで昇温し、その
温度にて3分間放置した後、降温速度10℃/分で室温
まで冷却したサンプルを、昇温速度10℃/分で昇温し
て熱履歴を測定した際の、ガラス転移温度以下のベース
ラインの延長線と、ピークの立ち上がり部分からピーク
の頂点までの間での最大傾斜を示す接線との交点の温度
をいう。
Example Preparation of Kneaded Material Polyester resin [glass transition point (Tg) = 60 ° C., melting temperature Tm = 110 ° C. (acid component: terephthalic acid 40 parts by weight, fumaric acid 60 parts by weight; alcohol component: polyoxyethylene (2.0) -2,2-bis (4-hydroxyphenyl) propane 100 parts by weight)] 70 parts by weight Copper phthalocyanine pigment (CI Pigment Blue 15: 3) 30 parts by weight A raw material having the above composition was melt-mixed at 100 ° C. using a heating roll mill to prepare a kneaded product. The glass transition point is a differential scanning calorimeter (manufactured by Seiko Denshi Kogyo Co., Ltd., trade name: DSC210), the temperature is raised to 200 ° C., the temperature is left at that temperature for 3 minutes, and then the temperature decreasing rate is 10 ° C. When a sample cooled to room temperature at a heating rate of 10 ° C./min was heated at a heating rate of 10 ° C./min and the thermal history was measured, an extension line of the baseline below the glass transition temperature and a peak portion from the rising portion of the peak The temperature at the intersection with the tangent line showing the maximum slope up to.

【0037】 処方 混練物 17重量部 ポリエステル樹脂(混練物の調製に用いたものと同じ) 88重量部 荷電制御剤 ベンジル酸ホウ素錯体(商品名:LR-147、日本カーリット(株)製) 1.5重量部 サリチル酸クロム錯体(商品名:E-84、オリエント化学工業(株)製) 1.5重量部[0037] Prescription   Kneaded material 17 parts by weight   Polyester resin (same as that used to prepare the kneaded product) 88 parts by weight   Charge control agent     Benzyl borate complex (trade name: LR-147, manufactured by Nippon Carlit Co., Ltd.)                                                           1.5 parts by weight     Chromium salicylate complex (trade name: E-84, manufactured by Orient Chemical Industry Co., Ltd.)                                                           1.5 parts by weight

【0038】実施例1 前記処方の原料1.5kgを、テーブルフィーダーを
用いてオープンロール型連続混練機(三井鉱山(株)
製、商品名:ニーデックス)に連続的に供給した。その
際の各原料の供給位置とその供給量を表1に示す。な
お、各原料の供給位置が同じ場合には、各原料を混合装
置であるヘンシェルミキサー(有効容量10L)に投入
し、羽根回転数を2500回転/分にて1分間混合を行
って、得られた混合物を用いた。
Example 1 An open-roll type continuous kneader (Mitsui Mining Co., Ltd.) was used to mix 1.5 kg of the above raw material with a table feeder.
Manufactured, trade name: Kneedex). Table 1 shows the supply position and supply amount of each raw material at that time. When the feed positions of the raw materials are the same, the raw materials were put into a Henschel mixer (effective volume: 10 L), which is a mixing device, and mixed at a blade rotation speed of 2500 rpm for 1 minute to obtain a product. Different mixtures were used.

