JP2002304717A - Magnetic recording medium and method for manufacturing the same - Google Patents
Magnetic recording medium and method for manufacturing the sameInfo
- Publication number
- JP2002304717A JP2002304717A JP2001106017A JP2001106017A JP2002304717A JP 2002304717 A JP2002304717 A JP 2002304717A JP 2001106017 A JP2001106017 A JP 2001106017A JP 2001106017 A JP2001106017 A JP 2001106017A JP 2002304717 A JP2002304717 A JP 2002304717A
- Authority
- JP
- Japan
- Prior art keywords
- abrasive particles
- magnetic
- magnetic layer
- recording medium
- magnetic recording
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【0001】[0001]
【発明が属する技術分野】本発明は、磁気記録媒体及び
その製造方法に関するものである。The present invention relates to a magnetic recording medium and a method for manufacturing the same.
【0002】[0002]
【従来の技術】蒸着型の磁気記録媒体を使用することを
前提とした、デジタル記録システムの開発が進む中、互
換性のある高出力特性及び高C/N(キャリア/ノイズ
比)特性を持った塗布型の磁気記録媒体の開発が、その
生産性や生産コストという点から重要なテーマとなって
いる。2. Description of the Related Art As digital recording systems have been developed on the premise that a magnetic recording medium of a vapor deposition type is used, compatible high output characteristics and high C / N (carrier / noise ratio) characteristics are obtained. The development of coated magnetic recording media has become an important theme in terms of productivity and production cost.
【0003】こうした塗布型の磁気記録媒体において、
蒸着型の磁気記録媒体と同等の高出力特性及び高C/N
特性を実現するためには、媒体の表面を平滑にすること
はもとより、磁性層中における磁性粉の充填率を高める
ことが非常に重要となってくる。In such a coating type magnetic recording medium,
High output characteristics and high C / N equivalent to evaporation type magnetic recording media
In order to realize the characteristics, it is very important not only to smooth the surface of the medium but also to increase the filling ratio of the magnetic powder in the magnetic layer.
【0004】また、従来の塗布型磁気記録媒体媒体は、
通常、自己クリーニング効果を持たせることを目的とし
て、磁性塗膜中に研磨剤粒子を含有しており、これを添
加しない場合、走行信頼性を確保することができなかっ
た。Further, a conventional coating type magnetic recording medium is
Usually, for the purpose of giving a self-cleaning effect, abrasive particles are contained in the magnetic coating film, and when this is not added, running reliability cannot be ensured.
【0005】[0005]
【発明が解決しようとする課題】しかしながら、従来の
ように、磁性塗膜中に研磨剤粒子を含有する場合、研磨
剤粒子を所定の個数だけ磁性層の表面上に存在させるた
めに、磁性紛に対して相当量の研磨剤粒子を添加しなく
てはならない。これにより、磁性層中の単位体積当たり
の磁性粉の充填率が低下してしまい、高出力特性及び高
C/N特性を得ることが困難であった。However, when abrasive particles are contained in a magnetic coating film as in the prior art, a predetermined number of abrasive particles are present on the surface of the magnetic layer. A considerable amount of abrasive particles must be added to the mixture. As a result, the packing ratio of the magnetic powder per unit volume in the magnetic layer is reduced, and it has been difficult to obtain high output characteristics and high C / N characteristics.
【0006】本発明は、上述したような問題点を解決す
るためになされたものであって、その目的は、出力特性
等の電磁変換特性に優れ、かつ走行信頼性を有する、磁
気記録媒体及びその製造方法を提供することにある。The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a magnetic recording medium having excellent electromagnetic conversion characteristics such as output characteristics and running reliability. It is to provide a manufacturing method thereof.
【0007】[0007]
【課題を解決するための手段】即ち、本発明は、磁性層
を有し、研磨剤粒子が前記磁性層の表面域にのみ分布し
ている、磁気記録媒体に係るものである。That is, the present invention relates to a magnetic recording medium having a magnetic layer, wherein abrasive particles are distributed only in the surface area of the magnetic layer.
【0008】また、磁性層上に、研磨剤粒子を含有する
塗料を塗布し、前記研磨剤粒子を前記磁性層の表面域に
のみ分布させる、磁気記録媒体の製造方法に係るもので
ある。Further, the present invention relates to a method for manufacturing a magnetic recording medium, wherein a coating material containing abrasive particles is applied on a magnetic layer, and the abrasive particles are distributed only in a surface area of the magnetic layer.
【0009】本発明によれば、前記磁性層の表面上に、
前記研磨剤粒子を含有する前記塗料を塗布して、前記研
磨剤粒子を前記磁性層の表面域にのみ分布させるので、
従来のように、前記磁性層の表面上に、前記研磨剤粒子
を所定の個数分存在させるために、前記磁性層中に、前
記磁性紛の相当量の前記研磨剤粒子を添加していたのに
比べて、前記研磨剤粒子を、前記磁性層の表面域での必
要最小限の存在量分だけ塗布すればよく、しかも均一な
高さで存在させることが可能となり、効率良く磁気記録
媒体を製造することができ、かつ得られる磁気記録媒体
は走行信頼性にも優れている。According to the present invention, on the surface of the magnetic layer,
Since the coating containing the abrasive particles is applied to distribute the abrasive particles only in the surface area of the magnetic layer,
As in the prior art, a considerable amount of the abrasive particles of the magnetic powder was added to the magnetic layer in order to cause a predetermined number of the abrasive particles to exist on the surface of the magnetic layer. As compared with the above, the abrasive particles may be applied only in a necessary minimum amount in the surface area of the magnetic layer, and can be present at a uniform height. The magnetic recording medium that can be manufactured and obtained has excellent running reliability.
【0010】また、前記研磨剤粒子が前記磁性層の表面
域にのみ分布しているので、前記磁性層を形成する磁性
塗料には前記研磨剤粒子を一切添加しないですみ、前記
磁性層は、非常に磁性紛の充填率が高い状態を維持する
ことが可能となる。例えば、磁性紛の配向過程において
も、配向を阻害するような粒子が存在しないため効率を
向上することができ、高い出力特性等の電磁変換特性を
得ることができる。[0010] Further, since the abrasive particles are distributed only in the surface area of the magnetic layer, the abrasive particles need not be added to the magnetic paint forming the magnetic layer at all. It is possible to maintain a state where the filling rate of the magnetic powder is very high. For example, in the process of aligning the magnetic powder, the efficiency can be improved because there are no particles that hinder the alignment, and electromagnetic conversion characteristics such as high output characteristics can be obtained.
【0011】[0011]
【発明の実施の形態】以下、本発明を実施の形態に基づ
いて更に詳しく説明する。DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the present invention will be described in more detail based on embodiments.
【0012】前記研磨剤粒子は結合剤で被覆されている
ことが好ましく、また、前記研磨剤粒子が、前記磁性層
の表面上に付着されているか、或いは、前記研磨剤粒子
の少なくとも一部分が前記磁性層の表面域に埋設されて
いることが好ましい。これにより、前記研磨剤粒子と前
記磁性層の接着性が向上し、より走行信頼性を向上する
ことができる。Preferably, the abrasive particles are coated with a binder, and the abrasive particles are adhered on the surface of the magnetic layer, or at least a part of the abrasive particles are It is preferably embedded in the surface area of the magnetic layer. Thereby, the adhesion between the abrasive particles and the magnetic layer is improved, and the running reliability can be further improved.
【0013】また、前記磁性層の表面域に存在する前記
研磨剤粒子の個数が、1〜100個/1μm2であるこ
とが好ましく、1個/1μm2より少ないと、通常言わ
れているような前記研磨剤粒子の量不足と同様のことが
起こり、走行信頼性が低下することがある。また、10
0個/1μm2より多くなると、前記研磨剤粒子の数が
多くなりすぎ、電磁変換特性が悪化することがある。The number of the abrasive particles present in the surface area of the magnetic layer is preferably 1 to 100/1 μm 2 , and it is generally said that the number is less than 1/1 μm 2 . The same thing as the insufficient amount of the abrasive particles may occur, and the running reliability may decrease. Also, 10
If it exceeds 0 particles / 1 μm 2, the number of the abrasive particles becomes too large, and the electromagnetic conversion characteristics may be deteriorated.