【0039】この際に使用したオープンロール型連続混
練機はロール外径0.14〔m〕、有効ロール長0.6
〔m〕のものであり、運転条件は、高回転側ロール(前
ロール)回転数75回転/分、低回転側ロール(後ロー
ル)回転数50回転/分、ロール間隙0.1mm、ロー
ル内の加熱及び冷却媒体温度は、高回転ロールの原料投
入側が100℃及び混練物排出側が100℃であり、低
回転ロールの原料投入側が30℃及び混練物排出側が3
0℃、原材料混合物の供給速度は10kg/時、平均滞
留時間は約2分間であった。
The open roll type continuous kneader used at this time had a roll outer diameter of 0.14 [m] and an effective roll length of 0.6.
[M], and operating conditions are: high rotation side roll (front roll) rotation speed 75 rotations / minute, low rotation side roll (rear roll) rotation speed 50 rotations / minute, roll gap 0.1 mm, inside roll The heating and cooling medium temperatures are 100 ° C. on the raw material charging side of the high rotation roll and 100 ° C. on the kneading material discharging side of the high rotation roll, and 30 ° C. on the raw material charging side of the low rotation roller and 3 ° C.
At 0 ° C., the feed rate of the raw material mixture was 10 kg / hour and the average residence time was about 2 minutes.

【0040】得られたトナー混練物を冷却ベルトにて冷
却後、φ2〔mm〕のスクリーンを有するミルにて粗砕
した。次に、この粗砕物を衝突板型ジェットミルにて粉
砕し、更に、サイクロン型風力分級機にて粗粉及び微粉
をカットし、重量平均粒径が9μmのシアントナーとし
た。なお、トナーの重量平均粒径は、コールターカウン
ターにて測定した。更に得られたトナー100重量部に
対して、疎水性シリカ(「アエロジルR−972」、日
本アエロジル(株)製)1.0重量部を外添して、現像
剤とした。得られた現像剤を透過型電子顕微鏡(250
0倍)にて荷電制御剤粒径について観察をしたところ、
平均粒径0.3μmに分散していた。更に、直径15m
mの現像ロールを有する市販の非磁性一成分方式のフル
カラー電子写真記録装置を用いて、10,000枚の耐
刷試験を行ったところ、安定した画像を得ることができ
た。
The obtained toner kneaded product was cooled with a cooling belt and then roughly crushed with a mill having a screen of φ2 [mm]. Next, this coarsely pulverized product was pulverized by a collision plate type jet mill, and further, coarse powder and fine powder were cut by a cyclone type air classifier to obtain a cyan toner having a weight average particle diameter of 9 μm. The weight average particle diameter of the toner was measured with a Coulter counter. Further, to 100 parts by weight of the obtained toner, 1.0 part by weight of hydrophobic silica (“Aerosil R-972”, manufactured by Nippon Aerosil Co., Ltd.) was externally added to obtain a developer. The obtained developer was used as a transmission electron microscope (250
Observation of the particle size of the charge control agent at 0 times)
The particles had an average particle size of 0.3 μm. Furthermore, diameter 15m
Using a commercially available non-magnetic one-component type full-color electrophotographic recording apparatus having a m developing roller, a printing durability test of 10,000 sheets was performed, and a stable image could be obtained.

【0041】実施例2 処方を用いて、各原料の供給位置と供給量を表1に示
すようにした以外は、実施例1と同条件で溶融混練等の
製造を行い、現像剤(重量平均粒径9μm)を得た。得
られた現像剤を透過型電子顕微鏡(2500倍)にて荷
電制御剤粒径について観察をしたところ、平均粒径0.
5μmに分散していた。さらに10,000枚の耐刷試
験においても安定した画像を得ることができた。
Example 2 Using the formulation, melt kneading and the like were carried out under the same conditions as in Example 1 except that the feed position and feed amount of each raw material were as shown in Table 1. A particle size of 9 μm) was obtained. The developer thus obtained was observed with a transmission electron microscope (2500 times) for the particle size of the charge control agent.
It was dispersed in 5 μm. Further, stable images could be obtained even in the printing durability test of 10,000 sheets.

【0042】実施例3 処方を用いて、各原料の供給位置と供給量を表1に示
すようにした以外は、実施例1と同条件で溶融混練等の
製造を行い、現像剤(重量平均粒径9μm)を得た。得
られた現像剤を透過型電子顕微鏡(2500倍)にて荷
電制御剤粒径について観察をしたところ、平均粒径1μ
mに分散していた。さらに10,000枚の耐刷試験に
おいても安定した画像を得ることができた。
Example 3 Using the formulation, melt kneading and the like were carried out under the same conditions as in Example 1 except that the feed position and feed amount of each raw material were as shown in Table 1. A particle size of 9 μm) was obtained. The obtained developer was observed with a transmission electron microscope (2500 times) for the particle size of the charge control agent, and the average particle size was 1 μm.
It was dispersed in m. Further, stable images could be obtained even in the printing durability test of 10,000 sheets.