【0014】前記研磨剤粒子としての非磁性無機粉末
は、従来から公知のものがいずれも使用可能であって、
例示するならば、アルミナ(モース硬度9)、酸化クロ
ム(同9)、炭化珪素(同9)、酸化チタン、酸化珪素
(同7)、炭酸カルシウム(同3)、α−酸化鉄(同
6)、カオリン(同1〜2.5)、黒鉛(同0.5〜
1)、雲母(2.8)、炭化チタン、リン酸カルシウム
(同5)、アモルファスシリカ(同7)などが挙げられ
る。これらの中でも、モース硬度が3以上のものを用い
ることがより好ましく、さらに5以上とすることで、数
種類の金属材料からなる磁気ヘッドを均一に研磨するこ
とができ、より高い走行信頼性を得ることができる。ま
た、上記した非磁性無機粉末のうちの一種を単独で用い
ることもでき、或いは二種以上を適宜組み合わせて用い
てもよい。As the non-magnetic inorganic powder as the abrasive particles, any conventionally known non-magnetic inorganic powder can be used.
For example, alumina (Mohs hardness 9), chromium oxide (9), silicon carbide (9), titanium oxide, silicon oxide (7), calcium carbonate (3), α-iron oxide (6) ), Kaolin (1-2.5), graphite (0.5-)
1), mica (2.8), titanium carbide, calcium phosphate (5), amorphous silica (7) and the like. Among these, it is more preferable to use one having a Mohs' hardness of 3 or more, and by setting it to 5 or more, a magnetic head made of several kinds of metal materials can be uniformly polished, and higher running reliability is obtained. be able to. In addition, one of the above nonmagnetic inorganic powders may be used alone, or two or more of them may be used in an appropriate combination.
【0015】前記研磨剤粒子の形状は、球状、針状又は
板状などを用いることができ、特に限定されない。な
お、前記研磨剤粒子を含有する前記塗料を塗布した際の
平滑性を考慮して、前記研磨剤粒子の粒子サイズは、針
状であるならば長軸長が0.35μm以下、球状である
ならば粒径が0.35μm以下、板状であれば板の径が
0.35μm以下であることが好ましく、また、下限値
を0.02μmとすることが好ましい。前記粒子サイズ
が0.02μm未満の場合、前記研磨剤粒子の分散性が
低下することがあり、0.35μmを超えた場合、本発
明に基づく磁気記録媒体と前記ヘッドの空間が大きくな
りすぎるために、あまり高い出力特性を得ることができ
ないことがある。The shape of the abrasive particles can be spherical, needle-like or plate-like, and is not particularly limited. In addition, in consideration of the smoothness when the paint containing the abrasive particles is applied, the particle size of the abrasive particles is a spherical shape having a major axis length of 0.35 μm or less if it is acicular. If so, the particle size is preferably 0.35 μm or less, and if it is plate-like, the diameter of the plate is preferably 0.35 μm or less, and the lower limit is preferably 0.02 μm. When the particle size is less than 0.02 μm, the dispersibility of the abrasive particles may decrease. When the particle size exceeds 0.35 μm, the space between the magnetic recording medium according to the present invention and the head becomes too large. In some cases, very high output characteristics cannot be obtained.
【0016】非磁性支持体上に、磁性紛と結合剤を主体
とする前記磁性層を塗布し、前記磁性層が乾燥状態若し
くは湿潤状態のうちに、前記研磨剤粒子及び結合剤を含
有する前記塗料を塗布し、その後、前記塗料を乾燥する
ことで、本発明に基づく磁気記録媒体を製造することが
できる。前記磁性層が乾燥状態のときに、前記研磨剤粒
子を含有する前記塗料を塗布した場合、前記研磨剤粒子
が、前記磁性層の表面上に付着されている磁気記録媒体
を得ることができ、前記磁性層が湿潤状態のときに、前
記塗料を塗布した場合、前記研磨剤粒子の少なくとも一
部分が前記磁性層の表面域に埋設されている磁気記録媒
体を得ることができる。The magnetic layer mainly composed of a magnetic powder and a binder is coated on a non-magnetic support, and the magnetic layer contains the abrasive particles and the binder while the magnetic layer is in a dry state or a wet state. By applying a paint and then drying the paint, a magnetic recording medium according to the present invention can be manufactured. When the magnetic layer is in a dry state, when the paint containing the abrasive particles is applied, the abrasive particles can obtain a magnetic recording medium adhered on the surface of the magnetic layer, When the coating material is applied while the magnetic layer is in a wet state, it is possible to obtain a magnetic recording medium in which at least a part of the abrasive particles is embedded in a surface area of the magnetic layer.
【0017】前記研磨剤粒子を含有する前記塗料には、
前記結合剤で被覆されている前記研磨剤粒子の他に、分
散剤、防錆剤等を適宜添加することができ、これらの材
質は、後述する磁性塗料に含有することができる各組成
と同様のものを用いることができる。The paint containing the abrasive particles includes:
In addition to the abrasive particles coated with the binder, a dispersant, a rust inhibitor and the like can be appropriately added, and these materials are the same as the respective compositions that can be contained in the magnetic paint described below. Can be used.
【0018】前記磁性層上に、前記研磨剤粒子を含有す
る前記塗料を塗布するには、前記塗料の上記したような
各構成成分を前記結合剤中に分散し、前記結合剤の種類
等によってエーテル類、エステル類、ケトン類、芳香族
炭化水素、脂肪族炭化水素、有機塩素化合物系溶剤等か
ら選ばれる有機溶剤と共に分散して、前記塗料を調製す
ることができる。そして、前記塗料を調製するに際して
は、ロールミル、ボールミル、サンドミル、ニーダー、
エクストルーダー、ホモゲナイザー、超音波分散機等に
よって、配合成分の分散、混練を行えばよい。このよう
にして得られた前記塗料を前記磁性層上に塗付する際に
は、グラビアコーター、ナイフコーター、ブレードコー
ター、リバースロールコーター、ダイコーター等を用い
ればよい。In order to apply the coating material containing the abrasive particles on the magnetic layer, the above-described constituent components of the coating material are dispersed in the binder, and depending on the type of the binder, etc. The coating material can be prepared by dispersing together with an organic solvent selected from ethers, esters, ketones, aromatic hydrocarbons, aliphatic hydrocarbons, and organic chlorine compound solvents. And when preparing the paint, a roll mill, a ball mill, a sand mill, a kneader,
The components may be dispersed and kneaded using an extruder, a homogenizer, an ultrasonic disperser or the like. When applying the coating material thus obtained on the magnetic layer, a gravure coater, knife coater, blade coater, reverse roll coater, die coater, or the like may be used.
【0019】本発明に基づく磁気記録媒体の製造方法
は、前記磁性層の表面上に、前記研磨剤粒子を含有する
前記塗料を塗布して、前記研磨剤粒子を前記磁性層の表
面域にのみ分布させるので、前記研磨剤粒子を、前記磁
性層の表面域での必要最小限の存在量分だけ塗布すれば
よく、しかも均一な高さで存在させることが可能とな
り、一層効率良く磁気記録媒体を製造することができ、
かつ得られる本発明に基づく磁気記録媒体は、走行信頼
性にもより一層優れている。In the method for manufacturing a magnetic recording medium according to the present invention, the paint containing the abrasive particles is applied on the surface of the magnetic layer, and the abrasive particles are applied only to the surface area of the magnetic layer. Since the abrasive particles are distributed, the abrasive particles only need to be applied in a necessary minimum amount in the surface area of the magnetic layer, and can be present at a uniform height. Can be manufactured,
The obtained magnetic recording medium according to the present invention is further excellent in running reliability.
【0020】また、前記研磨剤粒子が前記磁性層の表面
域にのみ分布しているので、前記磁性層を形成する磁性
塗料には前記研磨剤粒子を一切添加しないですみ、前記
磁性層は、非常に磁性紛の充填率が高い状態を維持する
ことが可能となり、より一層高い電磁変換特性を得るこ
とができる。Further, since the abrasive particles are distributed only in the surface area of the magnetic layer, the abrasive particles need not be added to the magnetic paint forming the magnetic layer at all. It is possible to maintain a state where the filling ratio of the magnetic powder is extremely high, and it is possible to obtain much higher electromagnetic conversion characteristics.
【0021】本発明において、前記磁性塗料を構成する
強磁性粉末は、従来公知のものがいずれも使用可能であ
って、酸化磁性粉末又は金属磁性粉末でもよい。前記酸
化物磁性粉末としては、例えば、γ−Fe2O3、Co含
有γ−Fe2O3、Fe3O4、Co含有Fe3O4、Co被
着γ−Fe2O3、Co被着Fe3O4、CrO2等が挙げ
られる。前記金属磁性粉末としては、例えば、Fe、C
o、Ni、Fe−Co、Fe−Ni、Fe−Co−N
i、Co−Ni、Fe−Co−B、Fe−Co−Cr−
B、Mn−Bi、Mn−Al、Fe−Co−V等が挙げ
られる。また、これらの種々の特性を改善する目的でA
l、Si、Ti、Cr、Mn、Cu、Zn等の金属成分
やYを含む希土類元素を適当量含有してもよい。さら
に、Fe5C2等の炭化鉄、窒化鉄等も使用可能である。
強磁性紛としては、上述した材料のうち、一種類を選択
してもよいし、二種類以上を併用することもできる。In the present invention, as the ferromagnetic powder constituting the magnetic paint, any conventionally known ferromagnetic powder can be used, and it may be an oxide magnetic powder or a metal magnetic powder. Examples of the oxide magnetic powder include γ-Fe 2 O 3 , Co-containing γ-Fe 2 O 3 , Fe 3 O 4 , Co-containing Fe 3 O 4 , Co-coated γ-Fe 2 O 3 , and Co-coated Fe 3 O 4 , CrO 2 and the like. Examples of the metal magnetic powder include Fe and C.
o, Ni, Fe-Co, Fe-Ni, Fe-Co-N
i, Co-Ni, Fe-Co-B, Fe-Co-Cr-
B, Mn-Bi, Mn-Al, Fe-Co-V and the like. Further, in order to improve these various characteristics, A
l, Si, Ti, Cr, Mn, Cu, Zn and other metal components and rare earth elements containing Y may be contained in appropriate amounts. Further, iron carbide such as Fe 5 C 2 , iron nitride and the like can also be used.
As the ferromagnetic powder, one of the above-mentioned materials may be selected, or two or more thereof may be used in combination.
【0022】本発明に基づく磁気記録媒体に使用可能な
結合剤(これは、前記磁性塗料の他に、前記研磨剤粒子
を含有する前記塗料の構成成分のうちの前記結合剤とし
ても使用可能である。)としては、通常この種の媒体に
おいて用いられている樹脂材料がいずれも使用可能であ
って、特にその種類は限定されない。代表的な前記結合
剤樹脂を例示すれば、塩化ビニル−酢酸ビニル共重合
体、塩化ビニル−酢酸ビニル−ビニルアルコール共重合
体、塩化ビニル−酢酸ビニル−マレイン酸共重合体、塩
化ビニル−塩化ビニリデン共重合体、塩化ビニル−アク
リロニトリル共重合体、アクリル酸エステル−塩化ビニ
リデン共重合体、メタクリル酸エステル−塩化ビニリデ
ン共重合体、メタクリル酸エステル−スチレン共重合
体、熱可塑性ポリウレンタン樹脂、ポリフッ化ビニル、
塩化ビニリデン−アクリロニトリル共重合体、ブタジエ
ン−アクリロニトリル共重合体、アクリロニトリル−ブ
タジエン−メタクリル酸共重合体、ポリビニルブチラー
ル、ポリビニルアセタール、セルロース誘導体、スチレ
ン−ブタジエン共重合体、ポリエステル樹脂、フェノー
ル樹脂、フェノキシ樹脂、エポキシ樹脂、熱硬化性ポリ
ウレタン樹脂、尿素樹脂、メラミン樹脂、アリキド樹
脂、尿素−ホルムアルデヒド樹脂などである。こうした
結合剤は、少なくともその一部にスルホン酸塩(−SO
3M;MはNa、K等のアルカリ金属又はアルキル基を
表す)、硫酸塩(−SO4M;MはNa、K等のアルカ
リ金属又はアルキル基を表す)、カルボン酸基、アミノ
酸類基、アミノスルホン酸類基、ホスホン基、ホスフィ
ン基、アミノ基等のうちの少なくとも一つが導入されて
いることが望ましい。A binder usable for the magnetic recording medium according to the present invention (this can be used as the binder among the constituents of the paint containing the abrasive particles in addition to the magnetic paint. Can be used, any of the resin materials usually used in this type of medium can be used, and the type thereof is not particularly limited. Typical examples of the binder resin include vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinyl acetate-vinyl alcohol copolymer, vinyl chloride-vinyl acetate-maleic acid copolymer, vinyl chloride-vinylidene chloride. Copolymer, vinyl chloride-acrylonitrile copolymer, acrylate-vinylidene chloride copolymer, methacrylate-vinylidene chloride copolymer, methacrylate-styrene copolymer, thermoplastic urethane resin, polyvinyl fluoride,
Vinylidene chloride-acrylonitrile copolymer, butadiene-acrylonitrile copolymer, acrylonitrile-butadiene-methacrylic acid copolymer, polyvinyl butyral, polyvinyl acetal, cellulose derivative, styrene-butadiene copolymer, polyester resin, phenol resin, phenoxy resin, Epoxy resins, thermosetting polyurethane resins, urea resins, melamine resins, alkyd resins, urea-formaldehyde resins, and the like. Such binders include, at least in part, sulfonates (-SO
3 M; M represents an alkali metal or alkyl group such as Na or K), sulfate (—SO 4 M; M represents an alkali metal or alkyl group such as Na or K), carboxylic acid group, amino acid group , An aminosulfonic acid group, a phosphone group, a phosphine group, an amino group and the like are preferably introduced.
【0023】また、前記磁性塗料には、必要に応じてレ
シチン等の分散剤、カーボンブラック等の帯電防止剤が
加えられてもよい。これらの分散剤、帯電防止剤、及び
防錆剤としては、従来公知の材料がいずれも使用可能で
あり、なんら限定されるものではない。また、使用でき
る潤滑剤としては、脂肪酸及び脂肪酸エステルなどの従
来公知の材料がいずれも使用可能であり、特に限定され
るものではない。If necessary, a dispersant such as lecithin and an antistatic agent such as carbon black may be added to the magnetic paint. As the dispersant, antistatic agent, and rust inhibitor, any of conventionally known materials can be used, and there is no particular limitation. As the lubricant that can be used, any of conventionally known materials such as fatty acids and fatty acid esters can be used, and there is no particular limitation.
【0024】また、耐久性を向上させるために前記磁性
塗料へ硬化性樹脂を添加することも可能である。具体的
には、ポリイソシアネート化合物、ポリエポキシ化合物
に代表されるような熱硬化樹脂や電子線反応型硬化樹脂
などが挙げられる。これらは、単独若しくは2つ以上用
いて使用することができる。Further, a curable resin can be added to the magnetic paint in order to improve the durability. Specific examples include a thermosetting resin represented by a polyisocyanate compound and a polyepoxy compound, and an electron beam reactive curing resin. These can be used alone or in combination of two or more.