【0043】実施例4 処方を用いて、各原料の供給位置と供給量を表1に示
すようにした以外は、実施例1と同条件で溶融混練等の
製造を行い、現像剤(重量平均粒径9μm)を得た。得
られた現像剤を透過型電子顕微鏡(2500倍)にて荷
電制御剤粒径について観察をしたところ、平均粒径0.
5μmに分散していた。さらに10,000枚の耐刷試
験においても安定した画像を得ることができた。
Example 4 A melt kneading process was carried out under the same conditions as in Example 1 except that the prescription was used and the feed positions and feed rates of the respective raw materials were as shown in Table 1. A particle size of 9 μm) was obtained. The developer thus obtained was observed with a transmission electron microscope (2500 times) for the particle size of the charge control agent.
It was dispersed in 5 μm. Further, stable images could be obtained even in the printing durability test of 10,000 sheets.

【0044】比較例1 処方を用いて、各原料の供給位置と供給量を表1に示
すようにした以外は、実施例1と同条件で溶融混練等の
製造を行い、現像剤(重量平均粒径9μm)を得た。得
られた現像剤を透過型電子顕微鏡(2500倍)にて荷
電制御剤粒径について観察をしたところ、平均粒径3.
5μmに分散し、10,000枚の耐刷試験において、
荷電制御剤の分散不良により、かぶり、転写率の低下及
び現像むらが生じ、安定した画像を得ることができなか
った。
Comparative Example 1 A developer (weight average) was prepared under the same conditions as in Example 1 except that the prescription was used and the feed position and feed amount of each raw material were as shown in Table 1. A particle size of 9 μm) was obtained. The obtained developer was observed with a transmission electron microscope (2500 times) for the particle size of the charge control agent, and the average particle size was 3.
Dispersed in 5 μm, in a printing durability test of 10,000 sheets,
Due to poor dispersion of the charge control agent, fogging, lowering of transfer rate and uneven development occurred, and stable images could not be obtained.

【0045】 処方 混練物 17重量部 ポリエステル樹脂(混練物の調製に用いたものと同じ) 88重量部 荷電制御剤 ベンジル酸ホウ素錯体 1.5重量部 サリチル酸クロム錯体 1.5重量部 カルナバワックス 10重量部[0045] Prescription   Kneaded material 17 parts by weight   Polyester resin (same as that used to prepare the kneaded product) 88 parts by weight   Charge control agent     Benzyl borate complex 1.5 parts by weight     Chromium salicylate complex 1.5 parts by weight   Carnauba wax 10 parts by weight

【0046】実施例5 処方を用いて、各原料の供給位置と供給量を表1に示
すようにした以外は、実施例1と同条件で溶融混練等の
製造を行い、現像剤(重量平均粒径9μm)を得た。得
られた現像剤を透過型電子顕微鏡(2500倍)にて荷
電制御剤粒径について観察をしたところ、平均粒径0.
5μmに分散していた。さらに10,000枚の耐刷試
験においても安定した画像を得ることができ、感光体へ
のフィルミングも無く良好であった。
Example 5 Using the prescription, melt kneading and the like were carried out under the same conditions as in Example 1 except that the feed position and feed amount of each raw material were as shown in Table 1. A particle size of 9 μm) was obtained. The developer thus obtained was observed with a transmission electron microscope (2500 times) for the particle size of the charge control agent.
It was dispersed in 5 μm. Further, a stable image could be obtained even in a printing durability test of 10,000 sheets, and there was no filming on the photoreceptor, which was good.