【0025】前記非磁性支持体上に前記磁性層を形成す
るには、前記磁性層の上記したような構成成分を前記結
合剤中に分散し、前記結合剤の種類等によってエーテル
類、エステル類、ケトン類、芳香族炭化水素、脂肪族炭
化水素、有機塩素化合物系溶剤等から選ばれる有機溶剤
と共に分散して、前記磁性塗料を調製することができ
る。そして、前記磁性塗料を調製するに際しては、ロー
ルミル、ボールミル、サンドミル、ニーダー、エクスト
ルーダー、ホモゲナイザー、超音波分散機等によって、
配合成分の分散、混練を行えばよい。このようにして得
られた磁性塗料を前記非磁性支持体上に塗付する際に
は、グラビアコーター、ナイフコーター、ブレードコー
ター、リバースロールコーター、ダイコーター等を用い
ればよい。In order to form the magnetic layer on the non-magnetic support, the above-described constituents of the magnetic layer are dispersed in the binder, and ethers and esters are used depending on the type of the binder. The magnetic coating material can be prepared by dispersing together with an organic solvent selected from ketones, aromatic hydrocarbons, aliphatic hydrocarbons, and organic chlorine compound solvents. Then, when preparing the magnetic paint, by a roll mill, a ball mill, a sand mill, a kneader, an extruder, a homogenizer, an ultrasonic disperser, and the like.
What is necessary is just to disperse and knead the compounding components. When the magnetic paint thus obtained is applied onto the non-magnetic support, a gravure coater, knife coater, blade coater, reverse roll coater, die coater or the like may be used.
【0026】また、前記非磁性支持体上の前記磁性層が
設けられていない面側(裏面)には、磁気記録媒体の走
行性の向上や帯電防止及び転写防止等を目的として、バ
ックコート層を設けることができる。前記バックコート
層の形成は、例えば無機顔料等の固体粒子を結合剤(基
本的には前記磁性層に使用できるものと同じ結合剤であ
ってよい。)中に分散させ、該結合剤の種類に応じて選
定された有機溶剤と共に混練して調製されたバックコー
ト層用塗料を調製し、これを非磁性支持体の裏面に塗布
する。On the surface of the non-magnetic support on which the magnetic layer is not provided (rear surface), a back coat layer is provided for the purpose of improving the running properties of the magnetic recording medium, preventing charging and preventing transfer, and the like. Can be provided. The back coat layer is formed by, for example, dispersing solid particles such as an inorganic pigment in a binder (which may be basically the same binder as that which can be used for the magnetic layer), and the type of the binder. Is prepared by kneading together with an organic solvent selected according to the above, and applying this to the back surface of the non-magnetic support.
【0027】前記固体粒子としては、帯電防止効果、潤
滑効果を賦与できるものであれば、従来公知の材料がい
ずれも使用可能であり、例えばグラファイト、カーボン
ブラック、酸化チタン等が挙げられる。これらの固体粒
子は、それぞれ一種を用いることができるが、二種以上
を併用してもよい。As the solid particles, any conventionally known materials can be used as long as they can impart an antistatic effect and a lubricating effect, and examples thereof include graphite, carbon black, and titanium oxide. These solid particles can be used alone or in combination of two or more.
【0028】なお、前記バックコート層を構成する材料
としては、前記固体粒子や前記結合剤のほかに、添加剤
としての分散剤、研磨剤、帯電防止剤などが加えられて
もよい。これらの添加剤としては、通常この種の磁気記
録媒体において用いられる材料であればよく、特に限定
されない。As a material constituting the back coat layer, in addition to the solid particles and the binder, a dispersant as an additive, an abrasive, an antistatic agent and the like may be added. These additives are not particularly limited as long as they are materials generally used in this type of magnetic recording medium.
【0029】前記非磁性支持体としては、ポリエチレン
テレフタレート、ポリエチレン−2,6−ナフタレート
フィルム等のポリエステル類、ポリオレフィン類、セル
ロース類、ビニル系樹脂、ポリイミド類、ポリアミド
類、ポリカーボネートなどに代表される高分子支持体
や、アルミニウム合金、チタン合金などからなる金属基
板、ガラス基板、アラミドフィルム等などがある。その
形状もなんら限定されるものではなく、テープ状、シー
ト状、ドラム状など、如何なる形態であってもよい。さ
らに、この非磁性支持体には、その表面性をコントロー
ルするために、微細な凹凸が形成されるような表面処理
が施されたものであってもよい。Examples of the nonmagnetic support include polyesters such as polyethylene terephthalate and polyethylene-2,6-naphthalate films, polyolefins, celluloses, vinyl resins, polyimides, polyamides and polycarbonates. Examples include a polymer support, a metal substrate made of an aluminum alloy, a titanium alloy, or the like, a glass substrate, an aramid film, and the like. The shape is not limited at all, and may be any shape such as a tape shape, a sheet shape, and a drum shape. Further, in order to control the surface properties, the non-magnetic support may be subjected to a surface treatment for forming fine irregularities.
【0030】なお、本発明に基づく磁気記録媒体は、前
記磁性層が単層であるものに限らず、複数の磁性層が積
層されたものであってもよい。さらに、前記磁性層と前
記非磁性支持体との間に、非磁性層が形成されていても
よく、また、接着性を向上させる目的で、接着層が形成
された構成としてもよい。It should be noted that the magnetic recording medium according to the present invention is not limited to the magnetic layer having a single layer, but may have a structure in which a plurality of magnetic layers are laminated. Further, a non-magnetic layer may be formed between the magnetic layer and the non-magnetic support, and an adhesive layer may be formed for the purpose of improving adhesiveness.
【0031】図1は、前記磁性層が湿潤状態のときに、
前記研磨剤粒子を含有する前記塗料を塗布する、本発明
に基づく磁気記録媒体の製造方法の一例を示すものであ
る。FIG. 1 shows that when the magnetic layer is in a wet state,
Fig. 3 shows an example of a method for producing a magnetic recording medium according to the present invention, in which the coating material containing the abrasive particles is applied.
【0032】まず、非磁性支持体1上に、前記磁性紛と
前記結合剤を主体とする磁性層2と、研磨剤粒子3と結
合剤4と溶剤5とを含有する前記塗料と、を塗布によっ
て形成する。図示するように、研磨剤粒子3は、結合剤
4で被覆されていることが好ましい。First, the non-magnetic support 1 is coated with the magnetic powder and the magnetic layer 2 mainly composed of the binder, and the coating material containing the abrasive particles 3, the binder 4 and the solvent 5. Formed by As shown, the abrasive particles 3 are preferably coated with a binder 4.
【0033】次いで、乾燥処理を施すことによって、前
記塗料の溶剤5がなくなり、非磁性支持体1上に、磁性
層2が形成され、研磨剤粒子3が、磁性層2の表面域に
のみ分布しており、かつ図示するように、研磨剤粒子3
の少なくとも一部分が磁性層2の表面域に埋設されてい
る、本発明に基づく磁気記録媒体を製造することができ
る。Next, by performing a drying treatment, the solvent 5 of the paint is eliminated, the magnetic layer 2 is formed on the nonmagnetic support 1, and the abrasive particles 3 are distributed only in the surface area of the magnetic layer 2. And as shown, the abrasive particles 3
The magnetic recording medium according to the present invention, in which at least a part of the magnetic recording medium is buried in the surface area of the magnetic layer 2, can be manufactured.
【0034】ここで、磁性層2が湿潤状態のときに、研
磨剤粒子3を含有する前記塗料を塗布するには、例えば
ウエット・オン・ウエット方式を適用することができ
る。このウエット・オン・ウエット方式を適用する場合
には、例えば、図2に示すように、磁性層2用の塗料6
と研磨剤粒子3を含有する塗料7とをそれぞれ供給する
2つの塗料溜り8、9と、各塗料6、7を非磁性支持体
1に向かって吐出させる2つのスリット10、11とを
有するダイコーター12を用い、矢印A方向に走行する
非磁性支持体1に向かって、上記2つのスリット10、
11から磁性塗料6と研磨剤粒子3を含有する塗料7を
同時に吐出させ、磁性塗料6の塗膜上に塗料7の塗膜を
形成すればよい。Here, when the magnetic layer 2 is in a wet state, the above-mentioned paint containing the abrasive particles 3 can be applied, for example, by a wet-on-wet method. When this wet-on-wet method is applied, for example, as shown in FIG.
And a paint 7 containing abrasive particles 3 and two slits 10 and 11 for discharging the paints 6 and 7 toward the non-magnetic support 1. The two slits 10 toward the non-magnetic support 1 traveling in the direction of arrow A using the
From 11, the magnetic paint 6 and the paint 7 containing the abrasive particles 3 may be simultaneously discharged to form a coat of the paint 7 on the coat of the magnetic paint 6.
【0035】このウエット・オン・ウエット方式におい
ては、湿潤状態にある磁性塗料6の塗膜上に、研磨剤粒
子3を含有する塗料7を塗布するので、上述したよう
に、研磨剤粒子3の少なくとも一部分が磁性層2の表面
域に埋設された構造とすることができ、この場合、研磨
剤粒子3と磁性層2の接着性がより向上し、より一層走
行信頼性も向上することができる。In the wet-on-wet method, the coating material 7 containing the abrasive particles 3 is applied on the wet coating film of the magnetic coating material 6. At least a part of the structure can be buried in the surface area of the magnetic layer 2, and in this case, the adhesion between the abrasive particles 3 and the magnetic layer 2 can be further improved, and the running reliability can be further improved. .
【0036】また、研磨剤粒子3の少なくとも一部分
が、磁性層2の表面域に埋没されているのではなく、研
磨剤粒子3の全体が、磁性層2の表面域に埋没されてい
てもよい。Further, at least a part of the abrasive particles 3 may not be buried in the surface area of the magnetic layer 2, but the whole of the abrasive particles 3 may be buried in the surface area of the magnetic layer 2. .
【0037】図3は、前記磁性層が乾燥状態のときに、
前記研磨剤粒子を含有する前記塗料を塗布する、本発明
に基づく磁気記録媒体の製造方法の一例を示すものであ
る。FIG. 3 shows that when the magnetic layer is in a dry state,
Fig. 3 shows an example of a method for producing a magnetic recording medium according to the present invention, in which the coating material containing the abrasive particles is applied.
【0038】まず、非磁性支持体1上に、前記磁性紛と
前記結合剤を主体とする磁性層2を塗布によって形成
し、乾燥する。その後、磁性層2上に、結合剤4に被覆
された研磨剤粒子3と溶剤5を含有する前記塗料を塗布
する。First, a magnetic layer 2 mainly composed of the magnetic powder and the binder is formed on a non-magnetic support 1 by coating and dried. Thereafter, the paint containing the abrasive particles 3 coated with the binder 4 and the solvent 5 is applied onto the magnetic layer 2.
【0039】次いで、乾燥処理を施すことによって、前
記塗料の溶剤5がなくなり、非磁性支持体1上に、磁性
層2が形成され、さらに研磨剤粒子3が、磁性層2の表
面域にのみ分布しており、かつ図示するように、研磨剤
粒子3が、磁性層の表面上に付着されている、本発明に
基づく磁気記録媒体を製造することができる。Next, by performing a drying treatment, the solvent 5 of the coating material is eliminated, the magnetic layer 2 is formed on the non-magnetic support 1, and the abrasive particles 3 are further deposited only on the surface area of the magnetic layer 2. A magnetic recording medium according to the invention can be produced in which the abrasive particles 3 are distributed and, as shown, are deposited on the surface of the magnetic layer.
【0040】本発明に基づく磁気記録媒体の製造方法
は、磁性層2の表面上に、研磨剤粒子3を含有する前記
塗料を塗布して、研磨剤粒子3を磁性層2の表面域にの
み分布させるので、研磨剤粒子3を、磁性層2の表面域
での必要最小限の存在量分だけ塗布すればよく、しかも
均一な高さで存在させることが可能となり、より一層効
率良く磁気記録媒体を製造することができ、かつ得られ
る本発明に基づく磁気記録媒体は、走行信頼性にもより
一層優れている。The method for producing a magnetic recording medium according to the present invention comprises applying the above-mentioned paint containing abrasive particles 3 on the surface of the magnetic layer 2 so that the abrasive particles 3 are applied only to the surface area of the magnetic layer 2. Since the abrasive particles 3 are distributed, the abrasive particles 3 need only be applied in a necessary minimum amount in the surface area of the magnetic layer 2, and can be present at a uniform height. The magnetic recording medium according to the present invention, from which a medium can be manufactured and obtained, has further excellent running reliability.
【0041】また、研磨剤粒子3が磁性層2の表面域に
のみ分布しているので、磁性層2を形成する前記磁性塗
料には研磨剤粒子3を一切添加しないですみ、磁性層2
は、非常に前記磁性紛の充填率が高い状態を維持するこ
とが可能となり、より一層高い電磁変換特性を得ること
ができる。Also, since the abrasive particles 3 are distributed only in the surface area of the magnetic layer 2, the abrasive particles 3 need not be added to the magnetic paint forming the magnetic layer 2 at all, and the magnetic layer 2
Can maintain a state in which the filling rate of the magnetic powder is extremely high, and can obtain much higher electromagnetic conversion characteristics.
【0042】[0042]
【実施例】以下、本発明の具体的な実施例について説明
するが、本発明はこの実施例に限定されるものではな
い。DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, specific embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
【0043】例1 まず、下記の組成となるように磁性塗料を調製した。 [磁性塗料組成] 微細強磁性粉末:Fe−Co合金(長軸長0.15μm) 100重量部 結合剤: ポリエステル−ポリウレタン(平均分子量=21000) 7重量部 極性基;スルホン酸ナトリウム塩 0.12mmol/g含有 ポリエステル主成分;イソフタル酸−エチレングリコール ウレタン化イソシアネート;ジフェニルメタンジイソシアネート 塩化ビニル系共重合体(平均重合度=305) 8重量部 極性基;硫酸カリウム塩 0.08mmol/g含有 その他主な置換基;エポキシ 0.8mmol/g含有 水酸基 0.3mmol/g含有 ニトリロ三酢酸 3重量部 潤滑剤:ステアリン酸 1重量部 ステアリン酸ブチル 2重量部 溶剤:メチルエチルケトン 20重量部 トルエン 20重量部 シクロヘキサノン 10重量部 Example 1 First, a magnetic paint was prepared to have the following composition. [Magnetic paint composition] Fine ferromagnetic powder: 100 parts by weight of Fe-Co alloy (major axis length: 0.15 μm) Binder: 7 parts by weight of polyester-polyurethane (average molecular weight = 21000) Polar group: sodium sulfonate 0.12 mmol / G content Polyester main component; isophthalic acid-ethylene glycol urethanized isocyanate; diphenylmethane diisocyanate vinyl chloride copolymer (average degree of polymerization = 305) 8 parts by weight Polar group; potassium sulfate salt 0.08 mmol / g content Other major substitutions Group: Epoxy 0.8 mmol / g content Hydroxyl group 0.3 mmol / g content Nitrilotriacetic acid 3 parts by weight Lubricant: 1 part by weight of stearic acid 2 parts by weight of butyl stearate Solvent: 20 parts by weight of methyl ethyl ketone 20 parts by weight of toluene 10 parts by weight of cyclohexanone
【0044】以上の材料をコンティニアスニーダーで混
練処理を施し、さらにメチルエチルケトン、トルエン、
シクロヘキサノンで希釈した後、サンドミル分散し磁性
塗料とした。以上のようにして調製された磁性塗料を、
ポリイソシアネート(日本ポリウレタン社製硬化剤「コ
ロネートL」)4重量部添加し、攪拌した後、非磁性支
持体としての、厚み6.0μmのポリエチレンナフタレ
ートフィルム(テープ走行方向ヤング率6.0GPa、
幅方向ヤング率10.0GPa)上に、乾燥後の厚さが
1.5μmとなるように塗布した。The above materials are subjected to a kneading treatment with a continuous kneader, and further, methyl ethyl ketone, toluene,
After dilution with cyclohexanone, the mixture was dispersed in a sand mill to obtain a magnetic paint. The magnetic paint prepared as described above,
After adding 4 parts by weight of a polyisocyanate (a curing agent “Coronate L” manufactured by Nippon Polyurethane Co., Ltd.) and stirring, a polyethylene naphthalate film having a thickness of 6.0 μm as a non-magnetic support (Young's modulus in the tape running direction 6.0 GPa,
The film was applied on the film in such a manner that Young's modulus in the width direction was 10.0 GPa) so that the thickness after drying was 1.5 μm.