【0047】比較例2 処方を用いて、各原料の供給位置と供給量を表1に示
すようにした以外は、実施例1と同条件で溶融混練等の
製造を行い、現像剤(重量平均粒径9μm)を得た。得
られた現像剤を透過型電子顕微鏡(2500倍)にて荷
電制御剤粒径について観察をしたところ、平均粒径3.
5μmに分散し、10,000枚の耐刷試験において、
荷電制御剤の分散不良により、かぶり、転写率の低下及
び現像むらが生じ、安定した画像を得ることができなか
った。
COMPARATIVE EXAMPLE 2 Melt-kneading and the like were carried out under the same conditions as in Example 1 except that the feed position and feed amount of each raw material were set as shown in Table 1 by using the formulation, and the developer (weight average) was used. A particle size of 9 μm) was obtained. The obtained developer was observed with a transmission electron microscope (2500 times) for the particle size of the charge control agent, and the average particle size was 3.
Dispersed in 5 μm, in a printing durability test of 10,000 sheets,
Due to poor dispersion of the charge control agent, fogging, lowering of transfer rate and uneven development occurred, and stable images could not be obtained.

【0048】[0048]

【表1】 [Table 1]

【0049】[0049]

【発明の効果】本発明を用いて、得られたトナーは、着
色剤の分散に優れ、また荷電制御剤、ワックスの分散度
が適度に制御されたものであり、特に電子写真法、静電
印刷法及び磁気記録法等において良好に用いられる。
The toner obtained by using the present invention is excellent in the dispersion of the colorant, and the dispersion degree of the charge control agent and the wax is appropriately controlled. It is preferably used in printing methods and magnetic recording methods.

───────────────────────────────────────────────────── フロントページの続き (56)参考文献 特開 平11−133660(JP,A) 特開 平3−149567(JP,A) 特開 平9−319145(JP,A) 特開 平5−249738(JP,A) 特開 平10−171159(JP,A) 特開 平6−308766(JP,A) (58)調査した分野(Int.Cl.7,DB名) G03G 9/08 ─────────────────────────────────────────────────── ─── Continuation of the front page (56) References JP-A-11-133660 (JP, A) JP-A-3-149567 (JP, A) JP-A-9-319145 (JP, A) JP-A-5- 249738 (JP, A) JP 10-171159 (JP, A) JP 6-308766 (JP, A) (58) Fields investigated (Int.Cl. 7 , DB name) G03G 9/08

Claims (2)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】 予め着色剤を結着樹脂に溶融混合した混
練物と結着樹脂と荷電制御剤とを含有する組成物を加熱
及び冷却機能を有するオープンロール型連続混練機を用
いて溶融混練する工程を有するトナーの製造方法であっ
て、前記溶融混練に際して、該混練機のロールの軸方向
に沿って複数の位置に供給口を設け、前記混練物と結着
樹脂と荷電制御剤とを該混練機の入り口側のロール端部
0L(但し、Lはロール長さを示す)〜0.9Lの位置
から連続的に供給して溶融混練を行う、トナーの製造方
法。
1. A kneaded product obtained by previously melt-mixing a colorant with a binder resin and a composition containing a binder resin and a charge control agent are melt-kneaded using an open roll type continuous kneader having a heating and cooling function. In the method for producing a toner having a step of, in the melt kneading, supply ports are provided at a plurality of positions along the axial direction of the roll of the kneading machine, and the kneaded product, the binder resin and the charge control agent are provided. A method for producing a toner, which comprises continuously feeding and kneading from a roll end portion 0L (where L represents roll length) to 0.9L on the inlet side of the kneading machine.
【請求項2】 1個所以上の供給口からワックスをさら
に供給する請求項1記載の製造方法。
2. The manufacturing method according to claim 1, wherein the wax is further supplied from one or more supply ports.
JP24624499A 1999-08-31 1999-08-31 Toner production method Expired - Lifetime JP3432774B2 (en)