【0045】次いで、下記の組成となるように研磨剤粒
子を含有する塗料を調製した。 [研磨層用塗料組成] 無機粉末:アルミナ粉末 100重量部 α化率=85% 平均粒径 0.08μm 結合剤: ポリエステル系ポリウレタン樹脂(数平均分子量=14000) 5重量部 極性基;スルホン酸ナトリウム塩 0.08mmol/g含有 ポリエステル主成分;イソフタル酸、 アジピン酸−ネオペンチルグリコール、 エチレングリコール ウレタン化イソシアネート;ジフェニルメタンジイソシアネート 潤滑剤:ステアリン酸 1重量部 ステアリン酸ブチル 2重量部 溶剤:メチルエチルケトン 70重量部 トルエン 70重量部 シクロヘキサノン 40重量部Next, a paint containing abrasive particles was prepared to have the following composition. [Coating composition for polishing layer] Inorganic powder: Alumina powder 100 parts by weight Alpha conversion = 85% Average particle size 0.08 μm Binder: Polyester polyurethane resin (number average molecular weight = 14000) 5 parts by weight Polar group: sodium sulfonate 0.08 mmol / g salt content Polyester main component; isophthalic acid, adipic acid-neopentyl glycol, ethylene glycol urethanized isocyanate; diphenylmethane diisocyanate Lubricant: 1 part by weight stearic acid 2 parts by weight butyl stearate Solvent: 70 parts by weight methyl ethyl ketone Toluene 70 parts by weight Cyclohexanone 40 parts by weight
【0046】以上の材料をサンドミル分散し、前記研磨
剤粒子を含有する前記塗料とした。The above-mentioned materials were dispersed in a sand mill to obtain the above-mentioned paint containing the above-mentioned abrasive particles.
【0047】前記研磨剤塗料を攪拌後、これを、前記磁
性塗膜が湿潤状態のうちに、先に前記非磁性支持体上に
塗布した前記磁性層上に、乾燥後の前記磁性層の表面域
に前記研磨剤粒子が1個/μm2相当量存在するように
塗布した。After the abrasive coating is agitated, the abrasive coating is placed on the magnetic layer previously coated on the non-magnetic support while the magnetic coating is wet, and the surface of the dried magnetic layer is dried. It was applied so that the abrasive particles were present in an area equivalent to 1 particle / μm 2 .
【0048】前記研磨剤粒子を含有する前記塗料を塗布
後は、前記磁性塗膜に磁場配向処理を行い、適度に乾燥
させて巻取りした。そして、カレンダー処理を施し、硬
化処理を行った。After the application of the paint containing the abrasive particles, the magnetic coating film was subjected to a magnetic field orientation treatment, dried appropriately, and wound up. Then, a calendering treatment was performed and a curing treatment was performed.
【0049】その後、下記の組成のバックコート層用塗
料に対し、硬化剤(コロネートL)20重量部を添加
し、前記磁性層とは反対側の非磁性支持体面側に厚さ
0.5μmとなるように塗布し、バックコート層を形成
した。 [バックコート層用塗料組成] 無機粉末:カーボンブラック−1(平均粒径=0.02μm) (キャボット社製、商品名:BLACK PEARLS-L) DBP吸油量=105cc/100g 95重量部 カーボンブラック−2(平均粒径=0.35μm) (COLUMBIAN社製、商品名:MT-C1) DBP吸油量=40cc/100g 3重量部 酸化チタン 平均粒径=0.4μm 2重量部 結合剤: ポリエステルポリウレタン(数平均分子量=24000) 50重量部 極性基;スルホン酸ナトリウム塩 0.08mmol/g含有 ポリエステル主成分;イソフタル酸、 アジピン酸−ネオペンチルグリコール、 エチレングリコール ウレタン化イソシアネート;ジフェニルメタンジイソシアネート ニトロセルロース (旭化成工業社 セルノバBTH 1/2) 30重量部 硬化剤:ポリイソシアネート(日本ポリウレタン社 コロネート L) 10重量部 潤滑剤:ステアリン酸 1重量部 ステアリン酸ブチル 2重量部 溶剤:メチルエチルケトン 500重量部 トルエン 500重量部Thereafter, 20 parts by weight of a curing agent (Coronate L) was added to the coating material for the back coat having the following composition, and a thickness of 0.5 μm was formed on the nonmagnetic support surface opposite to the magnetic layer. To form a back coat layer. [Coating composition for back coat layer] Inorganic powder: carbon black-1 (average particle size = 0.02 μm) (manufactured by Cabot Corporation, trade name: BLACK PEARLS-L) DBP oil absorption = 105 cc / 100 g 95 parts by weight carbon black- 2 (Average particle size = 0.35 μm) (manufactured by COLUMBIAN, trade name: MT-C1) DBP oil absorption = 40 cc / 100 g 3 parts by weight Titanium oxide Average particle size = 0.4 μm 2 parts by weight Binder: polyester polyurethane ( 50 parts by weight Polar group; sodium salt of sulfonic acid 0.08 mmol / g Polyester main component; isophthalic acid, adipic acid-neopentyl glycol, ethylene glycol urethanized isocyanate; diphenylmethane diisocyanate nitrocellulose (Asahi Chemical Industry Co., Ltd.) Cellnova BTH 1/2) 30 parts by weight Hard Agent: polyisocyanate (Nippon Polyurethane Co., Coronate L) 10 parts by weight Lubricant: Stearic acid 1 part by weight butyl stearate 2 parts by weight Solvent: Methyl ethyl ketone 500 parts by weight Toluene 500 parts by weight
【0050】その後、6.35mm幅に裁断することで
サンプルテープを作製した。Thereafter, a sample tape was prepared by cutting to a width of 6.35 mm.
【0051】例2 前記研磨剤粒子が、前記磁性層の表面域に50個/μm
2相当量存在するように塗布した以外は、実施例1と同
様にしてサンプルテープを作製した。 Example 2 The number of the abrasive particles was 50 particles / μm on the surface area of the magnetic layer.
A sample tape was prepared in the same manner as in Example 1 except that the coating was carried out so that 2 equivalents were present.
【0052】例3 前記磁性塗膜を乾燥した後に、前記研磨剤粒子が、前記
磁性層の表面域に100個/μm2相当量存在するよう
に塗布した以外は、実施例1と同様にしてサンプルテー
プを作製した。 Example 3 The procedure of Example 1 was repeated, except that after the magnetic coating film was dried, the abrasive particles were applied so as to be present in an amount of 100 particles / μm 2 on the surface area of the magnetic layer. A sample tape was prepared.
【0053】例4 前記研磨剤粒子が、前記磁性層の表面域に0.5個/μ
m2相当量存在するようにした以外は、実施例1と同様
にしてサンプルテープを作製した。[0053] Example 4 The abrasive particles, 0.5 or the surface area of the magnetic layer / mu
A sample tape was prepared in the same manner as in Example 1 except that m 2 was present in an amount equivalent to m 2 .
【0054】例5 前記研磨剤粒子が、前記磁性層の表面上に120個/μ
m2相当相当量存在するようにした以外は、実施例1と
同様にしてサンプルテープを作製した。[0054] Example 5 The abrasive particles, 120 / mu on the surface of the magnetic layer
A sample tape was prepared in the same manner as in Example 1 except that a corresponding amount of m 2 was present.
【0055】例6 平均粒径が0.02μmである前記研磨剤粒子を用いた
こと以外は、実施例1と同様にしてサンプルテープを作
製した。 Example 6 A sample tape was prepared in the same manner as in Example 1 except that the abrasive particles having an average particle size of 0.02 μm were used.
【0056】例7 平均粒径が0.35μmである前記研磨剤粒子を用いた
こと以外は、実施例1と同様にしてサンプルテープを作
製した。 Example 7 A sample tape was prepared in the same manner as in Example 1 except that the abrasive particles having an average particle diameter of 0.35 μm were used.
【0057】例8 下記の組成となるように磁性塗料を調整した。 [磁性塗料組成] 微細強磁性粉末:Fe−Co合金(長軸長0.15μm) 100重量部 結合剤: ポリエステル−ポリウレタン(平均分子量=21000) 8重量部 極性基;スルホン酸ナトリウム塩 0.12mmol/g含有 ポリエステル主成分;イソフタル酸−エチレングリコール ウレタン化イソシアネート;ジフェニルメタンジイソシアネート 塩化ビニル系共重合体(平均重合度=305) 10重量部 極性基;硫酸カリウム塩 0.08mmol/g含有 その他主な置換基;エポキシ 0.8mmol/g含有 水酸基 0.3mmol/g含有 ニトリロ三酢酸 3重量部 研磨剤:アルミナ粉末 8重量部 α化率=85% 平均粒径0.08μm 潤滑剤:ステアリン酸 1重量部 ステアリン酸ブチル 2重量部 溶剤:メチルエチルケトン 20重量部 トルエン 20重量部 シクロヘキサノン 10重量部 Example 8 A magnetic paint was prepared to have the following composition. [Magnetic paint composition] Fine ferromagnetic powder: 100 parts by weight of Fe-Co alloy (major axis length: 0.15 μm) Binder: 8 parts by weight of polyester-polyurethane (average molecular weight = 21000) Polar group: sodium sulfonate 0.12 mmol / G content Polyester main component; isophthalic acid-ethylene glycol urethanized isocyanate; diphenylmethane diisocyanate vinyl chloride copolymer (average degree of polymerization = 305) 10 parts by weight Polar group; potassium sulfate salt 0.08 mmol / g content Other major substitutions Group: Epoxy 0.8 mmol / g content Hydroxyl group 0.3 mmol / g content Nitrilotriacetic acid 3 parts by weight Abrasive: Alumina powder 8 parts by weight Alpha conversion = 85% Average particle size 0.08 μm Lubricant: Stearic acid 1 part by weight Butyl stearate 2 parts by weight Solvent: methyl ethyl ketone 0 parts by weight Toluene 20 parts by weight Cyclohexanone 10 parts by weight
【0058】前記非磁性支持体上に、上記した配合成分
からなる磁性塗料を塗布し、前記研磨剤粒子を含有する
前記塗料は塗布しなかったこと以外は、実施例1と同様
にしてサンプルテープを作製した。なお、前記磁性層の
表面上に、前記研磨剤粒子が2個/μm2相当量存在す
るよう調製した。A sample tape was prepared in the same manner as in Example 1 except that a magnetic paint comprising the above-mentioned components was applied onto the non-magnetic support, and the paint containing the abrasive particles was not applied. Was prepared. The abrasive particles were prepared so as to be present in an amount of 2 particles / μm 2 on the surface of the magnetic layer.
【0059】以上のようにして作製した各サンプルテー
プについて、下記に示す各種測定を行った。Various measurements shown below were performed on each sample tape produced as described above.
【0060】各種測定の方法は、以下のとおりである。 ・電磁変換特性(0.5μm波長信号出力)は、SON
Y製DV用VTR DCR−VX1000を用いて被測
定テープに1/2T信号を記録し、再生出力を測定し
た。 ・走行信頼性は、ソニー製DV用VTR DCR−VX
1000を用い22℃、湿度50%の環境下で被測定テ
ープを100回連続走行させた後に、RF出力劣化量を
測定し、ブロックエラーの発生や再生異常の発生するも
のを×、画質などに異常なく走行したものを○とした。 ・磁性層の表面の研磨剤粒子の存在量は、AFM(原子
間力顕微鏡)を用いて観察した。The various measuring methods are as follows.・ The electromagnetic conversion characteristic (0.5μm wavelength signal output) is SON
A 1 / 2T signal was recorded on the tape to be measured using a Y DV DVR DCR-VX1000, and the reproduction output was measured.・ Driving reliability is VCR DCR-VX for Sony DV.
After running the tape to be measured 100 times continuously in an environment of 22 ° C. and 50% humidity using a 1000, the amount of RF output deterioration was measured. The one that ran without any abnormality was marked with “○”. The amount of abrasive particles present on the surface of the magnetic layer was observed using an AFM (atomic force microscope).
【0061】上記の各評価方法によって得られた結果
を、下記表2にまとめて示す。The results obtained by each of the above evaluation methods are summarized in Table 2 below.
【0062】[0062]
【表1】 [Table 1]
【0063】表1より明らかなように、例1〜例5の各
サンプルテープは、前記磁性層上に、前記研磨剤粒子を
含有する前記塗料を塗布し、前記研磨剤粒子を前記磁性
層の表面域にのみ分布させ、前記磁性塗料中には前記研
磨剤粒子を内添しなかったので、前記磁性塗料中に前記
研磨剤粒子を含有する場合と比べて、前記磁性層は、磁
性紛の充填率が向上し、高い出力特性を得ることがで
き、走行信頼性にも優れていた。また、前記磁性層の表
面域に存在する前記研磨剤粒子の個数を1〜100個/
1μm2とすれば、上記の範囲外の場合に比べ、より安
定した走行性及び高い出力特性が得られることが分か
る。さらに、前記研磨剤粒子の粒径を0.02〜0.3
5μmとすれば、より優れた効果を発揮し得る磁気記録
媒体が得られることが分かる。As is clear from Table 1, each of the sample tapes of Examples 1 to 5 was prepared by applying the above-mentioned paint containing the above-mentioned abrasive particles on the above-mentioned magnetic layer, and applying the above-mentioned abrasive particles to the above-mentioned magnetic layer. The magnetic layer was distributed only on the surface area, and the abrasive particles were not internally added in the magnetic paint.Thus, compared with the case where the abrasive particles were contained in the magnetic paint, the magnetic layer was formed of magnetic powder. The filling rate was improved, high output characteristics could be obtained, and running reliability was excellent. Further, the number of the abrasive particles existing in the surface area of the magnetic layer is 1 to 100 / particle.
It can be seen that when the thickness is 1 μm 2 , more stable running characteristics and higher output characteristics can be obtained as compared with the case outside the above range. Further, the abrasive particles have a particle size of 0.02 to 0.3.
It can be seen that when the thickness is 5 μm, a magnetic recording medium that can exhibit more excellent effects can be obtained.
【0064】例6は、前記磁性層の表面域に存在する前
記研磨剤粒子の個数が0.5個/1μm2と、1個/1
μm2より少なかったため、前記磁性層がドライブなど
の走行系や磁気ヘッドに直接接触してしまい、走行信頼
性が悪化することがあった。In Example 6, the number of the abrasive particles existing in the surface area of the magnetic layer was 0.5 / 1 μm 2 and 1/1.
Since it was less than μm 2 , the magnetic layer was in direct contact with a traveling system such as a drive or a magnetic head, and traveling reliability was sometimes deteriorated.
【0065】例7は、前記磁性層の表面域に存在する前
記研磨剤粒子の個数が1200.5個/1μm2と、1
00個/1μm2を超えていたため、出力特性が低下す
ることがあった。In Example 7, the number of the abrasive particles existing in the surface area of the magnetic layer was 1200.5 / 1 μm 2 ,
Since it exceeded 00 pieces / 1 μm 2 , the output characteristics sometimes deteriorated.
【0066】例8は、前記磁性層の表面上に、前記研磨
剤粒子が2個/1μm2存在するように、前記磁性塗料
中に、前記研磨剤粒子を添加したので、走行信頼性には
優れていたが、前記磁性層中の磁性紛の充填率が低下
し、出力特性が低下した。In Example 8, the abrasive particles were added to the magnetic paint such that the abrasive particles existed at a rate of 2 particles / 1 μm 2 on the surface of the magnetic layer. Although excellent, the filling rate of the magnetic powder in the magnetic layer was reduced, and the output characteristics were reduced.
【0067】[0067]
【発明の作用効果】本発明によれば、前記磁性層の表面
上に、前記研磨剤粒子を含有する前記塗料を塗布して、
前記研磨剤粒子を前記磁性層の表面域にのみ分布させる
ので、前記研磨剤粒子を、前記磁性層の表面域での必要
最小限の存在量分だけ塗布すればよく、しかも均一な高
さで存在させることが可能となり、効率良く磁気記録媒
体を製造することができ、かつ得られる磁気記録媒体は
走行信頼性に優れている。According to the present invention, the paint containing the abrasive particles is applied on the surface of the magnetic layer,
Since the abrasive particles are distributed only in the surface area of the magnetic layer, the abrasive particles may be applied only in a necessary minimum amount in the surface area of the magnetic layer, and at a uniform height. The magnetic recording medium can be efficiently produced, and the obtained magnetic recording medium has excellent running reliability.
【0068】また、前記研磨剤粒子が前記磁性層の表面
域にのみ分布しているので、前記磁性層を形成する磁性
塗料には前記研磨剤粒子を一切添加しないですみ、前記
磁性層は、非常に磁性紛の充填率が高い状態を維持する
ことが可能となる。例えば、磁性紛の配向過程において
も、配向を阻害するような粒子が存在しないため効率を
向上することができ、高い出力特性等の電磁変換特性を
得ることができる。Also, since the abrasive particles are distributed only in the surface area of the magnetic layer, the abrasive particles need not be added to the magnetic paint forming the magnetic layer at all, and the magnetic layer is It is possible to maintain a state where the filling rate of the magnetic powder is very high. For example, in the process of aligning the magnetic powder, the efficiency can be improved because there are no particles that hinder the alignment, and electromagnetic conversion characteristics such as high output characteristics can be obtained.
【図1】本発明による、一実施の形態の磁気記録媒体の
製造方法を示す図である。FIG. 1 is a diagram illustrating a method of manufacturing a magnetic recording medium according to an embodiment of the present invention.
【図2】同、磁気記録媒体の製造に用いられる重層塗布
装置の概略構成図である。FIG. 2 is a schematic configuration diagram of a multilayer coating apparatus used for manufacturing a magnetic recording medium.
【図3】本発明による、他の実施の形態の磁気記録媒体
の製造方法を示す図である。FIG. 3 is a diagram illustrating a method of manufacturing a magnetic recording medium according to another embodiment of the present invention.
1…非磁性支持体、2…磁性層、3…研磨剤粒子、4…
結合剤、5…溶剤、6…磁性塗料、7…研磨剤粒子を含
有する塗料、8、9…塗料溜り、10、11…スリッ
ト、12…ダイコーターDESCRIPTION OF SYMBOLS 1 ... Nonmagnetic support, 2 ... Magnetic layer, 3 ... Abrasive particles, 4 ...
Binder, 5 solvent, 6 magnetic paint, 7 paint containing abrasive particles, 8, 9 paint pool, 10, 11 slit, 12 die coater
Claims (15)
の表面域にのみ分布している、磁気記録媒体。1. A magnetic recording medium having a magnetic layer, wherein abrasive particles are distributed only in a surface area of the magnetic layer.
る、請求項1に記載した磁気記録媒体。2. The magnetic recording medium according to claim 1, wherein the abrasive particles are coated with a binder.
に付着されている、請求項2に記載した磁気記録媒体。3. The magnetic recording medium according to claim 2, wherein the abrasive particles are attached on a surface of the magnetic layer.
記磁性層の表面域に埋設されている、請求項2に記載し
た磁気記録媒体。4. The magnetic recording medium according to claim 2, wherein at least a part of the abrasive particles is embedded in a surface area of the magnetic layer.
1μm2である、請求項1に記載した磁気記録媒体。5. The number of the abrasive particles is 1 to 100 /
2. The magnetic recording medium according to claim 1, which is 1 μm 2 .
35μmである、請求項1に記載した磁気記録媒体。6. The abrasive particles having a particle size of 0.02 to 0.5.
2. The magnetic recording medium according to claim 1, which has a thickness of 35 μm.
ある、請求項1に記載した磁気記録媒体。7. The magnetic recording medium according to claim 1, wherein the Mohs hardness of the abrasive particles is 3 or more.
を塗布し、前記研磨剤粒子を前記磁性層の表面域にのみ
分布させる、磁気記録媒体の製造方法。8. A method for producing a magnetic recording medium, wherein a coating material containing abrasive particles is applied on a magnetic layer, and the abrasive particles are distributed only in a surface area of the magnetic layer.
体とする前記磁性層を塗布で形成し、前記磁性層が乾燥
状態若しくは湿潤状態のうちに、前記研磨剤粒子及び結
合剤を含有する前記塗料を塗布し、その後、前記塗料を
乾燥する、請求項8に記載した磁気記録媒体の製造方
法。9. The method according to claim 1, wherein the magnetic layer mainly composed of a magnetic powder and a binder is formed by coating on a non-magnetic support, and the abrasive particles and the binder are formed while the magnetic layer is in a dry state or a wet state. The method for manufacturing a magnetic recording medium according to claim 8, wherein the paint containing is applied, and thereafter, the paint is dried.
た状態とする、請求項8に記載した磁気記録媒体の製造
方法。10. The method for manufacturing a magnetic recording medium according to claim 8, wherein the abrasive particles are coated with the binder.
に付着する、請求項10に記載した磁気記録媒体の製造
方法。11. The method for manufacturing a magnetic recording medium according to claim 10, wherein the abrasive particles are attached on a surface of the magnetic layer.
前記磁性層の表面域に埋設する、請求項10に記載した
磁気記録媒体の製造方法。12. The method of manufacturing a magnetic recording medium according to claim 10, wherein at least a part of the abrasive particles is embedded in a surface area of the magnetic layer.
/1μm2とする、請求項8に記載した磁気記録媒体の
製造方法。13. The method of manufacturing a magnetic recording medium according to claim 8, wherein the number of the abrasive particles is 1 to 100/1 μm 2 .
0.35μmとする、請求項8に記載した磁気記録媒体
の製造方法。14. The abrasive particles having a particle size of 0.02 to 0.02.
The method for manufacturing a magnetic recording medium according to claim 8, wherein the thickness is 0.35 µm.
粒子を用いる、請求項8に記載した磁気記録媒体の製造
方法。15. The method for producing a magnetic recording medium according to claim 8, wherein the abrasive particles having a Mohs hardness of 3 or more are used.